A composite oxygen carrier consisting of iron-manganese oxide-supported tobacco straw biochar, its preparation method, and its application.

By preparing iron-manganese oxide-supported tobacco stalk biochar composite materials, the problems of low efficiency in tannic acid wastewater treatment and poor catalyst stability were solved, achieving efficient and stable tannic acid degradation and mineralization, and catalytic performance adaptable to a wide pH range.

CN123102376APending Publication Date: 2026-11-17YUNNAN NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611386113.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-08
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies are difficult to effectively treat tannic acid wastewater. Traditional methods are inefficient and have secondary sludge problems. Heterogeneous catalyst nanoparticles are prone to agglomeration, affecting stability. Furthermore, existing research has not shown the application of iron-manganese oxides loaded on tobacco straw biochar for activating persulfate degradation of tannic acid.

Method used

Iron-manganese oxide-supported tobacco biochar composite material was prepared by ultrasonic treatment and pyrolysis, forming a multi-level porous structure with micropores, mesopores and macropores coexisting. Nanoparticles were uniformly loaded on the surface of biochar and used to activate persulfate to degrade tannic acid.

Benefits of technology

It achieves efficient and stable tannic acid degradation, with a removal rate of up to 97.52% within 90 minutes. The catalytic activity remains good within the pH range of 3-11, exhibiting wide pH adaptability, excellent catalytic performance, and strong mineralization ability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102376A_ABST
    Figure CN123102376A_ABST
Patent Text Reader

Abstract

This invention discloses a composite oxygen carrier made of iron-manganese oxide supported on tobacco straw biochar, its preparation method, and its application, belonging to the field of environmental functional materials technology. The composite oxygen carrier uses tobacco straw biochar as a carrier, with nano-sized iron-manganese oxide uniformly loaded on its surface, exhibiting a hierarchical porous structure. The preparation method involves mixing tobacco straw powder with an iron and manganese salt solution, followed by ultrasonication, stirring, drying, and then pyrolysis at 500-900℃ under an inert atmosphere. This composite oxygen carrier can act as a catalyst to activate persulfate, efficiently degrading organic pollutants (such as tannic acid) in water. It exhibits excellent catalytic activity and stability over a wide pH range of 3-11, realizing the resource utilization of agricultural waste.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of environmental functional materials technology, and particularly relates to an iron-manganese oxide-supported tobacco straw biochar composite oxygen carrier, its preparation method and application. Background Technology

[0002] Tannic acid (TA) wastewater is characterized by high color and poor biodegradability. Traditional physical adsorption and biological treatment methods are inefficient, while chemical precipitation methods easily generate secondary sludge. Advanced oxidation processes (AOPs) are an effective means of treating this type of recalcitrant organic wastewater, but traditional homogeneous catalytic systems suffer from narrow pH adaptability, difficulty in catalyst recovery, and the generation of iron-containing sludge. Although heterogeneous catalysts such as iron-manganese oxides show potential, their nanoparticles are prone to agglomeration during the reaction, leading to a reduction in active sites and metal ion leaching, affecting long-term stability. Loading catalysts onto biochar is an effective strategy to solve this problem, but existing studies mostly use rice husks and sugarcane bagasse as raw materials, and there are no systematic reports on loading iron-manganese oxides onto tobacco straw biochar as an oxygen-carrying catalyst for activating permonosulfate (PMS) degradation of tannic acid.

[0003] Therefore, there is an urgent need to provide a highly efficient, stable, and wide-range heterogeneous oxygen-supported catalyst prepared by loading iron and manganese oxides from agricultural waste tobacco stalks, so as to achieve efficient degradation of tannic acid wastewater and resource utilization of tobacco stalk waste. Summary of the Invention

[0004] To address the aforementioned technical problems, this invention proposes an iron-manganese oxide-supported tobacco straw biochar composite oxygen carrier, its preparation method, and its application.

[0005] To achieve the above objectives, the present invention provides the following technical solution: A method for preparing an iron-manganese oxide-supported tobacco straw biochar composite material includes the following steps: S1. Mix tobacco stalk powder with a mixed solution containing iron salt and manganese salt, sonicate and stir, filter, wash and dry to obtain the precursor; S2. The precursor is pyrolyzed under an inert atmosphere at a temperature of 500-900℃. After pyrolysis, it is ground and sieved to obtain the iron-manganese oxide-supported tobacco biochar composite material.

[0006] Optionally, in step S1, the iron salt is FeCl2 and the manganese salt is KMnO4.

[0007] Optionally, in step S1, the ultrasonic treatment time is 30 minutes, and the stirring is hydrothermal stirring for 6 hours.

[0008] Optionally, in step S2, the heating rate of the pyrolysis is 5℃ / min, and the pyrolysis time is 2h.

[0009] Optionally, in step S2, the pyrolysis temperature is preferably 500-800℃, more preferably 800℃.

[0010] A composite material of iron-manganese oxide supported tobacco biochar includes a tobacco biochar carrier and iron-manganese oxide nanoparticles loaded on the surface of the tobacco biochar carrier; the iron-manganese oxide nanoparticles are uniformly dispersed on the surface and in the pore structure of the tobacco biochar carrier, and the composite material has a multi-level pore structure in which micropores, mesopores and macropores coexist.

[0011] Optionally, the iron-manganese oxide nanoparticles contain a spinel phase of MnFe2O4.

[0012] Application of the above-mentioned iron-manganese oxide-supported tobacco biochar composite material in the degradation of organic pollutants by activated persulfate.

[0013] Optionally, the organic pollutant is tannic acid.

[0014] Optionally, the dosage of the iron-manganese oxide-supported tobacco biochar composite material is 0.5-1.5 g / L, and the dosage of the persulfate is 0.05-0.15 mol / L.

[0015] Optionally, the initial pH of the reaction system for the application is 3-11.

[0016] Compared with the prior art, the present invention has the following advantages and technical effects: This invention utilizes agricultural waste tobacco stalks as raw material to prepare an iron-manganese oxide-supported tobacco stalk biochar composite material (FMBC) via impregnation-pyrolysis, realizing the environmentally friendly concept of "treating waste with waste." This composite material possesses a hierarchical pore structure with micropores, mesopores, and macropores coexisting. Nanoscale iron-manganese oxides (mainly MnFe2O4 spinel phase) are uniformly loaded on the biochar surface, forming a stable composite catalytic material. In the application of activated persulfate (PMS) for the degradation of tannic acid (TA), this system exhibits excellent catalytic performance. Under optimal conditions (pyrolysis temperature 800℃, FMBC dosage 1.2 g / L, PMS concentration 0.08 mol / L, initial pH=7), the TA removal rate reaches 97.52% within 90 min, with a pseudo-first-order kinetic constant more than 630 times that of the PMS system alone. Furthermore, the total organic carbon (TOC) removal rate reaches 60.9%, indicating good mineralization ability. Furthermore, this system exhibits wide pH adaptability, maintaining high catalytic activity within a pH range of 3-11, demonstrating promising application potential for practical wastewater treatment. Its highly efficient catalytic activity is primarily attributed to the synergistic redox cycle between the Fe-Mn bimetals, the adsorption and enrichment by the biochar support and electron transfer, and the combined attack of reactive oxygen species (mainly ·OH). Attached Figure Description

[0017] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings: Figure 1 The standard curve for tannic acid; Figure 2 SEM images of FMBC at different magnifications; Figure 3 The adsorption-desorption isotherms and pore size distribution diagram of FMBC; Figure 4 FTIR plot of FMBC; Figure 5 Raman plot for FMBC; Figure 6 XRD pattern of FMBC; Figure 7 To investigate the effects of different reaction systems on TA degradation and the corresponding pseudo-first-order kinetic analysis; Figure 8 The effect of different FMBC preparation conditions on TA degradation and the corresponding pseudo-first-order kinetic analysis; Figure 9 The effect of PMS dosage on TA degradation and the corresponding pseudo-first-order kinetic analysis; Figure 10The effect of FMBC dosage on TA degradation and the corresponding pseudo-first-order kinetic analysis; Figure 11 The effect of initial pH on TA degradation and the corresponding pseudo-first-order kinetic analysis; Figure 12 The effects of common anions on TA degradation; Figure 13 TOC removal under optimal reaction conditions; Figure 14 The effects of different concentrations of EtOH and TBA on TA degradation and the corresponding pseudo-first-order kinetic analysis were conducted. Detailed Implementation

[0018] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0019] It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the invention. Furthermore, with respect to numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Every smaller range between any stated value or intermediate value within a stated range, and any other stated value or intermediate value within said range, is also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.

[0020] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.

[0021] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be apparent to those skilled in the art. This specification and embodiments are merely exemplary.

[0022] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.

[0023] All raw materials used in this invention were purchased from the market.

[0024] The technical solution of the present invention will be further illustrated by the following embodiments.

[0025] Examples 1 to 5 A method for preparing an iron-manganese oxide-supported tobacco straw biochar composite material includes the following steps: Weigh 10g of tobacco stalk powder (the tobacco stalks were collected from Panlong District, Kunming City, Yunnan Province, washed, dried at 80℃, and then pulverized and ground through a 200-mesh sieve to obtain the tobacco stalk powder) into a beaker, add 100mL of 0.10 mol / L KMnO4 and 100mL of 0.28 mol / L KMnO4. A mol / L FeCl2 mixed solution was ultrasonicated (100W) for 30 min and hydrothermally stirred (80℃) for 6 h. After filtration, the solid product was washed with deionized water until the filtrate was colorless and neutral. The sample was then filtered and dried in a 105℃ drying oven for 24 h to constant weight. The dried sample was then placed in a crucible, covered, and placed in a tube furnace under nitrogen protection. The sample was pyrolyzed at 500℃, 600℃, 700℃, 800℃, and 900℃ for 2 h at a heating rate of 5℃ / min. The sample was then removed, ground, and passed through a 100-mesh sieve for later use. The samples were labeled as FMBC-500, FMBC-600, FMBC-700, FMBC-800, and FMBC-900.

[0026] Effect verification: 1. Material Characterization Methods The specific surface area (SSA) of the materials was determined using the Bruner-Emmett-Taylor (BET) method on a surface analyzer (ASAP2460, USA). Scanning electron microscopy (SEM, JEM2010, Japan) combined with energy dispersive spectroscopy (EDS, Oxford XMAX, UK) was used to characterize the surface morphology and structural differences. The functional groups on the surface of each adsorbent were determined by Fourier transform infrared spectroscopy (FTIR, alpha, Bruker, Germany). The crystal structure of the adsorbent was analyzed by X-ray diffraction (XRD, Bruker D8advanc, Germany). Raman spectroscopy was used to measure the Raman scattering spectra of the materials to study their chemical structure, molecular vibrational information, and crystal structure. Finally, X-ray photoelectron spectroscopy (XPS, ThermoESCALAB 250, USA) determined the elemental chemical state and surface composition, with the C1s peak at a binding energy of 245 eV serving as the background signal.

[0027] 2. Analysis and determination of tannic acid Existing research and wavelength scanning analysis of TA solutions show that TA has the strongest absorption peak at 276 nm. TA solutions of 0.5 mg / L, 1 mg / L, 2 mg / L, 4 mg / L, 6 mg / L, 8 mg / L, and 10 mg / L were prepared by diluting 10 mg / L TA solution into colorimetric tubes. The absorbance was measured at 276 nm using a spectrophotometer, and a standard curve was plotted between TA concentration and absorbance. Figure 1 As shown. The formula for calculating TA removal rate is... ; Chemical reaction kinetics is a mathematical description method used to quantitatively describe the changes of a chemical reaction over time and to express the reaction rate and its relationship with various influencing factors. Based on formula (1), first-order kinetics were fitted to the degradation of TA.

[0028] In the formula: C0 is the initial concentration of TA, in mg / L; C t t represents the concentration of TA after reaction time (mg / L); k is the kinetic constant; and t is the reaction time (min).

[0029] 3. Determination of Total Organic Carbon (TOC) To analyze the mineralization of pollutants during the degradation process, the total organic carbon (TOC) content in the solution was determined using a Shimadu TOC-L CPH analyzer (model: Shimadu TOC-L CPH). Changes in TOC are an important indicator for evaluating pollutant degradation. To eliminate the influence of organic membrane materials on TOC measurement, solutions before and after the reaction were filtered through a 0.22 μm inorganic glass fiber membrane and measured rapidly.

[0030] 4. Determination of active species Due to the short lifetime of active species in water, there is no direct method to measure their concentration in PMS-based advanced oxidation processes. Therefore, a quenching method was used to evaluate the role of active species in TA degradation. The addition of quenchers only removes their target reactive substances without significantly affecting other reactions. Ethanol (EtOH) and tert-butanol (TBA) were selected as SO42- and SO42-, respectively. ·- EtOH is a quencher of ·OH-, among which EtOH can simultaneously quench SO42-. ·- TBA is used as a ·OH scavenger, while TBA is used only as a ·OH scavenger. To avoid changes in solution concentration due to the addition of the scavenger, all curves are blanks after deducting the scavenger itself.

[0031] Results and Discussion I. Material Characterization Analysis 1. SEM Analysis The microstructure of FMBC at different magnifications was observed using scanning electron microscopy (SEM), and the results are as follows: Figure 2 As shown in the low-magnification images, FMBC-800 exhibits an irregular blocky or granular morphology with uneven particle size distribution and a relatively rough surface. With increasing magnification, a large number of fine particles are clearly visible on the biochar surface, uniformly dispersed on the carbon matrix surface, with slight agglomeration in some areas. The particle size is mainly in the nanometer to submicron range, with some particles embedded in the porous structure of the biochar. This uniformly dispersed loading morphology is attributed to the full adsorption of iron and manganese ions on the surface of the tobacco stem precursor during the impregnation-pyrolysis preparation process, and the in-situ generation of iron and manganese oxide nanoparticles during pyrolysis. Furthermore, at higher magnification, a distinct porous structure is observed in the biochar matrix, with pores that are mainly irregular in shape and have a wide pore size distribution. This abundant porous structure and good particle dispersion provide numerous accessible active sites for the catalytic reaction, facilitating the diffusion and mass transfer of reactant molecules.

[0032] 2. BET Analysis The specific surface area and pore structure of FMBC-800 were characterized by N2 adsorption-desorption experiments, and the results are as follows: Figure 3 As shown. According to the IUPAC classification, the adsorption-desorption isotherm of FMBC-800 belongs to Type IV isotherms. In the low relative pressure region (P / P0 < 0.1), the adsorption amount increases rapidly, indicating the presence of a certain amount of microporous structure in the material. In the medium-to-high relative pressure region (P / P0 = 0.4–0.9), the isotherm shows obvious hysteresis loops, which is a typical characteristic of capillary condensation in mesoporous materials. The hysteresis loop type is close to Type H3, indicating the presence of slit-like pore structures in the material, which is consistent with the pore structure formed by its lamellar or irregular particle stacking.

[0033] BET analysis showed that the specific surface area of ​​FMBC was 67.79 m² / g, while that of Langmuir was 193.06 m² / g. t-Plot analysis revealed a micropore area of ​​45.84 m² / g and an external surface area of ​​21.96 m² / g, indicating that micropores contributed approximately 67.6% to the total specific surface area, with mesopores and macropores contributing the remainder. The total pore volume was 0.0760 cm³ / g, of which micropores accounted for 0.0195 cm³ / g, mesopores for 0.0385 cm³ / g (50.5%), and macropores for 0.0180 cm³ / g (23.6%). The average pore size of BJH desorption was 6.92 nm, falling within the typical mesoporous range.

[0034] The above results demonstrate that FMBC possesses a hierarchical porous structure with micropores, mesopores, and macropores coexisting. Abundant micropores provide a large specific surface area and numerous adsorption sites, while mesopores and macropores facilitate rapid diffusion and mass transfer of reactant molecules. This hierarchical porous structure is crucial for the efficient conduction of catalytic reactions: on the one hand, the microporous region provides a high density of active sites; on the other hand, the mesoporous and macroporous channels ensure that PMS and TA molecules can smoothly reach the active sites and rapidly release the products.

[0035] 3. FTIR analysis The surface functional groups of FMBC-800 were characterized using Fourier transform infrared spectroscopy (FTIR), and the results are as follows: Figure 4 As shown. At 3382 cm -1 A broad and strong absorption peak appears at 1617 cm⁻¹, attributed to the OH stretching vibration. This broad peak indicates the presence of numerous hydroxyl groups on the material surface, possibly originating from residual oxygen-containing functional groups (such as phenolic and alcoholic hydroxyl groups) on the biochar surface, as well as water molecules or structural water adsorbed on the iron-manganese oxide surface. -1 The weak absorption peak at 1029 cm⁻¹ can be attributed to NH bending vibration or C=C stretching vibration, possibly related to the skeletal vibrations of the aromatic ring structure in biochar. -1 The strong absorption peak at 798 cm⁻¹ is attributed to the CN stretching vibration or the Si-O stretching vibration of silicates. -1 and 694cm -1 The weak absorption peaks at 469 cm⁻¹ are attributed to the Si-O-Si stretching vibration and the CH bending vibration, respectively. -1 The moderate-intensity absorption peak at this point is a characteristic peak of the MO stretching vibration and can be attributed to the vibrational absorption of the Fe-O or Mn-O bonds.

[0036] The FTIR analysis results above indicate that the FMBC-800 surface contains abundant oxygen-containing functional groups (such as -OH, C=O, etc.) and metal-oxygen bonds (MO). These functional groups play multiple roles in catalytic reactions: on the one hand, the oxygen-containing functional groups on the biochar surface can act as electron donors, promoting Fe... 3+ / Fe 2+ and Mn 3+ / Mn 2+ The oxidation-reduction cycle between them; on the other hand, surface hydroxyl groups can adsorb TA molecules through hydrogen bonding, enhancing the contact between pollutants and catalytically active sites; in addition, the presence of MO bonds confirms that iron-manganese oxides were successfully loaded onto the surface of biochar.

[0037] 4. Raman analysis Raman spectroscopy was used to characterize the structural order and defect level of the carbon material FMBC-800, and the results are as follows: Figure 5As shown, two typical characteristic peaks appear in the spectrum: one located at approximately 1365 cm⁻¹. -1 The D-band and approximately 1581 cm -1 The G band corresponds to the disordered vibrations caused by sp³ hybridized carbon atoms or structural defects in carbon materials, reflecting defects and edge sites in the carbon framework; the G band corresponds to the in-plane E2g symmetric stretching vibrations of sp² hybridized carbon atoms in graphitized structures, reflecting the planar C=C vibrations of ordered graphitized carbon.

[0038] Peak fitting analysis of the three test points showed that the peaks of the D and G bands were located at 1356–1363 cm⁻¹, respectively. -1 and 1579–1582 cm -1 Within the specified range, the ID / IG intensity ratios were 0.8546, 0.8295, and 0.7941, with an average of 0.826. This ratio indicates that the carbon material in FMBC belongs to the high-defect / nanocrystalline carbon type. The high ID / IG ratio is attributed to two main reasons: first, the carbon structure formed during the pyrolysis of tobacco straw biomass itself has a high degree of disorder; second, the loading of iron-manganese oxide nanoparticles on the biochar surface introduces additional structural defects and interfacial sites.

[0039] Furthermore, compared to conventional graphite materials (where ID / IG is typically less than 0.5), the higher ID / IG ratio of FMBC-800 indicates the presence of numerous defect sites within the carbon framework. These defect sites can serve as additional active centers for PMS activation, promoting electron transfer and the generation of reactive oxygen species. Additionally, these defect sites facilitate the anchoring and dispersion of metal oxides, enhancing catalyst stability. Therefore, a moderate level of structural defects has a positive effect on catalytic performance.

[0040] 5. XRD Analysis The crystal structure and phase composition of FMBC were analyzed using X-ray diffraction (XRD), and the results are as follows: Figure 6 As shown, the XRD pattern exhibits a series of diffraction peaks at 2θ = 24.02°, 26.48°, 30.08°, 33.10°, 37.10°, 39.36°, 43.22°, and 57.22°. The strong diffraction peak at 26.48° is attributed to the (002) crystal plane of graphitized carbon, indicating the presence of a certain degree of graphitized carbon structure in the biochar matrix. The remaining diffraction peaks match the standard card for iron-manganese oxides, confirming the successful loading of the iron-manganese composite oxide.

[0041] Specifically, the diffraction peaks near 33.10° and 37.10° can be attributed to the characteristic diffraction of the MnFe2O4 spinel phase, while the diffraction peaks at 30.08°, 43.22°, and 57.22° may be related to a mixed phase of Fe2O3, Mn3O4, or Fe-Mn composite oxides. Furthermore, the diffraction peaks exhibit a certain degree of broadening, indicating that the iron-manganese oxide grains are small, at the nanoscale. Nanoscale grain size is beneficial for exposing more surface atoms and active sites, thus enhancing catalytic activity.

[0042] XRD analysis results corroborate SEM and Raman characterization: nanoscale iron-manganese oxide particles are uniformly loaded on the surface of biochar with a certain degree of graphitization, forming a structurally stable composite catalytic material.

[0043] II. The Influence of Different Systems on Degradation Performance To clarify the role of each component in the TA degradation process, this invention compared the degradation effects of five systems on TA: FMBC (FMBC-800) alone, PMS alone, H2O2 alone, FMBC / PMS, and FMBC / H2O2. The results are as follows: Figure 7 ([TA] = 100 mg / L, pH = 7, [FMBC] = 1 g / L, [PMS] = 0.1 mol / L, [H2O2] = 3%) and as shown in Table 1. When PMS or H2O2 is introduced alone, the degradation rate of TA within 90 min is close to 0%, and the corresponding pseudo-first-order kinetic constants are 1.77 × 10⁻⁶. -4 min -1 and 1.78×10 -4 min -1 This result indicates that, in the absence of a catalyst, PMS and H2O2 themselves are unable to rapidly generate reactive oxygen species with strong oxidizing capabilities, and their ability to oxidize and degrade TA is extremely limited.

[0044] When 1.0 g / L FMBC was added alone, the removal rate of TA reached 53.07% within 90 min, with a kinetic constant of 0.0198 min. -1 This removal efficiency is mainly attributed to the adsorption of TA by FMBC, which is consistent with the conclusions drawn from BET analysis that FMBC has a high specific surface area (67.79 m² / g) and a hierarchical porous structure. The porous structure of biochar exhibits excellent adsorption and enrichment capabilities for TA molecules.

[0045] When 1.0 g / L FMBC was combined with 0.1 mol / L PMS, the FMBC / PMS system exhibited the best degradation performance, with a TA removal rate of up to 97.52% within 90 min and a kinetic constant increased to 0.1118 min. -1These values ​​are 631.64 times that of the PMS system alone and 628.09 times that of the H2O2 system alone. The R² value of the FMBC / PMS system reaches 0.969, indicating that the pseudo-first-order kinetic model can fit the experimental data well. The significantly improved degradation efficiency proves that FMBC can effectively activate PMS to produce highly reactive oxygen species such as SO4·⁻ and ·OH.

[0046] When 1.0 g / L FMBC is combined with 3% H2O2, the degradation efficiency of the FMBC / H2O2 system reaches only 88.56%, with a kinetic constant of 0.0685 min. -1 The oxidation potential of SO4·⁻ was significantly lower than that of the FMBC / PMS system. This difference may be related to the differences in the molecular structures of PMS and H₂O₂: PMS has an asymmetric peroxy bond structure, making it more prone to heterolytic cleavage to form SO₄·⁻ under the action of transition metals; while the OO bond of H₂O₂ is more symmetrical, resulting in a relatively higher activation energy barrier. In addition, SO₄·⁻ generated by PMS activation has a higher oxidation potential and a longer lifetime than ·OH, which is beneficial for the deep oxidation of pollutants.

[0047] Based on the above comparison results, the FMBC / PMS system was selected for further in-depth research in subsequent experiments.

[0048] Table 1. Kinetic analysis of TA degradation under different reaction systems III. The Influence of Different Factors on Degradation Performance 1. Effect of FMBC preparation conditions on degradation performance Pyrolysis temperature is a key factor affecting the structure and performance of biochar-based catalytic materials. This invention investigated the degradation effect of FMBC prepared at five pyrolysis temperatures (500℃, 600℃, 700℃, 800℃, and 900℃) on TA. The results are as follows: Figure 8 ([TA]=100 mg / L, pH=7, [FMBC]=1 g / L, [PMS]=0.1mol / L) and as shown in Table 2.

[0049] After 40 min of degradation, the TA degradation rates of FMBC-500, FMBC-600, FMBC-700, FMBC-800, and FMBC-900 were 92.74%, 93.58%, 95.26%, 97.52%, and 89.75%, respectively, with corresponding kinetic constants of 0.0272 min. -1 0.0241 min -1 0.0330 min -1 0.0440 min -1 and 0.0023 min -1Among them, FMBC-800 exhibited the best catalytic activity, with a k-value 19.1 times that of FMBC-900.

[0050] The catalytic activity initially increases and then decreases with pyrolysis temperature, which can be explained by the following three aspects. First, a moderate pyrolysis temperature (700–800℃) is conducive to the formation of a well-developed porous structure and high specific surface area in biochar, providing ample space for the loading and dispersion of iron-manganese oxide nanoparticles. BET analysis results show that FMBC-800 has a specific surface area of ​​67.79 m² / g and a hierarchical pore structure with micropores, mesopores, and macropores coexisting. Second, a higher pyrolysis temperature helps to more thoroughly remove organic matter and other impurities adsorbed on the biochar surface, exposing more active sites. Third, the pyrolysis temperature affects the crystal phase structure and crystallinity of iron-manganese oxides. XRD analysis shows that the iron-manganese oxides in FMBC-800 mainly exist in the form of nanoscale spinel phase and mixed oxides. This stable structure has high surface energy and catalytic activity.

[0051] However, when the pyrolysis temperature rises to 900℃, the catalytic activity decreases sharply. This is mainly because excessively high pyrolysis temperatures lead to significant grain growth of iron-manganese oxides, reducing the specific surface area and the number of active sites. Simultaneously, excessive graphitization may cause extensive decomposition of oxygen-containing functional groups on the biochar surface, weakening the synergistic effect between the support and the metal oxide. Therefore, 800℃ was determined to be the optimal preparation temperature for FMBC.

[0052] Table 2. Kinetic analysis of TA degradation under different FMBC preparation conditions 2. Effect of PMS dosage on degradation performance As an oxidant and free radical precursor, the dosage of PMS directly affects the generation rate and concentration of reactive oxygen species. This invention investigated the effect of different initial PMS concentrations in the range of 0.05–0.15 mol / L on TA degradation, and the results are as follows: Figure 9 ([TA]=100 mg / L, pH=7, [FMBC]=1 g / L) and as shown in Table 3.

[0053] When the PMS concentration increased from 0.05 mol / L to 0.08 mol / L, the degradation rate of TA increased from 90.66% to 97.52%, and the kinetic constant increased from 0.0401 min / L. -1 Increased to 0.0758 min -1The improved degradation efficiency can be attributed to the increased collision frequency between PMS molecules and active sites on the catalyst surface: at lower PMS concentrations, the active sites on the catalyst surface are not fully occupied, and increasing the PMS concentration can promote the activation of more PMS molecules, generating more reactive oxygen species such as SO4·⁻ and ·OH.

[0054] However, when the PMS concentration was further increased to 0.10, 0.12, and 0.15 mol / L, the degradation rate of TA decreased to 94.27%, 93.36%, and 94.27%, respectively, and the kinetic constants decreased to 0.0550, 0.0557, and 0.0546 min, respectively. -1 This inhibitory effect stems from the free radical scavenging reaction initiated by excess PMS. Specifically, excess SO4·⁻ reacts with each other to form S2O8²⁻ (reaction 2), and ·OH also reacts with SO4·⁻ to form HSO5⁻ (reaction 3). These side reactions consume the reactive oxygen species that should participate in TA degradation, leading to a decrease in overall degradation efficiency.

[0055] Taking into account both degradation efficiency and the economic cost of PMS, this invention selects 0.08 mol / L as the optimal PMS dosage.

[0056] Table 3. Kinetic analysis of TA degradation under different PMS dosages 3. Effect of FMBC dosage on degradation performance The catalyst dosage determines the total number of active sites in the reaction system and the reaction rate of PMS activation. This invention investigated the effect of FMBC dosage in the range of 0.5–1.5 g / L on TA degradation, and the results are as follows: Figure 10 ([TA]=100 mg / L, pH=7, [PMS]=0.1mol / L) and as shown in Table 4.

[0057] When the FMBC dosage was gradually increased from 0.5 g / L to 1.2 g / L, the degradation rate of TA increased from 81.05% to 97.52%, and the kinetic constant increased from 0.0390 min⁻¹. -1 Increased to 0.0775 min -1 Increasing the FMBC dosage by 0.7 g / L increased the k-value to 1.99 times the original value. This positive dependence indicates that at lower catalyst dosages, the number of available active sites in the reaction system is insufficient, limiting the activation efficiency of PMS and the generation rate of reactive oxygen species.

[0058] However, when the FMBC dosage was further increased from 1.2 g / L to 1.5 g / L, the degradation rate of TA decreased from 97.52% to 95.24%, and the k value decreased from 0.0775 min. -1 Reduced to 0.0663 min -1 This inhibitory effect can be explained in two ways. First, excessive catalyst particles aggregate in the solution, reducing the exposed area of ​​effective active sites and decreasing the activation efficiency of PMS per unit mass of catalyst. Second, excessively high catalyst dosages may lead to ineffective consumption by free radicals or side reactions of PMS. Previous studies have shown that at higher catalyst dosages, the removal rate of pollutants reaches its maximum and then tends to decline due to free radical scavenging or ineffective consumption by PMS.

[0059] Therefore, taking into account both degradation efficiency and catalyst utilization efficiency, this invention selects 1.2 g / L as the optimal FMBC dosage.

[0060] Table 4. Kinetic analysis of TA degradation under different FMBC dosages 4. Effect of initial pH value on degradation performance The initial pH of the solution is a crucial factor affecting the catalytic reaction, influencing not only the speciation of PMS and the leaching behavior of metal ions, but also the surface charge of the catalyst and the ionization state of contaminants. This invention investigated the degradation effect of TA within the pH range of 3–11, and the results are as follows: Figure 11 ([TA]=100 mg / L, [FMBC]=1 g / L, [PMS]=0.1 mol / L) and as shown in Table 5. At initial pH values ​​of 3, 5, 7, 9, and 11, the TA removal rates after 90 min were 90.08%, 90.46%, 97.52%, 88.77%, and 87.08%, respectively. The FMBC / PMS system maintained high catalytic activity over a wide pH range (3–11), indicating good pH adaptability. The initial pH had a relatively small effect on TA degradation; lower degradation efficiency was observed under alkaline conditions. Under alkaline conditions, the oxidation activity weakened because ·OH reacts with SO42-. ·- The reaction produces OH - The reaction between ·OH and ·OH to form water reduces the formation of free radicals, thereby decreasing the degradation rate of TA. Furthermore, the Fe dissolved in FMBC... 3+ and Mn 2+ Under alkaline conditions, it reacts with OH-. - The reaction produces Fe(OH)3 and Mn(OH)2, thereby weakening the Fe content in the reaction system. 3+ and Mn 2+The activation effect. In a strongly acidic environment, PMS reacts with H₂SO₅ instead of HSO₅. - The presence of certain substances leads to a slightly lower removal rate compared to neutral conditions. The FMBC / PMS system exhibits higher degradation efficiency under weakly acidic and partially neutral conditions than under alkaline conditions. This may be due to the leaching of more metal ions as PMS is uniformly activated, resulting in the generation of additional free radicals. The high adaptability of the FMBC / PMS system to different solution pH values ​​ensures its promising application in treating practical TA wastewater.

[0061] Table 5. Kinetic analysis of TA degradation at different initial pH levels 6. Effects of common anions on degradation performance Inorganic anions (such as HCO3⁻, NO3⁻, Cl⁻, and SO4²⁻) that are commonly found in real water bodies may have a significant impact on advanced oxidation processes. This invention investigated the effects of different concentrations of anions on the degradation of TA in the FMBC / PMS system, and the results are as follows: Figure 12 As shown ([TA]=100 mg / L, pH=7, [FMBC]=1.2 g / L and [PMS]=0.08 mol / L).

[0062] Under low concentration (10 mmol / L) conditions, HCO3⁻, NO3⁻, Cl⁻, and SO4²⁻ had almost no inhibitory effect on the degradation of TA, with degradation rates of 94.92%, 93.69%, 96.15%, and 97.69% respectively within 30 min. This result indicates that the FMBC / PMS system has good anti-interference ability and practical application potential in low-salinity water bodies.

[0063] With increasing anion concentration, different anions exhibited differentiated effects. HCO3⁻ showed the most significant inhibitory effect: as the HCO3⁻ concentration increased from 0 mmol / L to 500 mmol / L, the TA removal rate continuously decreased from 97.52% to 62.77%. This is attributed to a synergistic effect of two factors. Firstly, SO4·⁻ reacts with HCO3⁻ to form HCO3· (reaction 4), and the redox potential of HCO3· (1.6 V) is much lower than that of SO4·⁻ (2.5–3.1 V), weakening the system's oxidation capacity. Secondly, HCO3⁻ possesses a strong metal complexing ability and can react with Fe. 3+ and Mn 2+ It forms a complex and inhibits the activation of PMS.

[0064] Cl -The effect on TA degradation was relatively limited. When the Cl⁻ concentration increased from 0 mmol / L to 50 mmol / L, the TA degradation rate only decreased from 97.52% to 86.77%. Although the Cl· generated from the reaction of SO₄·⁻ and Cl⁻ has a relatively low redox potential (2.09 V), the reaction between SO₄·⁻ and Cl⁻ is reversible (reaction equation 5-6), with a forward rate constant (2.7~3.4×10⁻). 8 M⁻¹·s⁻¹) and reverse rate constant (2.0~2.5×10) 8 The concentrations of SO⁻¹·s⁻¹ are very close. This reversible reaction maintains the effective concentration of SO⁻ in the system to some extent.

[0065] SO4²⁻ has the least impact on TA degradation. Even when the SO4²⁻ concentration increases to 100 mmol / L, the TA degradation rate remains at 94.46%. This is likely the result of two opposing effects canceling each other out. On one hand, to maintain local charge balance, Fe³⁺ and Mn²⁺ co-migrate with negatively charged SO4²⁻, increasing the dissolution rate of metal ions and the activation efficiency of PMS. On the other hand, SO4²⁻ can inhibit electron transfer mechanisms, reducing the generation of reactive oxygen species. The combined effect of these two effects results in SO4²⁻ having almost no net impact on TA degradation.

[0066] NO3⁻ also showed a significant inhibitory effect. When the NO3⁻ concentration increased to 50 mmol / L, the degradation efficiency of TA decreased to 65.54%. This is mainly because SO4·⁻ was consumed by NO3⁻, generating NO3· with lower oxidizing power (reaction formula 7), which was insufficient to effectively degrade TA.

[0067] IV. Investigation of the Degradation Reaction Mechanism 1. TOC removal under optimal reaction conditions To assess the mineralization degree of TA in the FMBC / PMS system, total organic carbon (TOC) analysis was performed on 100 mg / L TA under optimal reaction conditions (pH=7, FMBC=1.2 g / L, PMS=0.08 mol / L). The results are as follows: Figure 13 As shown ([TA]=100mg / L, pH=7, [FMBC]=1.2g / L, [PMS]=0.08mol / L).

[0068] After 5 min of reaction, the TOC content of the TA solution decreased from the initial 56.60 mg / L to 35.47 mg / L, with a TOC removal rate of 37.33%. This rapid initial mineralization indicates that the TA molecule contains fragile structures (such as phenolic hydroxyl groups and ester bonds) that are easily attacked by reactive oxygen species. After 30 min of reaction, the TOC content further decreased to 22.13 mg / L, with a TOC removal rate of 60.9%.

[0069] The high TOC removal rate reflects that the FMBC / PMS system not only efficiently degrades TA molecules but also further mineralizes most of the degradation intermediates into CO2 and H2O. However, the TOC did not drop to 0 after the reaction, indicating that some stable intermediates that are difficult to further oxidize were generated during the TA degradation process. These intermediates may include small molecule organic acids. A TOC removal rate of 60.9% is relatively high in PMS-based catalytic oxidation systems, demonstrating that the FMBC / PMS system can effectively reduce the total amount of organic pollutants in water during TA degradation, thus mitigating their potential harm to aquatic ecosystems.

[0070] 2. Identification of active species To identify the main reactive oxygen species involved in TA degradation in the FMBC / PMS system, a free radical quenching experiment was conducted. Ethanol (EtOH) was selected as a co-quencher for SO4·⁻ and ·OH, and tert-butanol (TBA) as a selective quencher for ·OH. EtOH exhibited high reaction rate constants for both free radicals, while the reaction rate constant of TBA with ·OH was much higher than that with SO4·⁻. Therefore, TBA can selectively quench ·OH.

[0071] like Figure 14 (TA=100 mg / L; pH=7; FMBC=1.2 g / L; PMS=0.08 mol / L) and as shown in Table 6, without the addition of quencher, the degradation rate of TA within 30 min was 97.52%, and the kinetic constant was 0.0867 min. -1 When different concentrations of EtOH were added, the degradation rate of TA decreased to 65.08%, and the average kinetic constant (k1) was 0.0361 min. -1 When different concentrations of TBA were added, the degradation rate of TA decreased to 77.54%, and the average kinetic constant (k2) was 0.0481 min. -1 .

[0072] Based on the kinetic data from the quenching experiment, the contribution rate of each active species was calculated using the following formula: Table 6. Kinetic analysis of TA degradation under different quenching conditions Calculations show that SO4·⁻ contributes 13.84% to TA degradation, while ·OH contributes 44.52%. ·OH is the most dominant reactive species in the FMBC / PMS system for TA degradation, with a significantly higher contribution than SO4·⁻. This result differs from the traditional transition metal / PMS system where SO4·⁻ dominates, possibly due to the following factors: First, oxygen-containing functional groups (such as -OH) on the biochar surface can promote the conversion of SO4·⁻ to ·OH. Second, water molecules in the reaction system can react with SO4·⁻ to generate ·OH. Third, hydroxyl groups on the FMBC surface (at 3382 cm⁻ in FTIR)... -1 The broad peak at [location missing] can serve as an additional source of ·OH generation. Notably, quenching experiments show that the combined contribution of SO4·⁻ and ·OH is 58.36%, leaving approximately 41.64% of the degradation contribution unexplained by EtOH and TBA quenching experiments. This remaining degradation contribution may originate from non-radical pathways (such as ¹O2) or direct electron transfer processes on the catalyst surface.

[0073] 3. Investigation of catalytic mechanism Based on the above experimental results and existing literature reports, the possible reaction mechanism of FMBC / PMS system activating PMS to degrade TA is proposed as follows: (1) Synergistic redox cycle of iron-manganese bimetals Fe on the surface of FMBC 3+ and Mn 2+ / Mn 3+ This is the core active site for PMS activation. As a peroxide, PMS (HSO5⁻)'s O₂ bonds can undergo heterolytic or homolytic cleavage under the influence of transition metals, generating reactive oxygen species. Specifically, Fe... 3+ It can be reduced to Fe by PMS 2+ Simultaneously, PMS is oxidized to SO5·⁻ (reaction 8); Fe 2+ Further reaction with PMS produces SO4·⁻ and Fe. 3+ (Reaction 9). Similarly, Mn 2+ It can react with PMS to generate Mn 3+ And SO4·⁻ / ·OH (reaction formula 10), Mn 3+ It can also be reduced to Mn by PMS 2+ And SO5·⁻ is generated (reaction 11).

[0074] More importantly, Fe 3+ With Mn 2+ There is a highly efficient redox synergistic effect between them: Fe 3+ Mn 2+Reduced to Fe 2+ (Reaction 12), while Mn 3+ / Mn 4+ It can also be Fe 2+ Reduction. This electron transfer cycle between the Fe-Mn bimetals significantly accelerates the valence state transition rate of metal ions, continuously regenerating low-valence active sites, thereby enhancing the sustained activation ability of PMS.

[0075] (2) The generation and evolution of reactive oxygen species In Fe 2+ / Mn 2+ At the biochar site, activated PMS primarily generates SO4·⁻ (reactions 9-10). SO4·⁻ possesses an extremely high oxidation potential (2.5–3.1 V), enabling it to rapidly attack the phenolic hydroxyl groups and ester bonds in the TA molecule. Simultaneously, SO4·⁻ can react with water molecules or OH⁻ to generate ·OH (reactions 13-14), with an oxidation potential of 1.9–2.7 V. Free radical quenching experiments showed that ·OH contributed 44.52% to TA degradation, while SO4·⁻ contributed 13.84%, indicating that ·OH is the main active species for TA degradation in the FMBC / PMS system. This result differs from the predominantly SO4·⁻-based degradation in the traditional Fe²⁺ / PMS system, possibly because oxygen-containing functional groups on the biochar surface promote the conversion of SO4·⁻ to ·OH.

[0076] (3) Synergistic effect of biochar carrier Biochar supports play multiple synergistic roles in catalysis. First, the porous structure of biochar ensures good dispersion of iron-manganese oxide nanoparticles, preventing their aggregation and ensuring high accessibility of active sites. Second, oxygen-containing functional groups (such as C=O and -OH) on the surface of biochar can act as electron donors or electron transfer mediators, promoting the redox cycle and electron transfer of metal ions. Third, the graphitized carbon structure of biochar has good electrical conductivity, which can act as an electron pool to store and transfer electrons, further promoting the activation of PMS. Fourth, the adsorption effect of biochar can enrich TA molecules near the catalyst surface, shortening the diffusion distance between reactive oxygen species and target pollutants, and improving reaction efficiency.

[0077] (4) Degradation and mineralization of TA Reactive oxygen species such as SO4·⁻ and ·OH attack the electron-rich phenolic hydroxyl groups and ester bonds in the TA molecule, decomposing it into intermediate products such as small-molecule organic acids. TOC analysis showed that under optimal reaction conditions (pH=7, FMBC=1.2 g / L, PMS=0.08 mol / L), the TOC removal rate reached 60.9% after 30 min, indicating that most of the TA was mineralized into CO2 and H2O. However, TOC was not completely removed (approximately 39.1% remained), indicating that some TA was converted into organic intermediates that are difficult to mineralize further. LC-MS analysis will further reveal the specific degradation pathway of TA.

[0078] In summary, the efficient degradation of TA by the FMBC / PMS system is attributed to the synergistic redox cycle of iron and manganese bimetals, the multiple auxiliary effects of the biochar support, and the combined attack of reactive oxygen species such as SO4·⁻ / ·OH. The outstanding advantages of this system are: (1) a wide pH adaptation range (maintaining high activity at pH 3 to 11); (2) excellent catalytic stability; and (3) the iron and manganese oxides loaded on biochar avoid the problems of difficult metal ion recovery and secondary sludge generation in homogeneous catalysis.

[0079] V. Conclusion This invention utilizes agricultural waste tobacco stalks as raw material to prepare iron-manganese oxide-supported modified tobacco stalk biochar composites (FMBC) via impregnation-pyrolysis. The performance, influencing factors, and reaction mechanism of FMBC in activating persulfate (PMS) degradation of tannic acid (TA) were systematically investigated. The main conclusions are as follows: (1) Material characterization showed that FMBC has a hierarchical porous structure with micropores, mesopores and macropores coexisting (specific surface area 67.79 m² / g). Nanoscale iron and manganese oxides are uniformly loaded on the surface of biochar, forming a complex dominated by the MnFe2O4 spinel phase. The abundant oxygen-containing functional groups (such as -OH) and high degree of structural defects (ID / IG≈0.826) on the surface of biochar provide a favorable physicochemical environment for catalytic reactions.

[0080] (2) In terms of catalytic performance, the FMBC / PMS system showed excellent degradation efficiency for TA. Under optimal conditions (pyrolysis temperature 800℃, FMBC dosage 1.2 g / L, PMS concentration 0.08 mol / L, initial pH=7), the TA removal rate reached 97.52% within 90 min, and the pseudo-first-order kinetic constant was 0.1118 min. -1 The levels were more than 630 times higher than those of PMS and H2O2 systems alone, respectively. The TOC removal rate reached 60.9%, indicating that the system has good mineralization capabilities.

[0081] (3) pH adaptability and anti-interference ability: The FMBC / PMS system maintains high catalytic activity in a wide pH range of 3 to 11, showing good potential for practical application. In the coexistence anion experiment, low concentrations (10 mmol / L) of HCO3⁻, NO3⁻, Cl⁻ and SO4²⁻ have almost no inhibitory effect on degradation, while only high concentrations of HCO3⁻ show a significant inhibitory effect.

[0082] (4) The reaction mechanism was elucidated. Free radical quenching experiments showed that ·OH was the most important active species in the system (contributing 44.52%), SO4·⁻ contributed 13.84%, and about 41.64% of the degradation contribution may have come from non-radical pathways (such as ¹O2) or surface electron transfer processes. The high catalytic activity of FMBC is attributed to the synergistic redox cycle between Fe-Mn bimetals, the adsorption and enrichment effect and electron transfer function of the biochar support, and the combined attack of reactive oxygen species on the phenolic hydroxyl and ester bond structures in the TA molecule.

[0083] In summary, the iron-manganese oxide-supported biochar composite material prepared using tobacco straw as a precursor in this invention can efficiently activate PMS to degrade tannic acid. It exhibits excellent catalytic performance, wide pH adaptability, and good stability, realizing the environmentally friendly concept of "treating waste with waste." This provides a feasible technical solution for the resource utilization of tobacco straw waste and the advanced oxidation treatment of tannic acid wastewater. Future research can further explore the treatment effect of this system on actual industrial wastewater and evaluate its long-term economic viability.

[0084] The above are merely preferred embodiments of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for preparing an iron-manganese oxide-supported tobacco straw biochar composite oxygen carrier, characterized in that, Includes the following steps: S1. Mix tobacco stalk powder with a mixed solution containing iron salt and manganese salt, sonicate and stir, filter, wash and dry to obtain the precursor; S2. The precursor is pyrolyzed under an inert atmosphere at a temperature of 500-900℃. After pyrolysis, it is ground and sieved to obtain the iron-manganese oxide-supported tobacco biochar composite oxygen carrier.

2. The method for preparing an iron-manganese oxide-supported tobacco straw biochar composite oxygen carrier according to claim 1, characterized in that, In step S1, the iron salt is FeCl2 and the manganese salt is KMnO4.

3. The method for preparing an iron-manganese oxide-supported tobacco straw biochar composite oxygen carrier according to claim 1, characterized in that, In step S1, the ultrasonic treatment time is 30 minutes, and the stirring is hydrothermal stirring for 6 hours.

4. The method for preparing an iron-manganese oxide-supported tobacco straw biochar composite oxygen carrier according to claim 1, characterized in that, In step S2, the pyrolysis heating rate is 5℃ / min, and the pyrolysis time is 2h.

5. The method for preparing an iron-manganese oxide-supported tobacco straw biochar composite oxygen carrier according to claim 1, characterized in that, In step S2, the pyrolysis temperature is 800℃.

6. A composite oxygen carrier consisting of iron-manganese oxide-supported tobacco straw biochar, characterized in that, It is prepared by the preparation method described in any one of claims 1-5.

7. The application of the iron-manganese oxide-supported tobacco biochar composite oxygen carrier as described in claim 6 in the degradation of organic pollutants by activated persulfate.

8. The application of the iron-manganese oxide-supported tobacco biochar composite oxygen carrier according to claim 7 in the degradation of organic pollutants by activated persulfate, characterized in that, The organic pollutant is tannic acid.

9. The application of the iron-manganese oxide-supported tobacco biochar composite oxygen carrier according to claim 7 in the degradation of organic pollutants by activated persulfate, characterized in that, The dosage of the iron-manganese oxide-supported tobacco biochar composite oxygen carrier is 0.5-1.5 g / L, and the dosage of the persulfate is 0.05-0.15 mol / L.

10. The application of the iron-manganese oxide-supported tobacco biochar composite oxygen carrier according to claim 7 in the degradation of organic pollutants by activated persulfate, characterized in that, The initial pH of the reaction system used in this application is 3-11.