A porous high-entropy alloy-oxide composite aerogel catalyst and its preparation method

A high-entropy alloy-oxide composite aerogel catalyst was prepared by combining propylene oxide-induced hydrolysis and condensation of multi-principal metal ions with supercritical carbon dioxide drying, low-temperature reduction, and medium-temperature crystallization. This solved the problems of easy catalyst dissolution, low specific surface area, and pore destruction in existing technologies, and achieved efficient and stable pollutant removal.

CN123102380APending Publication Date: 2026-11-17BEIJING NORMAL UNIVERSITY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611286682.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing heterogeneous persulfate activated catalysts have active metal components that are easily leached out, and their activity decays significantly after multiple cycles, with the risk of secondary pollution from heavy metals. Existing high-entropy catalytic materials have low specific surface area, lack three-dimensional interconnected channels, and have low utilization of internal active sites. Existing aerogel preparation methods destroy nanopores, making it difficult to obtain high specific surface area. Existing heat treatment processes lack segmented control, resulting in excessive growth of nanocrystals and sintering collapse of the framework.

Method used

Propylene oxide was used to induce the simultaneous hydrolysis and condensation of multiple principal metal ions in a homogeneous system. Combined with supercritical carbon dioxide drying to retain three-dimensional interconnected nanopores, a high-entropy alloy-oxide composite aerogel was formed through a two-stage heat treatment of low-temperature reduction and medium-temperature crystallization. The hysteresis diffusion effect was used to inhibit grain growth and promote electron redistribution and synergistic cycling of the metal-oxide heterostructure interface.

Benefits of technology

The catalyst was able to efficiently activate persulfate over a wide pH range, generating active species. The catalyst's specific surface area was increased by more than 6 times, the alloy nanocrystal size was stable, and the removal rate of target pollutants was no less than 92% after 5 cycles. Furthermore, the catalyst could be magnetically separated and recovered.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102380A_ABST
    Figure CN123102380A_ABST
Patent Text Reader

Abstract

This invention discloses a porous high-entropy alloy-oxide composite aerogel catalyst and its preparation method, belonging to the field of environmental functional materials technology. The method uses transition metal nitrates as raw materials, induces homogeneous gelation with propylene oxide to obtain a monolithic wet gel, and then prepares a high-entropy oxide aerogel through aging, ethanol replacement, and supercritical carbon dioxide drying. A two-stage heat treatment of reduction and crystallization in a hydrogen-argon mixture is then performed, causing face-centered cubic high-entropy alloy nanocrystals to be in situ embedded within a spinel-type high-entropy oxide framework, allowing for selective loading of platinum, palladium, or ruthenium. This invention solves the problems of low specific surface area, easy dissolution of metal components, and poor cycle stability in existing catalysts. It is used to activate persulfate to remove recalcitrant organic pollutants such as tetracycline, and allows for magnetic separation and recovery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of environmental functional materials technology, and specifically relates to a porous high-entropy alloy-oxide composite aerogel catalyst, its preparation method and application. Background Technology

[0002] With the rapid development of industries such as pharmaceuticals, fine chemicals, and textile printing and dyeing, the discharge of industrial wastewater containing recalcitrant organic pollutants such as tetracycline antibiotics, sulfonamide antibiotics, phenols, and azo dyes continues to increase. These pollutants have stable molecular structures and strong biotoxicity, and conventional biological treatment processes such as activated sludge processes have limited removal rates, often resulting in effluent that fails to consistently meet industry standards. Therefore, there is an urgent need to develop efficient advanced treatment technologies.

[0003] Advanced persulfate oxidation technology, using persulfate and perdisulfate as oxidants, generates reactive species such as sulfate radicals by activating peroxy bonds through catalyst activation. It boasts advantages such as high oxidation potential, a wide effective pH range, and convenient storage and transportation of the oxidant, making it an important technical route for the deep treatment of recalcitrant organic wastewater. The core of this technology lies in a highly active and stable heterogeneous activation catalyst.

[0004] Existing heterogeneous activation catalysts are mostly based on single transition metal oxides or binary / ternary spinel oxides. These catalysts have significant shortcomings in continuous operation: firstly, the active metal component is prone to dissolution in acidic or strongly oxidizing systems, leading not only to rapid catalytic activity decay but also to secondary pollution from dissolved cobalt and nickel ions; secondly, these catalysts are mostly dense powders with a specific surface area typically below 100 m². 2 / g, the internal active sites are difficult to utilize effectively.

[0005] High-entropy materials refer to multi-principal-component solid solution materials composed of five or more principal components in equimolar or near-equimolar ratios, with a configurational entropy of not less than 1.5R. Their high configurational entropy effect is conducive to the formation of single-phase solid solutions, the hysteresis diffusion effect can significantly inhibit atomic migration and grain growth under high-temperature conditions, and the lattice distortion effect can regulate the surface electronic structure. These characteristics give high-entropy materials a natural advantage in terms of resistance to sintering and dissolution. However, the mainstream preparation methods for high-entropy catalytic materials (such as mechanical alloying, arc melting, carbothermal shock, coprecipitation-high-temperature calcination, etc.) mostly produce bulk or low-specific-surface-area powders, making it difficult to simultaneously achieve the advantages of high-entropy components and a high-specific-surface-area porous structure.

[0006] Aerogels are a class of low-density porous materials composed of three-dimensional interconnected networks of nanoparticles or nanofibers. They possess high specific surface area and high porosity, making them ideal frameworks for constructing highly dispersed catalytic materials. However, the preparation of existing high-entropy aerogels generally involves freeze-drying to remove the solvent, which causes the ice crystal growth process to compress and destroy the nanoscale channels. At the same time, the subsequent reduction steps often involve a single-stage heating process to a high temperature, resulting in severe sintering of the nanoframework at high temperatures, significant collapse of the pore structure, and severe loss of specific surface area.

[0007] CN119571369A discloses a method for preparing high-entropy alloy aerogels for electrocatalysis. This method involves a one-step reduction of an inorganic metal salt, followed by static assembly to obtain a three-dimensional continuous porous network of high-entropy alloy aerogels, which can be used for the electrocatalytic reduction of nitrates to ammonia. CN118527180A discloses a high-entropy oxide aerogel composite catalyst and its preparation method. This catalyst, when applied in a concentrated solar thermal system, can effectively utilize solar energy to achieve efficient photothermal synergistic catalytic conversion of CO2 and H2O. CN118422249A discloses a high-entropy alloy aerogel catalyst, its preparation method, and its application. This catalyst utilizes sodium borohydride as a reducing agent and ammonium fluoride as an ion regulator to control the growth of the high-entropy alloy aerogel, resulting in the formation of a network-structured metal aerogel, which is then applied to the electrocatalytic reduction of nitrates to ammonia. In general, high-entropy aerogels are mostly used in CO2RR and NO3RR reactions, and their application in the environmental field is still lacking.

[0008] Current research and technical solutions still have significant shortcomings, as follows:

[0009] 1) The active metal components of existing heterogeneous persulfate activated catalysts are easily leached out, and their activity decays significantly after multiple cycles, and there is a risk of secondary pollution from heavy metals.

[0010] 2) Existing methods for preparing high-entropy catalytic materials result in products with low specific surface area, lack of three-dimensional interconnected channels, and low utilization of internal active sites.

[0011] 3) Existing aerogel desolvation processes severely damage nanopores, making it difficult to obtain high-entropy aerogels with high specific surface area;

[0012] 4) Existing heat treatment processes use single-stage heating for direct high-temperature reduction, lacking segmented control over the reduction and crystallization processes, resulting in excessive growth of nanocrystals and sintering collapse of the framework. Summary of the Invention

[0013] This invention is made in view of the problems existing in the prior art. The purpose of this invention is to provide a porous high-entropy alloy-oxide composite aerogel catalyst, its preparation method and application, so as to solve the technical problems of low specific surface area, easy dissolution of metal components and poor cycle stability of existing heterogeneous persulfate activated catalysts.

[0014] This invention uses propylene oxide as a proton scavenger to induce the simultaneous hydrolysis and condensation of multiple principal metal ions in a homogeneous system, achieving uniform mixing of more than five transition metals at the molecular scale to obtain a monolithic wet gel. Subsequently, supercritical carbon dioxide drying is used to eliminate capillary tension at the gas-liquid interface, completely preserving the three-dimensional interconnected nanopores. Finally, through a two-stage atmospheric heat treatment of low-temperature reduction and medium-temperature crystallization, under the effect of the hysteretic diffusion of the high-entropy system, high-entropy alloy nanocrystals with a face-centered cubic structure are precipitated in situ and uniformly embedded in a high-entropy oxide framework with a spinel structure, forming a rich alloy / oxide heterogeneous interface.

[0015] The mechanism of action of this invention lies in the fact that the hysteresis diffusion effect increases the migration barrier of atoms in the crystal lattice, enabling the nanocrystals to maintain a size of 5-15 nm without significant growth during crystallization at 600-700 °C; the electron redistribution at the alloy / oxide heterojunction promotes the synergistic cycling of multiple redox couples such as iron, cobalt, and manganese, accelerates the breaking of peroxy bonds in persulfate molecules and generates active species such as sulfate radicals and hydroxyl radicals; at the same time, the lattice distortion caused by the coexistence of multiple principal elements increases the bonding strength of metal-oxygen bonds, and thermodynamically inhibits the dissolution of active metal components.

[0016] To achieve the above objectives, the present invention provides a method for preparing a porous high-entropy alloy-oxide composite aerogel catalyst, characterized in that the method includes the following steps:

[0017] Step 1: Weigh out five or more transition metal nitrates, namely ferric nitrate, cobalt nitrate, nickel nitrate, copper nitrate, and manganese nitrate, in an equimolar ratio. Dissolve them in a mixed solvent of deionized water and anhydrous ethanol, wherein the volume ratio of deionized water to anhydrous ethanol in the mixed solvent is 1:1. Control the total concentration of metal ions to be 0.4~0.6 mol / L. Stir magnetically at 300 r / min for 20~30 min at 20~30 ℃ and relative humidity below 60% until the solid is completely dissolved and the solution is clear and free of precipitate to obtain a homogeneous precursor solution.

[0018] Step 2: Under continuous stirring, propylene oxide is added to the homogeneous precursor solution in one step. The molar ratio of propylene oxide to metal ions is 8:1 to 12:1. Stirring is continued at 300 r / min for 3 to 5 min, and then stirring is stopped. The solution is allowed to stand at 20 to 30°C for 2 to 6 h. The propylene oxide ring-opening process abstracts protons, causing the pH of the system to rise slowly. The metal ions hydrolyze and condense to form a three-dimensional interconnected network, resulting in a monolithic wet gel.

[0019] Step 3: Seal the wet gel together with the mother liquor and age it at 45~55 ℃ for 20~28 h to further condense and strengthen the network skeleton. After aging, allow it to cool naturally to room temperature.

[0020] Step 4: Use anhydrous ethanol as the replacement solvent, with an amount three times the volume of the wet gel. Replace the replacement solvent every 12 hours, repeating 3 to 5 times. The replacement process temperature is 20 to 30 °C. Continue until the mass fraction of residual water in the gel is less than 0.5%, and you will get an alcohol gel.

[0021] Step 5: Transfer the alcohol gel to a supercritical drying reactor, seal it, and introduce liquid carbon dioxide. Replace the ethanol in the reactor for 4-8 hours at a pressure of 8-10 MPa and a temperature of 15-20 °C, during which alcohol-containing carbon dioxide is discharged and fresh liquid carbon dioxide is replenished every hour. After replacement, raise the temperature to 40-45 °C and the pressure to 12-15 MPa to convert the carbon dioxide in the reactor to a supercritical state and maintain this state for 1-2 hours. Then, under constant temperature conditions, slowly depressurize to atmospheric pressure at a rate of 0.5 MPa / h, and remove the gel to obtain a porous high-entropy oxide aerogel with a specific surface area of ​​250-350 m². 2 / g, pore volume 1.2~1.6 cm³ 3 / g, apparent density is 0.06~0.12 g / cm³ 3 ;

[0022] Step 6: Place the porous high-entropy oxide aerogel in a tubular atmosphere furnace, and introduce a hydrogen-argon mixture with a hydrogen volume fraction of 5% at a flow rate of 100 mL / min. First, heat the aerogel to 450-550 ℃ at a heating rate of 3 ℃ / min and hold it for 2-3 h to complete the partial reduction of the oxide to the alloy phase. Then, heat the aerogel to 600-700 ℃ at a heating rate of 2 ℃ / min and hold it for 1-2 h to complete the crystallization of the alloy nanocrystals and the reconstruction of the heterostructure interface. After the holding period, cool the aerogel to room temperature with the furnace, and then passivate it with an oxygen-argon mixture with an oxygen volume fraction of 0.5% for 2 h to obtain a porous high-entropy alloy-oxide composite aerogel.

[0023] Step 7: The porous high-entropy alloy-oxide composite aerogel is impregnated in a soluble salt solution containing platinum, palladium or ruthenium, with the theoretical loading mass fraction of the noble metal controlled at 0.3%~1.0%. It is first ultrasonically dispersed at 40 kHz and 150 W for 30 min at 20~30 ℃, then allowed to stand for impregnation for 4~6 h, followed by rotary evaporation to dryness at 60 ℃, drying at 105 ℃ for 4 h, and finally reduced at 300 ℃ for 1 h in a hydrogen-argon mixture with a hydrogen gas fraction of 5% to obtain the porous high-entropy alloy-oxide composite aerogel catalyst.

[0024] Step 8: Add the porous high-entropy alloy-oxide composite aerogel catalyst to the wastewater to be treated at a dosage of 0.1~0.5 g / L, and simultaneously add persulfate or perdisulfate as an oxidant at a dosage of 0.5~2.0 mmol / L. React for 20~60 min at a temperature of 20~40 ℃, pH 3~10, and mechanical stirring speed of 200~400 r / min. After the reaction, the catalyst is magnetically separated and recovered within 5~10 min using a 0.3~0.5 T permanent magnet. The recovered catalyst is washed with deionized water, vacuum dried at 60 ℃ for 6 h, and then reused.

[0025] For the above technical solution, further specified, the number of principal components of the transition metal nitrates in step 1 is 5 to 6, and the mole fraction of each principal component is 1 / N, where N is the number of principal components, and the configuration entropy of the system is expressed as ΔS. conf =-R·Σx i ·lnx i Calculate at least 1.5R, where R is the molar gas constant, and x i Let be the mole fraction of the i-th principal component.

[0026] For the above technical solution, further specified, in the porous high-entropy alloy-oxide composite aerogel obtained in step 6, the face-centered cubic high-entropy alloy nanocrystals are uniformly embedded in the spinel high-entropy oxide framework, the average grain size of the alloy nanocrystals is 5~15 nm, and the specific surface area of ​​the composite aerogel is 150~220 m². 2 / g, with a saturation magnetization of 18~32 emu / g.

[0027] For the above technical solution, further specified, in the two-stage atmosphere heat treatment described in step 6, there is no cooling or gas exchange between the reduction stage and the crystallization stage, and the hydrogen-argon mixture is continuously introduced throughout the process to avoid re-oxidation of intermediate products.

[0028] For the above technical solution, it is further specified that the wastewater to be treated in step 8 is industrial wastewater containing tetracycline, sulfonamide, phenol, bisphenol or azo dye recalcitrant organic pollutants, and the initial mass concentration of the target pollutant is 10~200 mg / L.

[0029] The advantages of this invention are:

[0030] 1) This invention adopts a route that combines epoxide-induced gelation with supercritical carbon dioxide drying, avoiding the damage to the pores caused by capillary tension and ice crystal growth during atmospheric pressure drying and freeze drying. The specific surface area of ​​the resulting high-entropy oxide aerogel is more than 6 times higher than that of the atmospheric pressure dried control sample, providing a structural basis for the full exposure of active sites and rapid mass transfer of pollutants.

[0031] 2) This invention employs a two-stage heat treatment process of low-temperature reduction followed by medium-temperature crystallization, utilizing the inherent hysteresis diffusion effect of the high-entropy system to suppress grain growth. The average grain size of the resulting alloy nanocrystals is 5~15 nm, and the target pollutant removal rate of the composite aerogel is still not less than 92% after 5 cycles of use.

[0032] 3) The catalyst of the present invention is applicable to a pH range of 3 to 10 and can efficiently activate persulfate at room temperature and pressure of 20 to 40 °C. It has a high removal rate for recalcitrant organic pollutants such as tetracycline, sulfamethoxazole, bisphenol A, phenol and azo dyes. In addition, the catalyst is ferromagnetic and can be rapidly separated and recovered by an external magnetic field. Attached Figure Description

[0033] Various other advantages and benefits will become apparent to those skilled in the art upon reading the following detailed description of preferred embodiments. The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. In the drawings:

[0034] Figure 1 This is a schematic diagram of the preparation process of the porous high-entropy alloy-oxide composite aerogel catalyst of the present invention;

[0035] Figure 2 This is a schematic diagram of the three-dimensional interconnected framework and alloy / oxide heterostructure interface of the catalyst of the present invention;

[0036] Figure 3 The degradation rate of tetracycline in Example 1 and Comparative Examples 1 to 4 is shown as a function of reaction time.

[0037] Figure 4 The graph shows the relationship between the number of catalyst cycles and the tetracycline removal rate and the total amount of metal ions dissolved in Example 1, Comparative Examples 2 and 3. Detailed Implementation

[0038] To enable those skilled in the art to better understand the present invention, the technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of the present invention.

[0039] It should be noted that, unless otherwise specified, the embodiments and features and technical solutions in the embodiments of this invention can be combined with each other. Similar reference numerals and letters in the following figures indicate similar items; therefore, once an item is defined in one figure, it does not need to be further defined and explained in subsequent figures.

[0040] As an embodiment of the present invention, a method for preparing a porous high-entropy alloy-oxide composite aerogel catalyst is provided, the overall process flow of which is attached. Figure 1 As shown, the specific steps include the following:

[0041] Step 1: Weigh out five transition metal nitrates (ferric nitrate, cobalt nitrate, nickel nitrate, copper nitrate, and manganese nitrate) in equimolar ratio, dissolve them in a mixed solvent of deionized water and anhydrous ethanol (volume ratio of deionized water to anhydrous ethanol is 1:1), control the total metal ion concentration to be 0.4-0.6 mol / L, and magnetically stir at 300 r / min for 20-30 min at 20-30 ℃ and relative humidity below 60% until the solids are completely dissolved and the solution is clear and free of precipitate to obtain a homogeneous precursor solution.

[0042] Step 2: Under continuous stirring, propylene oxide is added to the homogeneous precursor solution in one step. The molar ratio of propylene oxide to metal ions is 8:1 to 12:1. Stirring is continued at 300 r / min for 3 to 5 min, and then stirring is stopped. The solution is allowed to stand at 20 to 30°C for 2 to 6 h. The propylene oxide ring-opening process abstracts protons, causing the pH of the system to rise slowly. The metal ions hydrolyze and condense to form a three-dimensional interconnected network, resulting in a monolithic wet gel.

[0043] Step 3: Seal the wet gel together with the mother liquor and age it at 45~55 ℃ for 20~28 h to further condense and strengthen the network skeleton. After aging, allow it to cool naturally to room temperature.

[0044] Step 4: Use anhydrous ethanol as the replacement solvent, with an amount three times the volume of the wet gel. Replace the replacement solvent every 12 hours, repeating 3 to 5 times. The replacement process temperature is 20 to 30 °C. Continue until the mass fraction of residual water in the gel is less than 0.5%, and you will get an alcohol gel.

[0045] Step 5: Transfer the alcohol gel to a supercritical drying reactor, seal it, and introduce liquid carbon dioxide. Replace the ethanol in the reactor for 4-8 hours at a pressure of 8-10 MPa and a temperature of 15-20 °C, during which alcohol-containing carbon dioxide is discharged and fresh liquid carbon dioxide is replenished every hour. After replacement, raise the temperature to 40-45 °C and the pressure to 12-15 MPa to convert the carbon dioxide in the reactor to a supercritical state and maintain this state for 1-2 hours. Then, under constant temperature conditions, slowly depressurize to atmospheric pressure at a rate of 0.5 MPa / h, and remove the gel to obtain a porous high-entropy oxide aerogel with a specific surface area of ​​250-350 m². 2 / g, pore volume 1.2~1.6 cm³ 3 / g, apparent density is 0.06~0.12 g / cm³ 3 ;

[0046] Step 6: Place the porous high-entropy oxide aerogel in a tubular atmosphere furnace, and introduce a hydrogen-argon mixture with a hydrogen volume fraction of 5% at a flow rate of 100 mL / min. First, heat the aerogel to 450-550 ℃ at a heating rate of 3 ℃ / min and hold it for 2-3 h to complete the partial reduction of the oxide to the alloy phase. Then, heat the aerogel to 600-700 ℃ at a heating rate of 2 ℃ / min and hold it for 1-2 h to complete the crystallization of the alloy nanocrystals and the reconstruction of the heterostructure interface. After the holding period, cool the aerogel to room temperature with the furnace, and then passivate it with an oxygen-argon mixture with an oxygen volume fraction of 0.5% for 2 h to obtain a porous high-entropy alloy-oxide composite aerogel.

[0047] Step 7: The porous high-entropy alloy-oxide composite aerogel is impregnated in a soluble salt solution containing platinum, palladium or ruthenium, with the theoretical loading mass fraction of the noble metal controlled at 0.3%~1.0%. It is first ultrasonically dispersed at 40 kHz and 150 W for 30 min at 20~30 ℃, then allowed to stand for impregnation for 4~6 h, followed by rotary evaporation to dryness at 60 ℃, drying at 105 ℃ for 4 h, and finally reduced at 300 ℃ for 1 h in a hydrogen-argon mixture with a hydrogen gas fraction of 5% to obtain the porous high-entropy alloy-oxide composite aerogel catalyst.

[0048] Step 8: Add the porous high-entropy alloy-oxide composite aerogel catalyst to the wastewater to be treated at a dosage of 0.1~0.5 g / L, and simultaneously add persulfate or perdisulfate as an oxidant at a dosage of 0.5~2.0 mmol / L. React for 20~60 min at a temperature of 20~40 ℃, pH 3~10, and mechanical stirring speed of 200~400 r / min. After the reaction, the catalyst is magnetically separated and recovered within 5~10 min using a 0.3~0.5 T permanent magnet. The recovered catalyst is washed with deionized water, vacuum dried at 60 ℃ for 6 h, and then reused.

[0049] For the above technical solution, further specified, the number of principal components of the transition metal nitrates in step 1 is 5 to 6, and the mole fraction of each principal component is 1 / N, where N is the number of principal components, and the configuration entropy of the system is expressed as ΔS. conf =-R·Σx i ·lnx i Calculate at least 1.5R, where R is the molar gas constant, and x i Let be the mole fraction of the i-th principal component.

[0050] For the above technical solution, further specified, in the porous high-entropy alloy-oxide composite aerogel obtained in step 6, the face-centered cubic high-entropy alloy nanocrystals are uniformly embedded in the spinel high-entropy oxide framework, the average grain size of the alloy nanocrystals is 5~15 nm, and the specific surface area of ​​the composite aerogel is 150~220 m². 2 / g, with a saturation magnetization of 18~32 emu / g.

[0051] For the above technical solution, further specified, in the two-stage atmosphere heat treatment described in step 6, there is no cooling or gas exchange between the reduction stage and the crystallization stage, and the hydrogen-argon mixture is continuously introduced throughout the process to avoid re-oxidation of intermediate products.

[0052] For the above technical solution, it is further specified that the wastewater to be treated in step 8 is industrial wastewater containing tetracycline, sulfonamide, phenol, bisphenol or azo dye recalcitrant organic pollutants, and the initial mass concentration of the target pollutant is 10~200 mg / L.

[0053] The technical solution of the present invention will be further described below through specific embodiments.

[0054] Example 1

[0055] In this embodiment, the secondary effluent from the production wastewater of an antibiotic raw material manufacturer, after hydrolysis-acidification-aerobic biochemical treatment, has the following characteristics: tetracycline concentration of 50 mg / L, chemical oxygen demand (COD) of 180 mg / L, total organic carbon of 62 mg / L, pH of 6.8, chloride ion concentration of 320 mg / L, and bicarbonate concentration of 120 mg / L. Tetracycline in this secondary effluent is difficult to remove further by biochemical processes, and the COD cannot consistently meet the emission limit of 120 mg / L required by the "Water Pollutant Discharge Standard for Fermentation Pharmaceutical Industry" (GB 21903-2008). Therefore, advanced treatment is needed to achieve a tetracycline removal rate of at least 95% and an effluent COD not exceeding 120 mg / L.

[0056] The specific preparation and application process of this embodiment is as follows:

[0057] (1) Weigh 8.08 g of ferric nitrate nonahydrate, 5.82 g of cobalt nitrate hexahydrate, 5.82 g of nickel nitrate hexahydrate, 4.83 g of copper nitrate trihydrate, and 5.02 g of manganese nitrate tetrahydrate in equimolar ratio. Each component is 0.02 mol, and the total amount of metal ions is 0.10 mol. Add 100 mL of deionized water and 100 mL of anhydrous ethanol as a mixed solvent. The total concentration of metal ions is 0.5 mol / L. Stir magnetically at 300 r / min for 25 min at 25 ℃ and 52% relative humidity to obtain a clear homogeneous precursor solution.

[0058] (2) Under continuous stirring, 56 mL of propylene oxide (0.80 mol, with a molar ratio of propylene oxide to metal ions of 8:1) was added at once, and stirring was continued at 300 r / min for 4 min. After stirring was stopped, the system was allowed to stand at 25 °C for 4 h. The system gradually changed from a clear solution to a non-flowing, monolithic wet gel.

[0059] (3) Seal the wet gel together with the mother liquor and age it at 50 °C for 24 h, then let it cool naturally to room temperature.

[0060] (4) Anhydrous ethanol was used as the replacement solvent, and the amount was 3 times the volume of the wet gel. It was replaced every 12 h for a total of 4 replacements. The replacement temperature was 25 °C. After the replacement was completed, the mass fraction of residual water in the gel was measured to be 0.31%.

[0061] (5) The alcohol gel was transferred to a supercritical drying vessel, and liquid carbon dioxide was introduced. The mixture was purged at 10 MPa and 18°C ​​for 6 h, with alcohol-containing carbon dioxide being discharged and fresh liquid carbon dioxide replenished every h. The temperature was then increased to 45°C and the pressure to 14 MPa, maintained for 1 h. The pressure was then slowly released to atmospheric pressure at a rate of 0.5 MPa / h. The obtained porous high-entropy oxide aerogel was a monolithic block, with a specific surface area of ​​312 m² as determined by nitrogen adsorption-desorption testing. 2 / g, pore volume 1.42 cm³ 3 The average pore size is 15.8 nm, and the apparent density is 0.09 g / cm³. 3 .

[0062] (6) The aerogel was placed in a tube furnace, and a hydrogen-argon mixture with a hydrogen volume fraction of 5% was introduced at a flow rate of 100 mL / min. The temperature was increased to 500 °C at 3 °C / min and held for 2 h, then increased to 650 °C at 2 °C / min and held for 1 h. After cooling to room temperature with the furnace, an oxygen-argon mixture with an oxygen volume fraction of 0.5% was introduced for passivation for 2 h. X-ray diffraction analysis showed that the product consisted of a face-centered cubic high-entropy alloy phase and a spinel-type high-entropy oxide phase. The average grain size of the alloy nanocrystals was calculated to be 8.6 nm according to the Scherrer formula, and the specific surface area was 187 m². 2 / g, apparent density is 0.14 g / cm³ 3 The saturation magnetization is 26.4 emu / g.

[0063] (7) Using an aqueous solution of chloroplatinic acid hexahydrate as the impregnation solution, the theoretical loading mass fraction of platinum was controlled at 0.5%. The platinum was first ultrasonically dispersed at 40 kHz and 150 W for 30 min at 25 °C, then allowed to stand for 4 h. It was then rotary evaporated to dryness at 60 °C, dried at 105 °C for 4 h, and finally reduced at 300 °C for 1 h in a hydrogen-argon mixture with a hydrogen gas fraction of 5% to obtain the catalyst of this embodiment. Inductively coupled plasma atomic emission spectrometry (ICP-AES) determined the actual loading mass fraction of platinum to be 0.48%.

[0064] (8) Take 1 L of the above secondary effluent, add 0.2 g / L of the catalyst of this embodiment, and add 1.0 mmol / L of potassium persulfate complex salt (calculated as potassium persulfate). React for 60 min at 25 ℃, initial pH 6.8 and mechanical stirring speed of 300 r / min. After the reaction, complete the magnetic separation and recovery of the catalyst within 8 min using a 0.4 T permanent magnet.

[0065] The implementation results of this embodiment are as follows: after 60 min of reaction, the tetracycline removal rate is 98.6%, and the apparent rate constant fitted according to pseudo-first-order kinetics is 0.070 min. -1 The total organic carbon removal rate was 68.3%, and the chemical oxygen demand in the effluent decreased from 180 mg / L to 52 mg / L, meeting the emission limits of GB 21903-2008. The total dissolved concentration of five metal ions (iron, cobalt, nickel, copper, and manganese) in the effluent was 0.31 mg / L, of which cobalt ions were 0.06 mg / L. The catalyst magnetic separation recovery rate was 98.7%, and the tetracycline removal rate remained at 92.4% after five cycles. The total dissolved concentration of metal ions in the fifth cycle was 0.44 mg / L.

[0066] Comparative Example 1

[0067] This comparative example did not use the supercritical carbon dioxide drying in step 5. Instead, the alcohol gel obtained in step 4 was directly placed in a 105 °C forced-air drying oven and dried at normal pressure for 12 h, with the remaining conditions the same as in Example 1. During the drying process, the gel volume shrank by approximately 72% and significant cracking occurred, resulting in a dry gel with a specific surface area of ​​only 43 m². 2 / g, further reduced to 21m after heat treatment in step 6. 2 / g. Under the same application conditions as in Example 1, the tetracycline removal rate was only 46.2% and the total organic carbon removal rate was only 18.7% after 60 min of reaction. This comparative example illustrates that supercritical carbon dioxide drying is a key step in preserving three-dimensional interconnected nanopores and obtaining a high specific surface area.

[0068] Comparative Example 2

[0069] This comparative example did not employ the two-stage atmosphere heat treatment in step 6. Instead, it directly heated to 650 °C at a heating rate of 3 °C / min and held at that temperature for 3 h, with all other conditions remaining the same as in Example 1. The resulting sample exhibited an increased average grain size of 26.4 nm alloy nanocrystals and a decreased specific surface area to 94 m². 2 / g. Under the same application conditions as in Example 1, the tetracycline removal rate was 71.5% and the total organic carbon removal rate was 33.6% after 60 min of reaction; after 5 cycles, the tetracycline removal rate decreased to 48.3%, and the total mass concentration of dissolved metal ions increased to 2.16 mg / L in the 5th cycle. This comparative example illustrates that segmented control of the reduction and crystallization process plays a decisive role in inhibiting grain growth and maintaining cycle stability.

[0070] Comparative Example 3

[0071] This comparative example uses only three transition metal nitrates—iron, cobalt, and nickel—as precursors, with each component in equimolar amounts. The total metal ion concentration remains at 0.5 mol / L, and all other conditions are the same as in Example 1. The configurational entropy of this ternary system, calculated using the formula, is 1.10R, which is below the high entropy criterion threshold of 1.5R. Under the same application conditions as in Example 1, the tetracycline removal rate was 88.1% after the first 60 min of reaction, but decreased to 51.6% after 5 cycles. In the 5th cycle, the total mass concentration of dissolved metal ions reached as high as 3.42 mg / L, of which cobalt ions were 1.28 mg / L. This comparative example demonstrates that when the number of principal components is insufficient and the configurational entropy does not meet the high entropy criterion, the synergistic effect of anti-dissolution and anti-sintering cannot be obtained.

[0072] Comparative Example 4

[0073] The catalyst preparation process in this comparative example is exactly the same as in Example 1, except that potassium persulfate complex salt is not added in the application step; only 0.2 g / L of catalyst is added, and the other conditions are the same as in Example 1. After 60 min of reaction, the tetracycline removal rate was 21.3%, and this removal mainly came from the physical adsorption of the catalyst, while the total organic carbon removal rate was only 3.1%. This comparative example illustrates that the catalyst of the present invention needs to be used in conjunction with a persulfate oxidant to achieve the oxidative mineralization of organic pollutants; when used alone, it only has limited adsorption effect.

[0074] Comparative Example 5

[0075] This comparative example does not include propylene oxide. Instead, in step 2, the pH of the system is adjusted to 8.0 with 25% ammonia to precipitate metal ions. The remaining conditions are the same as in Example 1. During the dropwise addition of ammonia, the system directly forms a flocculent precipitate rather than a monolithic wet gel. After solvent displacement and supercritical carbon dioxide drying, the resulting product is a loose powder with a specific surface area of ​​only 68 m². 2 / g, and energy dispersive spectroscopy showed that the distribution of the five metal elements was uneven. Under the same application conditions as in Example 1, the tetracycline removal rate was 63.8% after 60 min of reaction. This comparative example illustrates that epoxide-induced homogeneous slow gelation is a necessary condition for achieving homogeneous mixing at the multi-principal molecular level and the construction of a three-dimensional network.

[0076] Example 2

[0077] This embodiment is a variation of Example 1, with the following differences: in step 1, the total concentration of metal ions is adjusted to 0.4 mol / L; in step 2, the molar ratio of propylene oxide to metal ions is adjusted to 10:1; in step 6, the reduction stage is adjusted to 450℃ for 3 h and the crystallization stage is adjusted to 600℃ for 2 h; in step 7, the noble metal is changed from platinum to ruthenium, and ruthenium trichloride aqueous solution is used as the impregnation solution, with a theoretical ruthenium loading mass fraction of 0.3%; in step 8, the catalyst dosage is adjusted to 0.3 g / L, the potassium persulfate complex salt dosage is adjusted to 1.5 mmol / L, and the reaction time is 60 min. Other conditions are the same as in Example 1 and will not be repeated.

[0078] In this embodiment, the wastewater from the workshop of a sulfonamide raw material pharmaceutical manufacturing enterprise was selected. After pretreatment, the sulfamethoxazole mass concentration was 30 mg / L, the chemical oxygen demand was 145 mg / L, the pH was 7.2, and the sulfate mass concentration was 480 mg / L.

[0079] The implementation effect of this embodiment is as follows: the specific surface area of ​​the obtained composite aerogel is 203 m². 2 / g, the average grain size of the alloy nanocrystals is 6.9 nm; after 60 min of reaction, the removal rate of sulfamethoxazole is 97.8%, the removal rate of total organic carbon is 62.5%, and the total mass concentration of metal ions dissolved in the effluent is 0.28 mg / L. After 5 cycles, the removal rate is 91.7%. Compared with Example 1, the lower crystallization temperature results in finer grains and a higher specific surface area, but the intrinsic activity of the active sites is slightly reduced, which needs to be compensated by increasing the dosage of catalyst and oxidant.

[0080] Example 3

[0081] This embodiment is a variation of Example 1. The difference lies in the following steps: In step 1, cerium nitrate hexahydrate is introduced in equal molar amounts to the five principal components of iron, cobalt, nickel, copper, and manganese, forming a six-principal-component system with a configuration entropy of 1.79R, and the total concentration of metal ions is adjusted to 0.6 mol / L; in step 2, the molar ratio of propylene oxide to metal ions is adjusted to 12:1; in step 6, the reduction stage is adjusted to be held at 550 ℃ for 2 h, and the crystallization stage is adjusted to be held at 700 ℃ for 1 h; the noble metal modification in step 7 is omitted; in step 8, the catalyst dosage is 0.4 g / L, the potassium persulfate complex salt dosage is 1.2 mmol / L, and the reaction temperature is 30 ℃. Other conditions are the same as in Example 1 and will not be repeated.

[0082] In this embodiment, alkaline rinsing wastewater from an epoxy resin production enterprise was selected. The bisphenol A concentration was 20 mg / L, the chemical oxygen demand was 96 mg / L, and the pH was 9.2.

[0083] The implementation results of this embodiment show that the oxygen vacancy concentration in the framework increased after the introduction of cerium. After 60 min of reaction, the bisphenol A removal rate was 96.4%, the total organic carbon removal rate was 59.1%, and the total mass concentration of dissolved metal ions in the effluent was 0.36 mg / L. After 5 cycles, the removal rate was 93.1%. This embodiment demonstrates that, without the use of precious metals, excellent alkaline catalytic performance can still be obtained by introducing variable-valence rare earth elements, and the catalyst raw material cost is reduced by approximately 40% compared to Example 1.

[0084] Example 4

[0085] This example is a variation of Example 1, the difference being that: the noble metal modification in step 7 is omitted; in step 8, the oxidant is changed from potassium peroxymonosulfate complex salt to sodium persulfate, with an addition amount of 2.0 mmol / L, the catalyst addition amount is 0.5 g / L, the reaction temperature is 40 ℃, and the reaction time is 60 min. Other conditions are the same as in Example 1 and will not be repeated.

[0086] This embodiment uses rinsing wastewater from the reactive bright red dyeing section of a printing and dyeing enterprise. After coagulation and sedimentation pretreatment, the chemical oxygen demand is 420 mg / L, the color is 400 times, and the pH is 8.6. It needs to be treated to meet the requirements for indirect discharge of the "Water Pollutant Discharge Standard for Textile Dyeing and Finishing Industry" (GB 4287-2012).

[0087] The implementation results of this embodiment are as follows: after 60 minutes of reaction, the color removal rate is 98.9%, the chemical oxygen demand (COD) removal rate is 76.2%, the COD of the effluent is reduced to 100 mg / L, and the color is reduced by 4 times, meeting the requirements for indirect discharge; the total mass concentration of dissolved metal ions in the effluent is 0.47 mg / L. This embodiment demonstrates that by using persulfate and appropriately increasing the reaction temperature, efficient treatment of wastewater with high color and high organic load can also be achieved, and the catalyst cost is significantly reduced by omitting the precious metal modification.

[0088] Example 5

[0089] This embodiment is a variation of Example 1, the difference being that in step 7, the precious metal is replaced by palladium instead of platinum, and a dilute hydrochloric acid solution of palladium chloride is used as the impregnation solution, with a theoretical palladium loading mass fraction of 1.0%; in step 6, the crystallization stage is adjusted to be held at 700 ℃ for 1 h; in step 8, the catalyst dosage is reduced to 0.15 g / L, the potassium persulfate composite salt dosage is reduced to 0.8 mmol / L, the reaction temperature is 30 ℃, and the reaction time is shortened to 40 min. Other conditions are the same as in Example 1 and will not be repeated.

[0090] This embodiment uses the biochemical effluent from a coking plant, with a phenol concentration of 100 mg / L, a chemical oxygen demand of 210 mg / L, a pH of 8.5, and an ammonia nitrogen concentration of 25 mg / L.

[0091] The implementation results of this embodiment are as follows: after 40 min of reaction, the phenol removal rate is 99.1%, the total organic carbon removal rate is 71.4%, and the total mass concentration of dissolved metal ions in the effluent is 0.29 mg / L. After 5 cycles, the phenol removal rate is 94.6%. This embodiment demonstrates that increasing the precious metal loading can achieve the same treatment effect with lower catalyst and oxidant dosages and shorter reaction times, making it suitable for renovation projects with strict requirements on land area and residence time.

[0092] The key indicators of Examples 1 to 5 and Comparative Examples 1 to 5 are compared in the table below.

[0093] serial number Target pollutant <![CDATA[Specific surface area / (m 2 / g)]]> Grain size / nm Removal rate / % Total organic carbon removal rate / % Removal rate after 5 cycles / % Metal leaching (mg / L) Example 1 tetracycline 187 8.6 98.6 68.3 92.4 0.31 Example 2 sulfamethoxazole 203 6.9 97.8 62.5 91.7 0.28 Example 3 Bisphenol A 176 10.2 96.4 59.1 93.1 0.36 Example 4 Active Brilliant Red X-3B 187 8.6 98.9 — 90.8 0.47 Example 5 phenol 169 11.4 99.1 71.4 94.6 0.29 Comparative Example 1 tetracycline 21 14.3 46.2 18.7 — 0.52 Comparative Example 2 tetracycline 94 26.4 71.5 33.6 48.3 2.16 Comparative Example 3 tetracycline 158 13.7 88.1 48.2 51.6 3.42 Comparative Example 4 tetracycline 187 8.6 21.3 3.1 — 0.09 Comparative Example 5 tetracycline 68 19.5 63.8 27.4 — 1.08

[0094] The specific embodiments described above are only used to illustrate the spirit of the present invention. The scope of protection of the present invention is not limited thereto. For those skilled in the art, other embodiments can be easily made by means of changes, substitutions or modifications based on the technical content disclosed in this specification. All such other embodiments should be covered within the scope of protection of the present invention.

Claims

1. A method for preparing a porous high-entropy alloy-oxide composite aerogel catalyst, characterized in that, Includes the following steps: Step 1: Weigh out five transition metal nitrates (ferric nitrate, cobalt nitrate, nickel nitrate, copper nitrate, and manganese nitrate) in equimolar ratio, dissolve them in a mixed solvent of deionized water and anhydrous ethanol in a volume ratio of 1:1, control the total concentration of metal ions to be 0.4~0.6 mol / L, and stir at 300 r / min for 20~30 min at 20~30 ℃ to obtain a homogeneous precursor solution; Step 2: Add propylene oxide to the homogeneous precursor solution in one step. The molar ratio of propylene oxide to metal ions is 8:1 to 12:

1. Stir for 3 to 5 min and let stand at 20 to 30 °C for 2 to 6 h to obtain a monolithic wet gel. Step 3: Age the wet gel at 45~55 ℃ for 20~28 h; Step 4: Use anhydrous ethanol as the replacement solvent, with an amount three times the volume of the wet gel. Replace the ethanol every 12 hours, repeating this process 3 to 5 times until the mass fraction of residual water in the gel is less than 0.5%, thus obtaining an alcohol gel. Step 5: The alcohol gel is replaced with liquid carbon dioxide at a pressure of 8-10 MPa and a temperature of 15-20 °C for 4-8 h, then heated to 40-45 °C and pressurized to 12-15 MPa and held for 1-2 h, and then depressurized to atmospheric pressure at a rate of 0.5 MPa / h to obtain a specific surface area of ​​250-350 m². 2 / g porous high-entropy oxide aerogel; Step 6: The porous high-entropy oxide aerogel is heated to 450~550 ℃ at 3℃ / min and held for 2~3 h in a hydrogen-argon mixture with a hydrogen gas volume fraction of 5%, and then heated to 600~700 ℃ at 2℃ / min and held for 1~2 h. After being cooled in the furnace, it is passivated in an oxygen-argon mixture with an oxygen volume fraction of 0.5% for 2 h to obtain the porous high-entropy alloy-oxide composite aerogel catalyst. Step 7: The porous high-entropy alloy-oxide composite aerogel obtained in Step 6 is immersed in a soluble salt solution containing platinum, palladium or ruthenium to reduce and prepare a noble metal-supported porous high-entropy alloy-oxide composite aerogel.

2. The preparation method according to claim 1, characterized in that, In step 1, the mole fraction of each principal component in the transition metal nitrate is 1 / N, where N is the number of principal components. The configuration entropy of the system is expressed as ΔS. conf =-R·Σx i ·ln x i Calculate at least 1.5R, where R is the molar gas constant and x is the value of x. i Let be the mole fraction of the i-th principal component.

3. The preparation method according to claim 1, characterized in that, In step 6, the hydrogen-argon mixture is continuously introduced at a flow rate of 100 mL / min between the reduction section and the crystallization section.

4. The preparation method according to claim 1, characterized in that, The process also includes step 7, in which the porous high-entropy alloy-oxide composite aerogel obtained in step 6 is impregnated in a soluble salt solution containing platinum, palladium or ruthenium, with the theoretical loading mass fraction of the noble metal controlled at 0.3%~1.0%. The aerogel is first ultrasonically dispersed at 40 kHz and 150 W for 30 min at 20~30 ℃, then allowed to stand for 4~6 h, followed by rotary evaporation at 60 ℃ to dryness, drying at 105 ℃ for 4 h, and finally reduction at 300 ℃ for 1 h in a hydrogen-argon mixture with a hydrogen gas integral of 5%.

5. A porous high-entropy alloy-oxide composite aerogel catalyst, characterized in that, The catalyst is prepared by the method according to any one of claims 1 to 4, wherein face-centered cubic high-entropy alloy nanocrystals are uniformly embedded in a spinel-structured high-entropy oxide framework, the average grain size of the high-entropy alloy nanocrystals is 5-15 nm, and the specific surface area of ​​the catalyst is 150-220 m². 2 / g, with a saturation magnetization of 18~32 emu / g.

6. The application of the porous high-entropy alloy-oxide composite aerogel catalyst according to claim 5 in the treatment of recalcitrant organic wastewater, characterized in that, The catalyst is added at a dosage of 0.1–0.5 g / L to wastewater containing tetracyclines, sulfonamides, phenols, bisphenols, or azo dyes, with an initial target pollutant concentration of 10–200 mg / L. Simultaneously, 0.5–2.0 mmol / L of persulfate or perdisulfate is added. The reaction is carried out at a temperature of 20–40 °C, a pH of 3–10, and a stirring speed of 200–400 r / min for 20–60 min. After the reaction is completed, the catalyst is magnetically separated and recovered within 5–10 min using a 0.3–0.5 T permanent magnet.

Citation Information

Patent Citations

  • High-entropy alloy aerogel catalyst as well as preparation method and application thereof

    CN118422249A

  • High-entropy oxide aerogel composite catalyst as well as preparation method and application thereof

    CN118527180A

  • Preparation method and application of high-entropy alloy aerogel for electro-catalysis

    CN119571369A