A Ni@C / CdS composite photocatalyst, its preparation method and application
By preparing Ni@C/CdS catalysts by combining Ni-MOF with CdS, the problems of high recombination rate of photogenerated carriers and photocorrosion of cadmium sulfide in MOF materials were solved, achieving high efficiency of photocatalytic hydrogen evolution performance and structural stability, which is suitable for industrial production.
Patent Information
- Application Number
- CN202611324644.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing MOF materials suffer from high photogenerated carrier recombination rates, severe cadmium sulfide photocorrosion, and rapid electron-hole recombination, resulting in insufficient photocatalytic hydrogen evolution performance.
Using Ni-MOF as a precursor, Ni@C material was prepared by controlled pyrolysis and then combined with CdS to construct a Ni@C/CdS heterojunction, thereby improving the photogenerated carrier separation efficiency and structural stability.
It significantly improves the separation efficiency of photogenerated carriers, enhances photocatalytic activity and structural stability, and exhibits excellent visible light photocatalytic hydrogen production performance, making it suitable for industrial production.
Smart Images

Figure CN123102383A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of photocatalytic materials technology, specifically to a Ni@C / CdS composite photocatalyst, its preparation method, and its application. Background Technology
[0002] Photocatalytic water splitting for hydrogen production is an effective way to convert solar energy into chemical energy, with significant energy and environmental implications. Metal-organic frameworks (MOFs) have attracted widespread attention in the field of photocatalysis due to their high specific surface area, tunable structure, and porous properties. However, in practical applications, MOFs face technical bottlenecks such as low light energy utilization, high photogenerated carrier recombination rate, and insufficient photocatalytic hydrogen evolution performance. Cadmium sulfide (CdS), as a typical visible-light-responsive semiconductor material, possesses good light absorption performance, but the photogenerated holes generated by this photocatalyst can combine with sulfur ions, resulting in an irreversible auto-oxidation reaction (CdS + h⁻¹). + →Cd 2+ On the one hand, cadmium ions dissolve, causing the loss of active components; on the other hand, elemental sulfur or sulfates are deposited on the catalyst surface, destroying the crystal structure. Therefore, cadmium sulfide suffers from severe photocorrosion. In addition, sulfur vacancy defects formed during the synthesis process lead to a high electron-hole recombination rate. These defects become recombination centers for charge carriers, restricting its application.
[0003] Therefore, developing a novel composite photocatalyst material that can effectively suppress photogenerated carrier recombination while improving structural stability and light energy utilization efficiency has become the key to solving the above-mentioned technical bottlenecks. Summary of the Invention
[0004] To address the problems of high photogenerated carrier recombination rate, severe photocorrosion of cadmium sulfide, and rapid electron-hole pair recombination in MOF materials, the present invention aims to provide a method for preparing Ni@C / CdS composite photocatalysts, specifically including the following steps: (1) Preparation of Ni-MOF: Nickel nitrate hexahydrate, 1,3,5-benzenetricarboxylic acid and polyvinylpyrrolidone were added to a mixed solvent in sequence and mixed evenly to obtain a light green mixture; the mixture was heated to react, and after the reaction was completed, it was cooled, the solid and liquid were separated, washed and dried to obtain Ni-MOF material.
[0005] (2) Preparation of CdS: Thiourea and cadmium nitrate tetrahydrate were dissolved together in water and stirred to obtain a mixed solution; the mixed solution was heated to react, filtered, washed and dried to obtain CdS crystals.
[0006] (3) Preparation of Ni@C: Ni-MOF material and sodium hypophosphite are placed separately in a tube furnace. Ni-MOF material is placed upstream of the tube furnace and sodium hypophosphite is placed downstream of the tube furnace. They are calcined in an inert atmosphere to obtain Ni@C material.
[0007] (4) Preparation of Ni@C / CdS: CdS and Ni@C materials were mixed and ground with organic solvent, and then dried to obtain Ni@C / CdS composite photocatalyst.
[0008] Preferably, in step (1) of the present invention, the mixed solvent is composed of water, N,N-dimethylformamide and ethanol in a volume ratio of 0.5~2:0.5~2:0.5~2; the molar ratio of nickel nitrate hexahydrate, 1,3,5-benzenetricarboxylic acid and polyvinylpyrrolidone is 1~3:0.5~2:0.01~0.1; the concentration of nickel nitrate hexahydrate in the mixture is 0.02~0.1 mol / L; the heating reaction conditions are: reaction at 120~180 ℃ for 8~12 hours.
[0009] Preferably, the molecular weight of polyvinylpyrrolidone in step (1) of the present invention is 40,000.
[0010] Preferably, in step (2) of the present invention, the molar ratio of thiourea and cadmium nitrate tetrahydrate is 1~2.5:0.5~1.5; the concentration of thiourea in the mixed solution is 0.05~0.1 mol / L; and the heating reaction conditions are: reaction at 150~200 ℃ for 10~15 hours.
[0011] Preferably, in step (3) of the present invention, the mass ratio of Ni-MOF material to sodium hypophosphite is 0.5~1.5:5~15; the calcination conditions are calcination at 400~600°C for 1~3 hours.
[0012] Preferably, in step (4) of the present invention, the mass ratio of CdS to Ni@C material is 0.5~1.5:5~15; and the organic solvent is ethanol.
[0013] Another object of the present invention is to provide a Ni@C / CdS composite photocatalyst prepared by the method described in the present invention.
[0014] Another objective of this invention is to provide an application of Ni@C / CdS composite photocatalyst in photocatalytic hydrogen production.
[0015] This invention provides a Ni@C / CdS composite photocatalyst, its preparation method, and its application, which have the following beneficial effects: (1) In this invention, a nickel-based compound Ni@C with a hierarchical porous structure is prepared by controlled pyrolysis using Ni-MOF as a precursor. Its huge surface area and porous structure not only expose a large number of active sites, but also promote the diffusion of reactants and electron transport. A Ni@C / CdS composite photocatalyst with a tight heterojunction is constructed by combining the nickel-based compound Ni@C with cadmium sulfide.
[0016] (2) The Ni@C / CdS composite photocatalyst of the present invention significantly improves the overall conductivity, accelerates the interfacial electron transfer, effectively suppresses the recombination of photogenerated electron-hole pairs, and promotes the efficient migration of photogenerated electrons from CdS to Ni@C through the heterostructure, thereby significantly improving the separation efficiency of photogenerated carriers.
[0017] (3) The Ni@C / CdS composite photocatalyst of the present invention exhibits excellent hydrogen production performance under visible light irradiation, showing extremely high photocatalytic activity, and can maintain good structural stability and catalytic activity in long-term photocatalytic reactions, and shows excellent performance in water splitting to produce hydrogen.
[0018] (4) The present invention uses a hydrothermal method combined with a controllable pyrolysis process. The preparation process is simple, the raw materials are readily available, and the cost is low, making it suitable for industrial production and large-scale application. Attached Figure Description
[0019] Figure 1 This is a schematic diagram illustrating the synthesis of the Ni@C / CdS composite catalyst of this invention.
[0020] Figure 2 This is a schematic diagram of the Ni@C / CdS photocatalytic hydrogen production mechanism of the present invention.
[0021] Figure 3 These are XRD patterns of the materials prepared in Example 1 and Comparative Examples 1-3 of this invention.
[0022] Figure 4 These are XRD comparison images of 40-NC-450 material before and after the reaction of this invention.
[0023] Figure 5 This is a comparison chart of the hydrogen production rates prepared in Examples 1-5 and Comparative Example 4 of the present invention. Detailed Implementation
[0024] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0025] Example 1 A method for preparing a Ni@C / CdS composite photocatalyst, the preparation process is as follows: Figure 1 As shown, the specific steps are as follows: (1) Preparation of Ni-MOF: Water (20 mL), N,N-dimethylformamide (20 mL) and ethanol (20 mL) were added to a beaker and stirred with a stirrer to form a uniform mixed solvent. 3 mmol of nickel nitrate hexahydrate [Ni(NO3)2·6H2O], 1.5 mmol of 1,3,5-benzenetricarboxylic acid and 0.075 mmol of polyvinylpyrrolidone (weight average molecular weight 40,000, i.e., PVP K30) were added to the mixed solvent in sequence. The mixture was stirred continuously to obtain a light green mixture. The mixture was poured into a reaction vessel and placed in an oven at 150 °C for 10 hours. After natural cooling, the mixture was centrifuged at 3000 rpm for 10 minutes and washed three times with anhydrous ethanol. The product was dried at 80 °C for 12 hours to obtain a well-crystallized Ni-MOF material (green powder).
[0026] (2) Preparation of CdS: First, add 4 mmol of thiourea [CH4N2S] and 2 mmol of cadmium nitrate tetrahydrate [Cd(NO3)2·4H2O] to a beaker, then add 40 mL of deionized water, stir at room temperature until completely dissolved to obtain a mixed solution; react the mixed solution at 180℃ for 12 hours, filter, wash and dry to obtain yellow crystal CdS.
[0027] (3) Preparation of Ni@C: 0.03g of Ni-MOF material was evenly spread in an alumina ceramic boat; 0.3g of sodium hypophosphite was weighed and placed in another ceramic boat and ground evenly; then the two ceramic boats were placed in the upstream and downstream sections of the tube furnace respectively (sodium hypophosphite was placed upstream, i.e., the gas inlet side; Ni-MOF was placed downstream, i.e., the gas outlet side), and calcined at a reaction temperature of 450°C for 2 hours in a flowing nitrogen atmosphere to obtain NC-450 material.
[0028] (4) Preparation of Ni@C / CdS (i.e. 40-NCS-450): Yellow crystalline CdS and NC-450 material were placed in an agate mortar (the mass ratio of NC-450 to CdS material was 0.4:1), 4 ml of anhydrous ethanol was added and the mixture was continuously ground until the ethanol was completely evaporated. After grinding, the mixture was transferred to an oven and dried at 60°C for 24 hours to obtain the composite photocatalyst, which was named 40-NCS-450.
[0029] The composite photocatalyst 40-NCS-450 obtained in this embodiment exhibits excellent photocatalytic hydrogen production performance, with a hydrogen evolution rate as high as 40.23 mmol g. -1 h -1 The cumulative hydrogen production reached 201.15 mmol·g. -1 ·h -1 Its performance is 20 times that of pure CdS.
[0030] Example 2 The difference between this embodiment and Example 1 is that the mass ratio of NC-450 to CdS material in step (4) is 0.2:1, while the other steps are the same; the catalyst prepared is named 20-NCS-450.
[0031] The composite photocatalyst obtained in this embodiment has a hydrogen evolution rate as high as 25.52 mmol g. -1 h -1 The cumulative hydrogen production over 5 hours reached 127.60 mmol·g. -1 ·h -1 .
[0032] Example 3 The difference between this embodiment and embodiment 1 is that the mass ratio of NC-450 to CdS in step (4) is 0.3:1, while the other steps are the same; the catalyst prepared is named 30-NCS-450.
[0033] The composite photocatalyst obtained in this embodiment has a hydrogen evolution rate as high as 35.94 mmol g. -1 h -1 The cumulative hydrogen production over 5 hours reached 179.71 mmol·g. -1 ·h -1 .
[0034] Example 4 The difference between this embodiment and embodiment 1 is that the mass ratio of NC-450 to CdS material in step (4) is 0.5:1, while the other steps are the same; the catalyst prepared is named 50-NCS-450.
[0035] The composite photocatalyst obtained in this embodiment has a hydrogen evolution rate as high as 32.21 mmol g. -1 h -1 The cumulative hydrogen production reached 161.09 mmol·g. -1 ·h -1 .
[0036] Example 5 The difference between this embodiment and Example 1 is that the mass ratio of NC-450 to CdS material in step (4) is 0.6:1, while the other steps are the same; the catalyst prepared is named 60-NCS-450.
[0037] The composite photocatalyst obtained in this embodiment has a hydrogen evolution rate as high as 26.14 mmol g. -1 h -1 The cumulative hydrogen production reached 130.70 mmol·g -1 ·h -1 .
[0038] Example 6 (1) Preparation of Ni-MOF: Water (10 mL), N,N-dimethylformamide (40 mL) and ethanol (10 mL) were added to a beaker and stirred with a stirrer to form a uniform mixed solvent. 2.4 mmol of nickel nitrate hexahydrate [Ni(NO3)2·6H2O], 1.2 mmol of 1,3,5-benzenetricarboxylic acid and 0.12 mmol of polyvinylpyrrolidone (weight average molecular weight 40,000, i.e., PVP K30) were added to the mixed solvent in sequence. The mixture was stirred continuously to obtain a light green mixture. The mixture was poured into a reaction vessel and placed in an oven at 120 °C for 8 hours. After natural cooling, the mixture was centrifuged at 3000 rpm for 10 minutes and washed three times with anhydrous ethanol. The product was dried at 80 °C for 12 hours to obtain a well-crystallized Ni-MOF material (green powder).
[0039] (2) Preparation of CdS: First, 2 mmol of thiourea [CH4N2S] and 3 mmol of cadmium nitrate tetrahydrate [Cd(NO3)2·4H2O] were added to a beaker, and then 40 mL of deionized water was added. The mixture was stirred at room temperature until completely dissolved to obtain a mixed solution. The mixed solution was reacted at 150 °C for 15 hours, filtered, washed and dried to obtain yellow crystals of CdS.
[0040] (3) Preparation of Ni@C: 0.05g of Ni-MOF material was evenly spread in an alumina ceramic boat; 1.5g of sodium hypophosphite was weighed and placed in another ceramic boat and ground evenly; then the two ceramic boats were placed in the upstream and downstream sections of the tube furnace respectively (sodium hypophosphite was placed upstream, i.e., the gas inlet side; Ni-MOF was placed downstream, i.e., the gas outlet side), and calcined at a reaction temperature of 400°C for 3 hours in a flowing nitrogen atmosphere to obtain NC-400 material.
[0041] (4) Preparation of Ni@C / CdS (i.e. 20-NCS-400): Yellow crystalline CdS and NC-450 material were placed in an agate mortar (the mass ratio of NC-450 to CdS material was 0.2:1), 4 ml of anhydrous ethanol was added and the mixture was continuously ground until the ethanol was completely evaporated. After grinding, the mixture was transferred to an oven and dried at 60°C for 24 hours to obtain the composite photocatalyst, which was named 20-NCS-400.
[0042] The composite photocatalyst obtained in this embodiment has a hydrogen evolution rate as high as 25.61 mmol g. -1 h -1 The cumulative hydrogen production reached 128.05 mmol·g. -1 ·h -1 .
[0043] Example 7 (1) Preparation of Ni-MOF: Water (6 mL), N,N-dimethylformamide (24 mL) and ethanol (24 mL) were added to a beaker and stirred with a stirrer to form a homogeneous mixed solvent. 8.1 mmol of nickel nitrate hexahydrate [Ni(NO3)2·6H2O], 5.4 mmol of 1,3,5-benzenetricarboxylic acid and 0.27 mmol of polyvinylpyrrolidone (weight average molecular weight 40,000, i.e., PVP K30) were added to the mixed solvent in sequence. The mixture was stirred continuously to obtain a light green mixture. The mixture was poured into a reaction vessel and placed in an oven at 180 °C for 12 hours. After natural cooling, the mixture was centrifuged at 3000 rpm for 10 minutes and washed three times with anhydrous ethanol. The product was dried at 80 °C for 12 hours to obtain a well-crystallized Ni-MOF material (green powder).
[0044] (2) Preparation of CdS: First, 2 mmol of thiourea [CH4N2S] and 0.4 mmol of cadmium nitrate tetrahydrate [Cd(NO3)2·4H2O] were added to a beaker, and then 40 mL of deionized water was added. The mixture was stirred at room temperature until completely dissolved to obtain a mixed solution. The mixed solution was reacted at 200℃ for 10 hours, filtered, washed and dried to obtain yellow crystals of CdS.
[0045] (3) Preparation of Ni@C: 0.15g of Ni-MOF material was evenly spread in an alumina ceramic boat; 0.75g of sodium hypophosphite was weighed and placed in another ceramic boat and ground evenly; then the two ceramic boats were placed in the upstream and downstream sections of the tube furnace respectively (sodium hypophosphite was placed upstream, i.e., the gas inlet side; Ni-MOF was placed downstream, i.e., the gas outlet side), and calcined at a reaction temperature of 600°C for 1 hour in a flowing nitrogen atmosphere to obtain NC-600 material.
[0046] (4) Preparation of Ni@C / CdS (i.e. 40-NCS-450): Yellow crystalline CdS and NC-450 material were placed in an agate mortar (the mass ratio of NC-450 to CdS material was 0.6:1), 4 ml of anhydrous ethanol was added and the mixture was continuously ground until the ethanol was completely evaporated. After grinding, the mixture was transferred to an oven and dried at 60°C for 24 hours to obtain a composite photocatalyst, named 60-NCS-600.
[0047] The composite photocatalyst obtained in this embodiment has a hydrogen evolution rate as high as 26.11 mmol g. -1 h -1 The cumulative hydrogen production reached 130.60 mmol·g -1 ·h -1 .
[0048] Comparative Example 1 The specific steps for preparing Ni-MOF are as follows: Water (20 mL), N,N-dimethylformamide (20 mL), and ethanol (20 mL) were added to a beaker, and the beaker was stirred with a stirrer to form a homogeneous mixed solvent. 3 mmol of nickel nitrate hexahydrate [Ni(NO3)2·6H2O], 1.5 mmol of 1,3,5-benzenetricarboxylic acid, and 0.075 mmol of polyvinylpyrrolidone (weight average molecular weight 40,000, i.e., PVPK30) were added sequentially to the mixed solvent. The mixture was stirred continuously to obtain a light green mixture. The mixture was poured into a reaction vessel and placed in an oven at 150 °C for 10 hours. After natural cooling, the mixture was centrifuged at 3000 rpm for 10 minutes and washed three times with anhydrous ethanol. The product was dried at 80 °C for 12 hours to obtain a well-crystallized Ni-MOF material (green powder).
[0049] The hydrogen evolution rate of the Ni-MOF material obtained in this comparative example is as high as 0.23 mmol g. -1 h -1 The cumulative hydrogen production reached 1.15 mmol·g. -1 ·h -1 .
[0050] Comparative Example 2 The specific steps for preparing pure CdS material are as follows: Add 4 mmol of thiourea [CH4N2S] and 2 mmol of cadmium nitrate tetrahydrate [Cd(NO3)2·4H2O] to a beaker, then add 40 mL of deionized water and stir at room temperature until completely dissolved to obtain a mixed solution. React the mixed solution at 180 °C for 12 hours, filter, wash and dry to obtain yellow crystalline CdS.
[0051] The hydrogen evolution rate of the CdS material obtained in this comparative example is as high as 1.99 mmol g. -1 h -1 The cumulative hydrogen production reached 9.95 mmol·g -1 ·h -1 .
[0052] Comparative Example 3 The specific steps for preparing NC-450 material are as follows: (1) Add water (20 mL), N,N-dimethylformamide (20 mL) and ethanol (20 mL) to a beaker and stir the beaker with a stirrer to form a uniform mixed solvent; add 3 mmol nickel nitrate hexahydrate [Ni(NO3)2·6H2O] 1.5 mmol, 1,3,5-benzenetricarboxylic acid and 0.075 mmol polyvinylpyrrolidone (weight average molecular weight 40000, i.e. PVP K30) to the above mixed solvent in sequence; continue stirring to obtain a light green mixture; pour the mixture into a reaction vessel, place it in an oven at 150℃ and react for 10 hours, cool naturally, centrifuge at 3000 rpm for 10 minutes, and wash 3 times with anhydrous ethanol. Dry the product at 80℃ for 12 hours to obtain a well-crystallized Ni-MOF material (green powder).
[0053] (2) Spread 0.03g of Ni-MOF material evenly in an alumina ceramic boat; weigh 0.3g of sodium hypophosphite and grind it evenly in another ceramic boat; then place the two ceramic boats in the upstream and downstream sections of the tube furnace respectively (sodium hypophosphite is placed upstream, i.e., on the side of the gas inlet; Ni-MOF is placed downstream, i.e., on the side of the gas outlet), and calcine at a reaction temperature of 450°C for 2 hours in a flowing nitrogen atmosphere to obtain NC-450 material.
[0054] The hydrogen evolution rate of the NC-450 material obtained in this comparative example is basically zero, and the cumulative hydrogen production is basically zero.
[0055] Comparative Example 4 (1) Preparation of Ni-MOF: Water (20 mL), N,N-dimethylformamide (20 mL) and ethanol (20 mL) were added to a beaker and stirred with a stirrer to form a uniform mixed solvent. 3 mmol of nickel nitrate hexahydrate [Ni(NO3)2·6H2O], 1.5 mmol of 1,3,5-benzenetricarboxylic acid and 0.075 mmol of polyvinylpyrrolidone (weight average molecular weight 40,000, i.e., PVP K30) were added to the mixed solvent in sequence. The mixture was stirred continuously to obtain a light green mixture. The mixture was poured into a reaction vessel and placed in an oven at 150 °C for 10 hours. After natural cooling, the mixture was centrifuged at 3000 rpm for 10 minutes and washed three times with anhydrous ethanol. The product was dried at 80 °C for 12 hours to obtain a well-crystallized Ni-MOF material (green powder).
[0056] (2) Preparation of CdS: First, add 4 mmol of thiourea [CH4N2S] and 2 mmol of cadmium nitrate tetrahydrate [Cd(NO3)2·4H2O] to a beaker, then add 40 mL of deionized water, stir at room temperature until completely dissolved to obtain a mixed solution; react the mixed solution at 180℃ for 12 hours, filter, wash and dry to obtain yellow crystal CdS.
[0057] (3) Preparation of Ni@C: 0.03g of Ni-MOF material was evenly spread in an alumina ceramic boat; 0.3g of sodium hypophosphite was weighed and placed in another ceramic boat and ground evenly; then the two ceramic boats were placed in the upstream and downstream sections of the tube furnace respectively (sodium hypophosphite was placed upstream, i.e., the gas inlet side; Ni-MOF was placed downstream, i.e., the gas outlet side), and calcined at a reaction temperature of 450°C for 2 hours in a flowing nitrogen atmosphere to obtain NC-450 material.
[0058] (4) Preparation of Ni@C / CdS (i.e. 10-NCS-450): Yellow crystalline CdS and NC-450 material were placed in an agate mortar (the mass ratio of CdS to NC-450 material was 0.11:1), 4 ml of anhydrous ethanol was added and the mixture was continuously ground until the ethanol was completely evaporated. After grinding, the mixture was transferred to an oven and dried at 60°C for 24 hours to obtain the composite photocatalyst, which was named 10-NCS-450.
[0059] The 10-NCS-450 catalyst obtained in this comparative example exhibited an 8.62 mmol·g⁻¹ Mg²⁺ stoichiometry. -1 ·h -1 The catalytic hydrogen evolution rate reached 43.08 mmol·g. -1 .
[0060] The photocatalyst materials (5 mg) prepared in Examples 1-7 and Comparative Examples 1-3 were added to a quartz reactor along with 50 mL of a mixed aqueous solution (the concentration of Na2S·9H2O in the mixed solution was 0.25 mol / L and the concentration of Na2SO3 was 0.35 mol / L). The solution was ultrasonically treated for 30 minutes to ensure thorough mixing. Then, vacuum grease was applied to the interface of the quartz reactor before connecting it to the photocatalytic reaction system. Before the reaction started, the vacuum pump was started to evacuate the system to ensure the accuracy of the test results. After evacuation was completed, the vacuum pump was turned off and the light source was turned on, maintaining a current intensity of 15 A. The distance between the xenon lamp light source and the reactor was kept constant at 5 cm, and the temperature was controlled at 6°C. The hydrogen production was detected by an online gas chromatography system (GC-5890 N, with Ar as the carrier gas). The system automatically injected samples every 30 minutes for 5 hours of quantitative analysis. The hydrogen production rate and cumulative amount were calculated based on the peak area and the standard curve.
[0061] The hydrogen production rates prepared in Examples 1-5 and Comparative Example 4 of this invention are as follows: Figure 5 As shown.
[0062] The XRD patterns of 40-NCS-450 prepared in Example 1, Ni-MOF prepared in Comparative Example 2, CdS prepared in Comparative Example 3, and NC-450 prepared in Comparative Example 4 are as follows: Figure 3As shown, Ni-MOF exhibits four characteristic peaks at 9.2°, 11.7°, 15.5°, and 18.5°, corresponding to the (100), (010), (101), and (200) crystal planes, respectively; CdS has a hexagonal structure, with characteristic peaks located at 24.9°, 26.4°, 28.2°, 43.7°, 47.8°, and 51.9°, consistent with the JCPDs#41-1049 standard card. This indicates that both Ni-MOF and CdS were successfully prepared. In the XRD pattern of NC-450, the (111), (200), and (220) crystal planes of nickel were observed, with characteristic peaks appearing at 44.8°, 52.2°, and 76.8°, respectively, consistent with the standard card JCPDs#04-0850. In addition, the broad peaks appearing in the 20°-30° range originated from partially graphitized carbon materials, indicating the presence of incompletely crystalline carbon species in the NC-450 sample, with a structure intermediate between amorphous carbon and complete graphite crystals. Compared with NC-45 and CdS, the characteristic peak intensity of 40-NC-450 was weakened, but the positions of its characteristic peaks simultaneously included the characteristic peaks of NC-45 and CdS, indicating that the 40-NC-450 composite material was successfully prepared.
[0063] The XRD patterns of the 40-NC-450 material before and after the reaction are as follows: Figure 4 As shown, the characteristic diffraction peaks of 40-NCS-450 do not exhibit obvious migration, indicating that the overall crystal structure of the material has good stability during the catalytic reaction.
[0064] The bandgap widths of CdS and 40-NCS-450 were analyzed using equation (1): αhν =A(hν-E g ) (n / 2) (1) In equation (1): α represents the absorption coefficient, h represents Planck's constant, v represents the frequency of the incident light, Eg corresponds to the bandgap width, A represents the proportionality constant of the material, and the exponent n is related to the semiconductor characteristics: n is 1 / 2 for direct bandgap semiconductors and 2 for indirect bandgap semiconductors. Since both CdS and 40-NCS-450 samples are direct bandgap semiconductors, 1 / n is taken as 2. The measurement results are as follows: the bandgap width of CdS is 2.31 eV; the bandgap width of 40-NCS-450 is 2.26 eV; the bandgap width of NCS-450 is narrower than that of the original CdS, which indicates that the composite material is more conducive to the absorption of visible light. Therefore, the visible light utilization rate of 40-NCS-450 is higher than that of CdS.
[0065] The rational photocatalytic hydrogen evolution reaction mechanism of the Ni@C / CdS ternary composite system of this invention is as follows: Figure 2As shown, under visible light irradiation, electrons in the CdS valence band (VB) gain photon energy and transition to the conduction band (CB), leaving positively charged holes in the valence band. The unique structure of the Ni@C cocatalyst plays a crucial role in the entire photocatalytic reaction: on the one hand, the presence of the highly conductive carbon layer allows for rapid transport of photogenerated electrons; on the other hand, thanks to the close contact between CdS and Ni@C, nickel nanoparticles loaded on the carbon layer surface can capture electrons. Furthermore, when some nickel nanoparticles directly contact the CdS surface, electrons in the CdS semiconductor conduction band can be directly captured by the nickel nanoparticles, thus completing the photocatalytic water splitting to produce hydrogen. Simultaneously, photogenerated holes in the CdS valence band are captured and oxidized by Na2SO3 and Na2S·9H2O.
[0066] This invention prepares CdS and Ni-MOF materials via a hydrothermal method, and successfully prepares a high-performance Ni@C / CdS composite material by using Ni-MOF as a precursor and controlling the calcination temperature. The high catalytic activity of the composite material prepared by this invention stems from the following mechanisms: the presence of carbon materials enhances conductivity and accelerates electron transport; simultaneously, the heterojunction constructed between Ni / C and CdS effectively promotes the separation of photogenerated electron-hole pairs.
[0067] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a Ni@C / CdS composite photocatalyst, characterized in that, Specifically, the following steps are included: (1) Preparation of Ni-MOF: Nickel nitrate hexahydrate, 1,3,5-benzenetricarboxylic acid and polyvinylpyrrolidone were added to a mixed solvent in sequence and mixed evenly to obtain a mixture; the mixture was heated to react, and after the reaction was completed, it was cooled, the solid and liquid were separated, washed and dried to obtain Ni-MOF material; (2) Preparation of CdS: Thiourea and cadmium nitrate tetrahydrate were dissolved together in water and stirred to obtain a mixed solution; the mixed solution was heated to react, filtered, washed and dried to obtain CdS crystals; (3) Preparation of Ni@C: Ni-MOF material and sodium hypophosphite are placed separately in a tube furnace. Ni-MOF material is placed upstream of the tube furnace and sodium hypophosphite is placed downstream of the tube furnace. They are calcined in an inert atmosphere to obtain Ni@C material. (4) Preparation of Ni@C / CdS: CdS and Ni@C materials were mixed and ground with organic solvent, and then dried to obtain Ni@C / CdS composite photocatalyst.
2. The preparation method of the Ni@C / CdS composite photocatalyst according to claim 1, characterized in that, The mixed solvent in step (1) is composed of water, N,N-dimethylformamide and ethanol in a volume ratio of 0.5~2:0.5~2:0.5~2; the molar ratio of nickel nitrate hexahydrate, 1,3,5-benzenetricarboxylic acid and polyvinylpyrrolidone is 1~3:0.5~2:0.01~0.1; the concentration of nickel nitrate hexahydrate in the mixture is 0.02~0.1 mol / L; the heating reaction conditions are: reaction at 120~180℃ for 8~12 hours.
3. The preparation method of the Ni@C / CdS composite photocatalyst according to claim 1, characterized in that, The molar ratio of thiourea and cadmium nitrate tetrahydrate in step (2) is 1~2.5:0.5~1.5; the concentration of thiourea in the mixed solution is 0.05~0.1mol / L; the heating reaction conditions are: reaction at 150~200℃ for 10~15 hours.
4. The preparation method of the Ni@C / CdS composite photocatalyst according to claim 1, characterized in that, The mass ratio of Ni-MOF material to sodium hypophosphite in step (3) is 0.5~1.5:5~15; the calcination conditions are calcination at 400~600°C for 1~3 hours.
5. The preparation method of the Ni@C / CdS composite photocatalyst according to claim 1, characterized in that, The mass ratio of CdS to Ni@C material in step (4) is 0.25~1.5:
1.
6. The Ni@C / CdS composite photocatalyst prepared by the method according to any one of claims 1 to 5.
7. The application of the Ni@C / CdS composite photocatalyst according to claim 6 in photocatalytic hydrogen production.