A bimetallic supported MXene-based ammonia oxidation catalyst, its preparation method and application
By using a Pt-Cu bimetallic supported Ti3C2MXene-based catalyst, the problems of insufficient low-temperature activity and poor N2 selectivity of existing catalysts have been solved, achieving high efficiency and high N2 selectivity in low-temperature ammonia catalytic oxidation, which is suitable for high-volume, low-concentration operating conditions.
Patent Information
- Application Number
- CN202611627181.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-21
- Publication Date
- 2026-11-17
AI Technical Summary
Existing ammonia catalytic oxidation catalysts have insufficient activity at low temperatures and poor N2 selectivity. Traditional supports have limited redox performance, Ti3C2MXene has poor thermal stability, and single-metal active components have failed to fully utilize their electronic regulation advantages.
A Pt-Cu bimetallic supported Ti3C2MXene-based catalyst is used. The -O and -OH groups on the surface of the Ti3C2MXene support form chemical bonds with Pt-Cu, achieving uniform dispersion and firm anchoring of the active components. By utilizing the electron migration characteristics and large specific surface area of Ti3C2MXene, the Pt-Cu bimetallic active components are synergistically lowered to reduce the reaction energy barrier, thereby improving the low-temperature activity and N2 selectivity of the catalyst.
The catalyst achieves efficient catalytic oxidation of ammonia at low temperatures, maintains high N2 selectivity, and exhibits minimal activity decay under high space velocity conditions, making it suitable for high-volume, low-concentration applications and reducing operating costs.
Smart Images

Figure CN123102394A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of catalyst technology, specifically relating to a bimetallic supported MXene-based ammonia catalytic oxidation catalyst, its preparation method, and its application. Background Technology
[0002] Ammonia (NH3) is a typical malodorous gaseous pollutant originating from coking, chemical, livestock farming, and flue gas denitrification processes where ammonia escapes. It can irritate and damage the human respiratory tract and can also combine with SO2 and NO in the atmosphere. x The reaction generates secondary aerosols, exacerbating PM2.5 pollution. Selective catalytic oxidation of ammonia (NH3-SCO) is the mainstream technology for purifying low-concentration ammonia, and its key lies in developing catalysts with high activity, high selectivity, and high stability.
[0003] Existing ammonia catalytic oxidation (NH3-SCO) catalysts are divided into two categories: noble metal catalysts (Pt, Pd, Ru, etc.) and non-noble metal oxide catalysts (Cu, Mn, Ce, Co, etc.). Noble metal catalysts exhibit excellent low-temperature activity but are costly, prone to sintering at high temperatures, and have poor N2 selectivity in single-noble metal systems. Non-noble metal catalysts are low-cost and have good N2 selectivity, but their low-temperature activity is insufficient, typically requiring temperatures above 300℃ for conversion, making them unsuitable for low-temperature flue gas conditions.
[0004] The support directly affects the dispersion of active components, metal-support electronic interactions, and catalyst stability. Traditional supports such as TiO2, Al2O3, and molecular sieves have limited redox properties, restricting the improvement of catalyst performance at low temperatures. Ti3C2MXene, with its two-dimensional layered structure, large specific surface area, and easy surface modification, can theoretically serve as a support for metal active components. However, Ti3C2MXene is often prepared using the traditional HF etching method, resulting in a relatively small specific surface area, limiting the effective loading of metal active components. Furthermore, existing technologies mostly employ single-metal active components, failing to fully utilize the electronic regulation advantages of MXene and failing to construct a bimetallic synergistic system. In addition, Ti3C2MXene exhibits poor thermal stability under oxidizing atmospheres, easily leading to the destruction of its two-dimensional structure. Summary of the Invention
[0005] The purpose of this invention is to provide a bimetallic supported MXene-based ammonia catalytic oxidation catalyst, its preparation method, and its application, thereby overcoming the shortcomings of the prior art. By utilizing the abundant defect sites, strong electron migration, and oxygen overflow characteristics of Ti3C2MXene, the catalyst promotes the migration of electrons and oxygen species, and synergistically lowers the energy barrier of ammonia activation reaction with the Pt-Cu bimetallic active component, thereby achieving the catalytic oxidation of ammonia at low temperatures while maintaining high N2 selectivity.
[0006] To achieve the above objectives, the technical solution of the present invention is as follows: In a first aspect, the present invention provides a Pt-Cu bimetallic supported MXene-based ammonia catalytic oxidation catalyst, comprising a Ti3C2MXene support and a Pt-Cu bimetallic active component supported on the surface and interior of the Ti3C2MXene support; the surface of the Ti3C2MXene support has -O and -OH groups, and the Ti3C2MXene support forms chemical bonds with the Pt-Cu bimetallic active component through the -O and -OH groups.
[0007] This invention utilizes the chemical bonds formed between oxygen-containing functional groups on the support surface and the Pt-Cu bimetallic active component, achieving a firm anchorage of the Pt-Cu active component on the support surface and within the interlayer, effectively inhibiting the migration and aggregation of active metal particles. The synergistic effect of Pt and Cu optimizes electron transfer behavior, modulates the catalyst's redox performance, and overcomes the drawbacks of single noble metal catalysts, such as poor nitrogen selectivity and susceptibility to high-temperature sintering. Simultaneously, the large specific surface area and excellent conductivity of Ti3C2MXene further accelerate electron transport during the reaction process, lower the reaction energy barrier, and enhance the low-temperature activity and N2 selectivity of ammonia catalytic oxidation.
[0008] Secondly, the present invention provides a method for preparing a Pt-Cu bimetallic supported MXene-based ammonia catalytic oxidation catalyst, comprising the following steps: mixing alkali-treated Ti3C2MXene, copper metal precursor, pore-forming agent and water, stirring and dispersing, and then grinding to obtain a mixed slurry A; Add the platinum metal precursor and dispersant to water and stir until fully mixed to obtain solution B; Solution B was added to the mixed slurry A and stirred until homogeneous. The mixture was then dried and calcined to obtain the Pt-Cu bimetallic supported MXene-based ammonia catalytic oxidation catalyst.
[0009] This invention first obtains a Ti3C2MXene support rich in hydroxyl groups through an alkaline etching process. The oxygen-containing groups provide anchoring sites for the bimetallic precursor. The Cu and Pt precursors are uniformly dispersed on the surface and between layers of the MXene support by stepwise liquid preparation and slurry grinding and mixing. Subsequently, the Pt-Cu bimetallic active component is constructed by drying and calcination. This preparation process is simple and controllable, effectively avoids the agglomeration of active metal particles, fully utilizes the synergistic effect of Pt-Cu bimetal, and ensures that the obtained catalyst has both high activity and high N2 selectivity in the low-temperature ammonia catalytic oxidation reaction. The process has a low operating threshold and is easy to prepare on a large scale.
[0010] Thirdly, this invention provides the application of Pt-Cu bimetallic supported MXene-based ammonia catalytic oxidation catalyst in ammonia catalytic oxidation at 140℃~300℃.
[0011] The Pt-Cu bimetallic supported MXene-based ammonia catalytic oxidation catalyst of the present invention can simultaneously achieve high ammonia conversion rate and N2 selectivity under low-temperature flue gas conditions, and has good anti-sintering ability and operating condition applicability.
[0012] The beneficial effects of this invention are: (1) The bimetallic active component in the catalyst of the present invention is loaded on the inside and outside surface of the two-dimensional sheet of Ti3C2MXene support. Ammonia molecules can directly contact the active site without long diffusion through micropores and mesopores. Under the high space velocity conditions of catalytic combustion, the apparent activity of the catalyst decreases by a small margin and the activity retention rate is significantly higher than that of traditional porous supports. It is more suitable for large air volume and low concentration conditions, thereby reducing the total amount of catalyst used and lowering the cost of use.
[0013] (2) The Ti3C2MXene surface used in this invention naturally generates a large number of hydrophilic -O, -OH and other functional group end groups during the etching process. The end group density is high and the distribution is uniform, and the surface is negatively charged as a whole. Pt can be uniformly anchored through coordination and electrostatic adsorption. 4+ Cu 2+ Using metal cation precursors, atomic-level uniform co-loading of bimetallic components can be achieved without additional surface modification, avoiding bimetallic phase separation. Simultaneously, strong metal-support electronic interactions can form between the support and the active metal, precisely controlling the electronic structure of the active metal and optimizing the adsorption strength of reaction intermediates. This promotes bond breaking and activation of reactant molecules while avoiding poisoning of active sites due to excessive adsorption of intermediates, effectively reducing the apparent activation energy of the catalytic reaction and significantly improving low-temperature catalytic activity.
[0014] (3) By utilizing the abundant defect sites, strong electron migration and oxygen overflow characteristics of Ti3C2MXene, the electron and oxygen species migration of the catalyst are promoted, and the Pt-Cu bimetallic active components are used in conjunction to reduce the energy barrier of ammonia activation reaction, so as to realize the catalytic oxidation of ammonia at low temperature while maintaining high N2 selectivity. Attached Figure Description
[0015] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an improper limitation of the invention.
[0016] Figure 1 This is a comparison chart of the NH3 conversion rates of the catalysts in Examples 1-3 and Comparative Examples 1-5 of the present invention; Figure 2 This is a comparison chart of the N2 selectivity of the catalysts in Examples 1-3 and Comparative Examples 1-5 of the present invention. Detailed Implementation
[0017] Those skilled in the art will understand that the following embodiments are for illustrative purposes only and should not be construed as limiting the scope of the invention. Specific conditions not specified in the embodiments are performed under conventional conditions or conditions recommended by the manufacturer. Components whose manufacturers are not specified are all commercially available conventional products.
[0018] In a first aspect, the present invention provides a Pt-Cu bimetallic supported MXene-based ammonia catalytic oxidation catalyst, comprising a Ti3C2MXene support and a Pt-Cu bimetallic active component supported on the surface and interior of the Ti3C2MXene support; the surface of the Ti3C2MXene support has -O and -OH groups, and the Ti3C2MXene support forms chemical bonds with the Pt-Cu bimetallic active component through the -O and -OH groups.
[0019] In some other embodiments, the mass ratio of Pt to Cu in the Pt-Cu bimetallic active component is 1:(1~50.5); exemplaryly, the mass ratio of Pt to Cu in the Pt-Cu bimetallic active component is any one or a range of values from 1:1, 1:10, 1:15, 1:20, 1:25, 1:30, 1:35, 1:40, 1:45, or 1:50.5.
[0020] In some other embodiments, the loading of the Pt-Cu bimetallic active component is 0.5 wt% to 14 wt%; For example, the loading of the Pt-Cu bimetallic active component is any one or a range of 0.5 wt%, 1 wt%, 2 wt%, 4 wt%, 8 wt%, 10 wt%, 12 wt%, or 14 wt%.
[0021] Secondly, the present invention provides a method for preparing a Pt-Cu bimetallic supported MXene-based ammonia catalytic oxidation catalyst, comprising the following steps: mixing alkali-treated Ti3C2MXene, copper metal precursor, pore-forming agent and water, stirring and dispersing, and then grinding to obtain a mixed slurry A; Add the platinum metal precursor and dispersant to water and stir until fully mixed to obtain solution B; Solution B was added to the mixed slurry A and stirred until homogeneous. The mixture was then dried and calcined to obtain the Pt-Cu bimetallic supported MXene-based ammonia catalytic oxidation catalyst.
[0022] In some other embodiments, alkali-treated Ti3C2MXene is prepared by the following method: Ti3AlC2 powder is added to concentrated alkali solution in batches and stirred to obtain a suspension; the suspension is subjected to hydrothermal reaction; after cooling to room temperature, water is added to the reaction system to terminate the reaction, and then the mixture is centrifuged, washed, freeze-dried and pulverized to obtain alkali-treated Ti3C2MXene.
[0023] Alkali treatment of Ti3C2MXene can etch away the Al layer to obtain two-dimensional Ti3C2MXene. At the same time, -O and -OH functional groups are enriched on the surface of Ti3C2MXene sheets, providing anchoring sites for Pt-Cu bimetallic precursors, strengthening metal-support interactions, and achieving uniform loading of active components.
[0024] In some other embodiments, the hydrothermal reaction is carried out at a temperature of 260°C to 280°C for 10 to 20 hours. The hydrothermal reaction can further remove residual aluminum impurities, regulate the -O and -OH content on the MXene surface, weaken the layer stacking effect, maintain the two-dimensional open structure, and increase the number of active anchoring points.
[0025] In some other embodiments, the mass ratio of alkali-treated Ti3C2MXene, copper metal precursor, and pore-forming agent is 10:(0.1~7):0.5; exemplaryly, the mass ratio of alkali-treated Ti3C2MXene, copper metal precursor, and pore-forming agent is any point value or range value among 10:0.143:0.5, 10:0.243:0.5, or 10:7:0.5.
[0026] The grinding speed is 300 r / min to 1500 r / min, and the grinding time is 2 min to 10 min. The grinding process can break up the Ti3C2MXene layer stacking, promote the uniform dispersion of copper precursor and pore-forming agent on the Ti3C2MXene surface and between layers, strengthen the interfacial contact of each component, and inhibit the agglomeration of metal particles in the subsequent calcination stage.
[0027] In some other embodiments, the drying temperature is 60°C to 120°C, and the time is 2 hours to 24 hours; The calcination temperature is 300℃~500℃, and the time is 1h~5h. The calcination treatment causes the Pt and Cu precursors to decompose thermally to form Pt-Cu bimetallic active components, which promotes the formation of chemical bonds between the bimetals and between the bimetals and the hydroxyl groups of the Ti3C2MXene support, constructing stable bimetallic synergistic active sites and regulating the pore structure of the material.
[0028] In some other embodiments, the copper metal precursor is at least one of copper nitrate hexahydrate or copper chloride; the platinum metal precursor is at least one of platinum nitrate or platinum chloride; the pore-forming agent is soluble starch; and the dispersant is polyethylene glycol.
[0029] Thirdly, this invention provides the application of Pt-Cu bimetallic supported MXene-based ammonia catalytic oxidation catalyst in ammonia catalytic oxidation at 140℃~300℃.
[0030] The following description, in conjunction with Examples 1-3 and Comparative Examples 1-5, further illustrates the following: Example 1 A method for preparing a Pt-Cu bimetallic supported MXene-based ammonia oxidation catalyst includes the following steps: S1. 13.0 g of Ti3AlC2 (400 mesh, purity >99%) powder was slowly added in 8 batches to a concentrated alkaline solution (27.5 mol / L NaOH aqueous solution at 270℃), and magnetically stirred for 60 min to prepare a uniform black suspension. The suspension was transferred to a 500 mL polytetrafluoroethylene hydrothermal liner, sealed in a stainless steel reactor, and the lid was tightened. The reactor was placed in a high-temperature oven and heated to 270℃ at a rate of 2℃ / min, and etched at that temperature for 12 h. After naturally cooling to room temperature, the reaction solution was slowly diluted in 1 L of deionized water (1:5 volume ratio) to terminate the reaction. The reaction solution was then loaded into centrifuges in batches and centrifuged at 3500 rpm for 5 min to remove the supernatant. The process of adding deionized water, shaking, centrifuging, and washing was repeated. The pH of the supernatant was measured after each centrifugation until the pH of the supernatant stabilized at 7.0. Each batch was washed 8 times. The centrifuged sample was freeze-dried and pulverized to obtain the alkali-treated Ti3C2MXene support (this treatment method can be found in: Fluorine-Free Synthesis of High-Purity Ti3C2T). x (T=OH, O) via Alkali Treatment, Li et al, Angew. Chem. Int. Ed. 2018) and store away from light for later use.
[0031] S2. Weigh 2.43g of copper nitrate hexahydrate and place it in 20g of deionized water and stir until fully dissolved to prepare a copper nitrate solution. Place 10g of alkali-treated Ti3C2MXene powder and 0.5g of soluble starch (pore-forming agent) into the copper nitrate solution and stir to mix. Then grind the mixture in a micro planetary mill at 300 rpm for 10 minutes at a grinding temperature of 25℃ to obtain mixed slurry A.
[0032] S3. Take 1g of polyethylene glycol and add it to 6g of deionized water and stir to mix well. Add 0.3g of platinum nitrate solution (Pt content 10%, the platinum nitrate solution used below is purchased from Anhui Tuosi Precious Metals Co., Ltd.) dropwise and stir to mix to obtain solution B.
[0033] S4. While stirring, slowly add solution B dropwise to the mixed slurry A, and continue stirring for 2 hours to prepare a mixed solution. Place the mixed solution in a constant temperature drying oven and dry it at 60℃ for 2 hours, then at 80℃ for 2 hours, and then at 100℃ until it is completely dry to obtain a dried sample.
[0034] S5. After crushing, grinding and sieving the dried sample, place it in an alumina crucible for calcination. The temperature is increased to 350°C at a rate of 2°C per minute and held for calcination for 2 hours to obtain the Pt-Cu bimetallic supported MXene-based ammonia catalytic oxidation catalyst (labeled as S1).
[0035] Example 2 The difference from Example 1 is that in step S2, 0.143g of copper nitrate hexahydrate was weighed and dissolved in 20g of deionized water to prepare a copper nitrate solution; 10g of Ti3C2MXene powder and 0.5g of soluble starch were added to the copper nitrate solution, stirred and mixed, and then transferred to a micro planetary mill and ground at 500r / min for 5min at a grinding temperature of 25℃ to obtain a mixed slurry A. In step S3, 0.3g of platinum nitrate solution (Pt content 10%) was added dropwise and stirred to obtain solution B. In step S5, the temperature was raised to 400℃ and calcined for 2h; other steps remained unchanged to obtain the Pt-Cu bimetallic supported MXene-based ammonia catalytic oxidation catalyst (labeled as S2).
[0036] Example 3 The difference from Example 1 is that in step S2, 7g of copper nitrate hexahydrate is weighed and dissolved in 20g of deionized water to prepare a copper nitrate solution; 10g of Ti3C2MXene powder and 0.5g of soluble starch are added to the copper nitrate solution, stirred and mixed, and then ground in a micro planetary mill at 1000 rpm for 2 min at a grinding temperature of 25°C to obtain a mixed slurry A. In step S3, 0.3g of platinum nitrate solution (Pt content 10%) is added dropwise and stirred to obtain solution B. In step S5, the temperature is raised to 500°C and calcined for 1 h; other steps remain unchanged to obtain the Pt-Cu bimetallic supported MXene-based ammonia catalytic oxidation catalyst (labeled as S3).
[0037] Comparative Example 1 The difference from Example 1 is that copper nitrate hexahydrate in step S2 is replaced with 0.275g cerium nitrate hexahydrate; the other steps remain unchanged, and a Pt-Ce bimetallic supported MXene-based ammonia catalytic oxidation catalyst (labeled D1) is obtained.
[0038] Comparative Example 2 The difference from Example 1 is that the addition of copper nitrate hexahydrate in step S2 is omitted; the other steps remain unchanged, and a Pt single-metal supported MXene-based ammonia catalytic oxidation catalyst (labeled as D2) is obtained.
[0039] Comparative Example 3 The difference from Example 1 is that the addition of platinum nitrate solution in step S3 is omitted; the other steps remain unchanged, and a Cu single metal supported MXene-based ammonia catalytic oxidation catalyst (labeled as D3) is obtained.
[0040] Comparative Example 4 The difference from Example 1 is that the alkali-treated Ti3C2MXene in step S2 is replaced with conventional alumina powder; the other steps remain unchanged, and a Pt-Cu bimetallic supported alumina-based ammonia catalytic oxidation catalyst (labeled D4) is obtained.
[0041] Comparative Example 5 The difference from Example 1 is that the alkali-treated Ti3C2MXene in step S2 is replaced with conventional titanium dioxide powder; the other steps remain unchanged, and a Pt-Cu bimetallic supported titanium dioxide-based ammonia catalytic oxidation catalyst (labeled D5) is obtained.
[0042] The catalysts prepared in Examples 1-3 and Comparative Examples 1-5 were subjected to catalytic activity testing under the following specific conditions: The catalyst was sequentially tableted, crushed, and sieved to 80 mesh. 0.2 g of the sieved catalyst was weighed and loaded into a tubular reactor for ammonia catalytic oxidation activity evaluation. The test gas composition was: NH3 = 1000 ppm, H2O = 10%, O2 = 10%, with the remainder being N2. The total flow rate of the test gas was 200 mL / min, and the space velocity was 60000 h⁻¹. -1 The test temperature range was 140℃-300℃. The testing instrument was a Gasmet (portable Fourier transform infrared spectrometer DX4000). The conversion rate of NH3 and the selectivity of N2 at 140-300℃ were tested for the catalysts prepared in Examples 1-3 and Comparative Examples 1-5, respectively. The test results are shown in Tables 1 and 2. Figure 1 and Figure 2 As shown.
[0043] The formula for calculating the NH3 conversion rate is: (NH3 concentration at reactor inlet) (NH3 concentration at reactor outlet) / NH3 concentration at reactor inlet × 100%; The formula for calculating the selectivity of N2 is: (NH3 concentration at reactor inlet - NH3 concentration at reactor outlet - NO concentration at reactor outlet - N2O concentration at reactor outlet × 2 - NO2 concentration at reactor outlet) / (NH3 concentration at reactor inlet - NH3 concentration at reactor outlet) × 100%.
[0044] Table 1. NH3 conversion rate of the catalyst at temperatures ranging from 140℃ to 300℃.
[0045] Table 2. Selectivity of catalysts for N2 at 140-300℃
[0046] Through Tables 1 and 2, Figure 1 and Figure 2 It can be seen that the catalyst in Example 1 exhibits good low-temperature activity and N2 selectivity. Compared to Examples 2 and 3, Examples 1-3 all demonstrate high activity. However, the low Cu content in Example 2 resulted in slightly lower N2 selectivity, while the excessive Cu content in Example 3 only slightly improved N2 selectivity. Comparative Examples 1-5 show that Pt is the main active material, while Cu demonstrates a particularly significant advantage in high N2 selectivity. In Comparative Examples 4-5, which used the same active components and preparation methods, only the commercially available alumina and titanium dioxide from different manufacturers were replaced, resulting in significantly lower activity and N2 selectivity compared to Example 1.
[0047] In summary, this invention utilizes the abundant defect sites, strong electron migration, and oxygen overflow characteristics of Ti3C2MXene to promote the migration of electron and oxygen species in the catalyst, and synergistically lowers the energy barrier of ammonia activation reaction with the Pt-Cu bimetallic active component, thereby achieving the catalytic oxidation of ammonia at low temperatures while maintaining high N2 selectivity.
[0048] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A bimetallic supported MXene-based ammocatalytic oxidation catalyst, characterized in that, The Pt-Cu bimetallic active component is loaded on the surface and inside of the Ti3C2 MXene carrier.
2. The bimetallic supported MXene-based ammocatalytic oxidation catalyst of claim 1, wherein, The mass ratio of Pt to Cu in the Pt-Cu bimetallic active component is 1: (1-50.5).
3. The bimetallic supported MXene-based ammocatalytic oxidation catalyst of claim 1, wherein, The loading amount of the Pt-Cu bimetallic active component is 0.5wt%-14wt%.
4. A method for preparing the bimetallic supported MXene-based ammocatalytic oxidation catalyst according to any one of claims 1 to 3, characterized in that, The method comprises the following steps: The Ti3C2 MXene after alkali treatment, a copper metal precursor, a pore-forming agent and water are mixed, stirred and dispersed, and then ground to obtain a mixed slurry A; A platinum metal precursor and a dispersing agent are added to water, and stirred until fully mixed to obtain a solution B; The solution B is added to the mixed slurry A and stirred until uniform, and then dried and calcined in sequence to obtain the Pt-Cu bimetallic loaded MXene-based ammonia catalytic oxidation catalyst.
5. The method for preparing a bimetallic supported MXene-based ammocatalytic oxidation catalyst according to claim 4, wherein, The alkali treatment method of the Ti3C2 MXene is as follows: Ti3AlC2 powder is added to concentrated alkali solution in batches and stirred and mixed to obtain a suspension; the suspension is subjected to hydrothermal reaction; after cooling to room temperature, water is added to the reaction system to terminate the reaction, and then centrifugal separation, washing, freeze-drying and crushing treatment are performed to obtain the Ti3C2 MXene after alkali treatment.
6. The method for preparing a dual-metal-loaded MXene-based ammocatalytic oxidation catalyst according to claim 5, wherein, The temperature of the hydrothermal reaction is 260-280℃, and the time is 10-20h.
7. The method for preparing a dual-metal-loaded MXene-based ammocatalytic oxidation catalyst according to claim 4, wherein The mass ratio of the Ti3C2 MXene after alkali treatment, the copper metal precursor and the pore-forming agent is 10: (0.1-7): 0.
5. The rotation speed of the grinding treatment is 300-1500r / min, and the grinding time is 2-10min.
8. The method for preparing a dual-metal-loaded MXene-based ammocatalytic oxidation catalyst according to claim 4, wherein, The temperature of the drying is 60-120℃, and the time is 2-24h. The temperature of the calcination treatment is 300-500℃, and the time is 1-5h.
9. The method for preparing a dual-metal-loaded MXene-based ammocatalytic oxidation catalyst according to claim 4, wherein, The copper metal precursor is at least one of copper nitrate hexahydrate or copper chloride; The platinum metal precursor is at least one of platinum nitrate or platinum chloride; The dispersing agent is polyethylene glycol.
10. Application of the bimetallic loaded MXene-based ammonia catalytic oxidation catalyst according to any one of claims 1-3 in ammonia catalytic oxidation at 140-300℃.