A nitrogen-doped biochar-supported iron-based PVC low-temperature dechlorination hydrogen production catalyst
By preparing a nitrogen-doped biochar-supported iron-based catalyst, the problems of high cost and easy deactivation at high temperatures of PVC dechlorination catalysts were solved, achieving low-temperature and efficient dechlorination and hydrogen production, which is suitable for large-scale production.
Patent Information
- Application Number
- CN202611209842.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-11
- Publication Date
- 2026-11-17
AI Technical Summary
Existing PVC dechlorination catalysts are expensive, their active components are prone to agglomeration, they require high-temperature operation, and their carrier pore structure is insufficient, resulting in high energy consumption and limited catalytic performance, making large-scale application difficult.
A nitrogen-doped biochar-supported iron-based catalyst was developed. The biochar carrier was prepared from corn stalk powder and combined with hydrothermal pre-carbonization, high-temperature roasting and low-temperature calcination processes to achieve highly dispersed loading and porous structure of iron active components, thereby reducing the activation energy of the dechlorination reaction.
It achieves efficient dechlorination and hydrogen production at low temperatures, reduces raw material costs and energy consumption, extends catalyst life, and is suitable for large-scale production.
Smart Images

Figure CN123102399A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of catalyst preparation technology, and in particular to a nitrogen-doped biochar-supported iron-based PVC low-temperature dechlorination and hydrogen production catalyst. Background Technology
[0002] Polyvinyl chloride (PVC) is a widely used general-purpose plastic, and improper disposal of its waste can cause a serious environmental burden. Thermal dechlorination of PVC to produce hydrogen is an important technical route for realizing the resource utilization of waste PVC. It can produce hydrogen-rich gas while recovering chlorine, which has both environmental benefits and resource value. The dechlorination catalyst is the core of this process, which directly determines the efficiency of the dechlorination reaction, the reaction temperature and the product distribution. Existing PVC dechlorination catalysts mostly use precious or rare metals as active components, resulting in high raw material costs and making large-scale industrial applications difficult. Some iron-based catalysts suffer from agglomeration and poor dispersion of active components, requiring higher temperatures to exert their catalytic activity, leading to high energy consumption. Furthermore, they are prone to coking and deactivation at high temperatures. Meanwhile, existing catalyst supports mostly rely on fossil-based carbon materials, resulting in high carbon emissions during the preparation process, which is inconsistent with the development direction of green production. Moreover, the pore structure and surface properties of the supports are not well controlled, failing to provide sufficient loading sites and mass transfer channels for the active components, further limiting the improvement of catalytic performance. Summary of the Invention
[0003] The purpose of this invention is to provide a nitrogen-doped biochar-supported iron-based PVC low-temperature dechlorination hydrogen production catalyst to solve the problems mentioned in the background art.
[0004] To achieve the above objectives, the present invention adopts the following technical solution: A nitrogen-doped biochar-supported iron-based PVC low-temperature dechlorination and hydrogen production catalyst, with a total dry basis of 100 parts, contains 62 parts corn stalk powder, 18 parts urea, 15 parts ferric chloride hexahydrate, and 5 parts potassium bicarbonate. The catalyst is prepared by the following steps: raw material pretreatment, hydrothermal precarbonization, high-temperature calcination carrier preparation, equal-volume impregnation loading, low-temperature calcination activation, and molding and sieving.
[0005] As a further improvement to this technical solution: the corn stalk powder has a cellulose content ≥40%, ash content ≤5%, and initial moisture content ≤8%; the urea has a purity ≥99.0% and a total nitrogen content ≥46.0%; the ferric chloride hexahydrate has a purity ≥99.0% and an iron content ≥20.0%; the potassium bicarbonate has a purity ≥99.5% and a particle size D... 50 ≤50μm.
[0006] As a further improvement to this technical solution: the raw material pretreatment step is as follows: corn stalks are rinsed with clean water and dried at 80℃ for 6 hours, crushed and passed through an 80-mesh sieve, and the sieve-filled straw powder is collected.
[0007] As a further improvement to this technical solution: the hydrothermal precarbonization step is as follows: weigh straw powder, urea and potassium bicarbonate according to the ratio, add deionized water and mix for 30 minutes. The material-liquid mass ratio is 1:10. Transfer the mixed slurry into a hydrothermal reactor and keep it at 180°C for 6 hours. After cooling, wash until the filtrate is neutral and vacuum dry at 80°C for 12 hours to obtain the precarbonized nitrogen-doped precursor.
[0008] As a further improvement to this technical solution: the specific steps for preparing the high-temperature calcination carrier are as follows: the pre-carbonized nitrogen-doped precursor is placed in a tube furnace and heated to 600°C at a rate of 5°C / min under a nitrogen atmosphere, held at a constant temperature for 2 hours, and cooled with the furnace to obtain crude biochar; the crude biochar is soaked in 1 mol / L hydrochloric acid for 4 hours, washed until neutral, and then dried to obtain a nitrogen-doped porous biochar carrier.
[0009] As a further improvement to this technical solution: the equal volume impregnation loading step is specifically as follows: ferric chloride hexahydrate is prepared into an aqueous solution and added dropwise to a nitrogen-doped porous biochar support while stirring. After the addition is completed, the solution is sealed and allowed to stand for 12 hours, and then vacuum dried at 70°C for 8 hours to obtain the iron-loaded catalyst precursor.
[0010] As a further improvement to this technical solution: the low-temperature calcination activation step is specifically as follows: the iron-loaded catalyst precursor is placed in a tube furnace, heated to 450°C at a rate of 3°C / min under a nitrogen atmosphere, kept at a constant temperature for 1.5 hours, and cooled with the furnace to obtain the crude catalyst.
[0011] As a further improvement to this technical solution: the molding and screening step is as follows: the crude catalyst is pressed into tablets under 10MPa pressure for 30s, crushed, and then passed through a double-layer sieve of 20 mesh and 40 mesh to collect particles of intermediate size.
[0012] Compared with the prior art, the beneficial effects of the present invention are: 1. This invention uses corn stalks, an agricultural waste, as a carbon source to prepare biochar carriers, replacing traditional fossil-based carbon materials. This realizes the resource utilization of biomass resources, reduces the raw material cost of catalysts and the environmental impact of the preparation process. At the same time, it uses urea as a nitrogen dopant source and iron salt as an active component precursor. The raw materials are readily available, the overall preparation process is clear and controllable, the parameters of each step are well-defined, the performance stability of batch products is high, and it is suitable for the needs of large-scale production. 2. This invention achieves in-situ nitrogen doping by combining hydrothermal predoping with high-temperature calcination. Combined with equal-volume impregnation and low-temperature calcination, the iron active component is loaded onto the surface of porous biochar in a highly dispersed state. The nitrogen doping sites and the iron active phase form a synergistic catalytic effect, which effectively reduces the activation energy of the PVC dechlorination reaction. It can achieve efficient dechlorination and hydrogen production at a lower temperature. At the same time, the hierarchical pore structure of the support ensures the mass transfer efficiency of the reaction process, helps to extend the service life of the catalyst, and improves the overall reaction economy.
[0013] The above description is merely an overview of the technical solution of the present invention. In order to better understand the technical means of the present invention and to implement it in accordance with the contents of the specification, the preferred embodiments of the present invention are described in detail below with reference to the accompanying drawings. Specific implementation methods are given in detail in the following embodiments and their accompanying drawings. Attached Figure Description
[0014] The accompanying drawings, which are included to provide a further understanding of the invention and form part of this application, illustrate exemplary embodiments of the invention and, together with their description, serve to explain the invention and do not constitute an undue limitation thereof. In the drawings: Figure 1 This is a schematic diagram of the structure of the present invention. Detailed Implementation
[0015] The principles and features of the present invention are described below with reference to the accompanying drawings. The examples given are for illustrative purposes only and are not intended to limit the scope of the invention. The invention is described more specifically in the following paragraphs by way of example with reference to the accompanying drawings. It should be noted that the drawings are in a very simplified form and use non-precise proportions, and are only used to facilitate and clarify the illustration of the embodiments of the present invention.
[0016] Please see Figure 1 In this embodiment of the invention, a nitrogen-doped biochar-supported iron-based PVC low-temperature dechlorination and hydrogen production catalyst is provided. The total dry basis of the materials is 100 parts, and the raw materials include 62 parts of corn stalk powder, 18 parts of urea, 15 parts of ferric chloride hexahydrate, and 5 parts of potassium bicarbonate. The catalyst is prepared by the following steps: raw material pretreatment, hydrothermal precarbonization, high-temperature calcination carrier preparation, equal volume impregnation and loading, low-temperature calcination activation, and molding and sieving. Specifically, in terms of raw material composition, the total dry basis material is measured in 100 parts, with corn straw powder as the precursor carbon source of biochar, urea as the nitrogen dopant, ferric chloride hexahydrate as the precursor of iron active component, and potassium bicarbonate as the pore-forming activator. The four types of raw materials respectively play the roles of carrier construction, nitrogen element introduction, active site loading, and pore structure regulation, and together constitute the material basis of the catalyst. The overall preparation process is divided into six core stages, namely raw material pretreatment, hydrothermal precarbonization, high-temperature calcination carrier preparation, equal-volume impregnation loading, low-temperature calcination activation, and molding and sieving. Each stage is connected in sequence to complete the conversion from biomass raw materials to finished catalyst.
[0017] Corn stalk powder: cellulose content ≥40%, ash content ≤5%, initial moisture content ≤8%; urea purity ≥99.0%, total nitrogen content ≥46.0%; ferric chloride hexahydrate purity ≥99.0%, iron content ≥20.0%; potassium bicarbonate purity ≥99.5%, particle size D... 50 ≤50μm; Specifically, corn stalk powder is derived from mature corn stalks, requiring a cellulose content of no less than 40%, an ash content of no more than 5%, an initial moisture content of no more than 8%, and freedom from mold, insect infestation, and obvious mud and sand impurities. The stalks must first be rinsed with clean water to remove surface mud and sand, drained, and then dried using a forced-air drying oven, model GZX-9070MBE. This equipment has a temperature control range covering room temperature to 200℃, a temperature control accuracy of ±1℃, and an air volume of 50 to 200 m³ / h. 3 The speed is adjustable within the range of 1000 to 3000 r / min. The inner liner is made of 304 stainless steel and equipped with a removable drying tray to remove free moisture from the straw and prevent sticking during subsequent crushing. After drying, the straw is fed into a high-speed universal crusher (model WF-130) for crushing. The inner liner is also made of 304 stainless steel. The speed is adjustable within the range of 1000 to 3000 r / min and equipped with an 80-mesh standard screen to crush the straw to the target particle size range, ensuring the uniformity of the subsequent carbonization reaction. The crushed material is then screened by a vibrating screener (model ZS-515). The screen is made of 304 stainless steel and the vibration frequency is adjustable within the range of 800 to 1800 times / min. The amplitude is adjustable within the range of 3 to 8 mm and equipped with a sealed dust cover to screen straw powder that meets the particle size requirements and remove coarse fibers and impurities. Urea is an analytical grade reagent with a purity of not less than 99.0% and a total nitrogen content of not less than 46.0%. It appears as white crystalline granules, without clumping or deliquescence. No additional pretreatment is required before use; it can be directly weighed and added. Ferric chloride hexahydrate is an analytical grade reagent with a purity of not less than 99.0% and an iron content of not less than 20.0%. It appears as orange-yellow crystals without obvious impurities. It needs to be prepared into an aqueous solution before use. During the preparation process, a magnetic stirrer is used to assist in dissolution to ensure complete dispersion of the iron salt. Potassium bicarbonate is an analytical grade reagent with a purity of not less than 99.5% and a particle size D. 50 It has a particle size of no more than 50 μm, a whiteness of no less than 90%, and is free of lumps. It can be directly fed into the container before use and is used to construct a porous structure during the carbonization process.
[0018] The specific steps of raw material pretreatment are as follows: corn stalks are rinsed with clean water and dried at 80℃ for 6 hours, crushed and passed through an 80-mesh sieve, and the straw powder under the sieve is collected. Specifically, the operation process is as follows: the corn stalks are rinsed with clean water to remove the mud and dust attached to the surface, and after draining the surface water, they are placed in a drying device and dried at 80℃ for 6 hours to reduce the moisture content of the stalks to a suitable range for crushing; the dried stalks are then put into a crushing device for crushing, and the crushed material is sieved through an 80-mesh screen. The straw powder that is sieved is collected, and the coarse fiber residue on the screen is returned to the crusher for further crushing until all of it passes through the screen. The core equipment used includes a blower drying oven, a high-speed universal pulverizer, and a vibrating screen, and the equipment models and uses are consistent with those described in claim 2; the core purpose is to obtain straw powder with uniform particle size and stable moisture content, so as to provide a uniform raw material basis for subsequent hydrothermal reactions.
[0019] The hydrothermal precarbonization step is as follows: weigh straw powder, urea and potassium bicarbonate according to the ratio, add deionized water and mix for 30 minutes. The material-liquid mass ratio is 1:10. Transfer the mixed slurry into the hydrothermal reactor and keep it at 180℃ for 6 hours. After cooling, wash until the filtrate is neutral and vacuum dry at 80℃ for 12 hours to obtain the precarbonized nitrogen-doped precursor. Specifically, the operation process is as follows: Weigh the pretreated straw powder, urea, and potassium bicarbonate according to the ratio, add them sequentially to a container, add deionized water, control the material-to-liquid mass ratio to be 1:10, turn on the magnetic stirrer and stir for 30 minutes to completely disperse the solid materials in the water and form a uniform slurry; transfer the slurry into the lining of a hydrothermal reactor, seal the reactor and place it in a constant temperature oven, and keep it at 180℃ for 6 hours; after the reaction is completed, stop heating, and after the reactor cools naturally to room temperature, take out the material, use a vacuum filtration device to separate the solid and liquid, and repeatedly wash the filter cake with deionized water until the pH value of the filtrate is in the neutral range of 6.5 to 7.0; put the washed filter cake into a vacuum drying oven and dry it at 80℃ for 12 hours to finally obtain the pre-nitrogen carbide doped precursor; The core equipment used includes a hydrothermal reactor, a constant temperature oven, and a vacuum drying oven. The hydrothermal reactor, model KH-200, is lined with polytetrafluoroethylene (PTFE), has a rated volume of 200 mL, a maximum withstand temperature of 220℃, and a maximum withstand pressure of 3 MPa. The reactor body is made of stainless steel with fastening bolts, providing a closed, high-pressure hydrothermal environment to support the initial carbonization process of biomass and the initial loading of nitrogen components. This allows nitrogen to be pre-embedded in the biomass carbon skeleton, reducing nitrogen loss during subsequent high-temperature roasting. Simultaneously, potassium bicarbonate is initially activated in the hydrothermal environment, laying the foundation for subsequent pore structure formation. The constant temperature drying oven, model DHG-9070A, has a temperature control range from room temperature to 250℃, with a temperature control accuracy of ±1℃. It has a 70L inner chamber and is equipped with a hot air circulation system to provide a uniform and stable temperature environment for the hydrothermal reaction, ensuring consistent reaction throughout the reactor. The vacuum drying oven, model DZF-6050, has a temperature control range of 5 to 200℃ and a maximum vacuum degree not exceeding -0.095MPa. Its inner chamber is made of 304 stainless steel and is equipped with three removable drying trays for drying hydrothermal reaction products and removing residual moisture. The vacuum environment also prevents the precursors from oxidizing upon contact with air.
[0020] The specific steps for preparing the high-temperature calcination support are as follows: the pre-carbonized nitrogen-doped precursor is placed in a tube furnace and heated to 600°C at a rate of 5°C / min under a nitrogen atmosphere. The temperature is maintained at 600°C for 2 hours and then cooled with the furnace to obtain crude biochar. The crude biochar is soaked in 1 mol / L hydrochloric acid for 4 hours, washed until neutral, and then dried to obtain a nitrogen-doped porous biochar support. Specifically, the operation process is as follows: The pre-carbonized nitrogen-doped precursor is evenly spread inside a corundum boat, with the thickness of the spread material not exceeding 2 cm. The boat is then pushed into the constant-temperature zone of a tubular atmosphere furnace. After closing the furnace door, high-purity nitrogen is introduced at a flow rate of 0.5 L / min for 10 minutes to replace the air inside the furnace. This replacement operation is repeated three times to ensure an inert atmosphere is formed inside the furnace. The programmed heating system is started, with a heating rate of 5℃ / min, raising the temperature from room temperature to 600℃. After reaching the set temperature, the temperature is held constant for 2 hours. After calcination, heating is stopped, and nitrogen is continuously introduced to allow the material to cool naturally to room temperature with the furnace. Crude biochar is then removed. The crude biochar is immersed in a 1 mol / L hydrochloric acid solution at a liquid-to-solid mass ratio of 5:1 for 4 hours to dissolve and remove ash and impurity minerals from the crude biochar. After immersion, the material is removed and repeatedly washed with deionized water until the filtrate is neutral. The washed material is then dried to constant weight using a drying device to finally obtain a nitrogen-doped porous biochar carrier. The core equipment used includes a tubular atmosphere furnace and a corundum boat. The tubular atmosphere furnace is model GSL-1200X, with a furnace tube diameter of φ80mm. Its temperature control range covers room temperature to 1200℃, with a temperature control accuracy of ±1℃. The gas flow rate is adjustable from 0.1 to 1L / min. It is equipped with a programmed temperature control system and an exhaust gas outlet to provide an inert nitrogen atmosphere and programmed temperature environment, supporting the high-temperature carbonization process of the precursor and the in-situ doping process of nitrogen. Under high-temperature conditions, biomass further carbonizes to form a carbon skeleton. The nitrogen-containing gas produced by urea decomposition reacts with the carbon skeleton, introducing nitrogen atoms into the carbon lattice to form nitrogen doping sites. Simultaneously, the gas produced by the high-temperature decomposition of potassium bicarbonate acts as a pore-forming agent, forming a rich porous structure. The corundum boat is made of 99% alumina, with dimensions of 100mm×50mm×20mm and a maximum withstand temperature of 1600℃. It is used to hold the roasting material, isolate the material from the inner wall of the furnace tube to prevent material contamination of the furnace tube, and ensure that the material is evenly spread and heated uniformly.
[0021] The specific steps of the equal volume impregnation loading are as follows: ferric chloride hexahydrate is prepared into an aqueous solution and added dropwise to a nitrogen-doped porous biochar support while stirring. After the addition is completed, the solution is sealed and allowed to stand for 12 hours. The solution is then vacuum dried at 70°C for 8 hours to obtain the iron-loaded catalyst precursor. Specifically, the operation process is as follows: First, the saturated liquid adsorption capacity of the nitrogen-doped porous biochar support is measured. Ferric chloride hexahydrate is weighed according to the ratio, and a quantitative amount of deionized water is added and stirred until completely dissolved to prepare an iron salt solution with a matching concentration. The biochar support is placed in a stirring container, and the iron salt solution is added to the support dropwise while gently stirring to ensure that the iron salt solution is uniformly adsorbed by the support until saturation adsorption is achieved. After the addition is completed, the container is sealed and allowed to stand for 12 hours to allow iron ions to fully diffuse into the pores of the biochar, achieving a uniform distribution of the active components on the surface and within the pores of the support. After standing, the material is transferred to a vacuum drying oven and dried at 70°C for 8 hours to remove solvent and moisture, obtaining the iron-loaded catalyst precursor. The core equipment used includes an electronic analytical balance and a vacuum drying oven. The electronic analytical balance, model FA2004, has a weighing range of 0 to 200g and a weighing accuracy of 0.1mg. It is used to accurately weigh iron salt raw materials and carrier raw materials to ensure the accuracy of impregnation solution concentration and load. The vacuum drying oven, model DZF-6050, is used in this process to dry the impregnated materials. The low-temperature vacuum environment can slowly remove moisture, prevent iron components from agglomerating with moisture migration, and ensure the dispersion of active components.
[0022] The specific steps of the low-temperature calcination activation are as follows: the iron-loaded catalyst precursor is placed in a tube furnace and heated to 450°C at a rate of 3°C / min under a nitrogen atmosphere, held at a constant temperature for 1.5 hours, and cooled with the furnace to obtain the crude catalyst. Specifically, the operation process is as follows: the iron-loaded catalyst precursor is evenly spread in the corundum boat and placed in the constant temperature zone of the tubular atmosphere furnace; high-purity nitrogen is introduced to replace the air in the furnace, and the gas flow rate is controlled at 0.5 L / min; the programmed heating system is started, the heating rate is set to 3℃ / min, and the temperature is raised from room temperature to 450℃. After reaching the set temperature, it is kept at a constant temperature for 1.5 hours; after calcination, heating is stopped, and nitrogen is continuously introduced to allow the material to cool naturally to room temperature with the furnace, and the crude catalyst product is obtained. The core equipment used is a tubular atmosphere furnace, the model of which is the same as that described in claim 5. In this process, the iron salt loaded on the surface of biochar decomposes under a low-temperature inert atmosphere to form an iron oxide composite active phase, which interacts with the nitrogen doping sites on the surface of the support to form a stable catalytic active center. The lower calcination temperature can prevent the iron particles from agglomerating and growing, maintain the high dispersion of the active components, and ensure that the pore structure of the biochar support is not destroyed.
[0023] The specific steps of the molding and screening process are as follows: the crude catalyst is pressed into tablets under 10MPa pressure for 30s, crushed and then passed through a double-layer sieve of 20 mesh and 40 mesh to collect particles of intermediate size. Specifically, the operation process is as follows: the crude catalyst is placed into the mold of the tablet press, the pressing pressure is set to 10MPa, and the pressure is held for 30 seconds to press the powdered catalyst into tablets; the tablets are then removed and crushed, and the crushed material is transferred to a vibrating screen, which is equipped with a double-layer stainless steel screen of 20 mesh and 40 mesh for grading and screening, collecting particles of the middle size, returning the large particles on the screen to the crushing process for further processing, and returning the fine powder under the screen to the impregnation process for recycling; The core equipment used includes a manual tablet press and a vibrating screen. The manual tablet press is model YP-15, with a pressure adjustment range of 0 to 15 MPa, and is equipped with a φ30mm tablet pressing mold. It is used to compress the powdered catalyst into shape, reduce the bed pressure drop of the catalyst in the reactor, and adapt to the filling requirements of the fixed bed reactor. The vibrating screen is model ZS-515, which is used in this process to classify and screen catalyst particles that meet the particle size requirements, ensuring that the finished product has a uniform particle size and avoiding problems such as bed blockage or uneven airflow distribution during use.
[0024] The method of use and working principle of this invention are as follows: Instructions for use: First, prepare the catalyst according to the preparation process. Fill the isothermal section of the fixed-bed reactor with the shaped and sieved finished catalyst. After filling, purge the air in the reactor with nitrogen. Then, heat the reactor to the set reaction temperature. After the temperature stabilizes, feed the PVC material into the reactor to ensure full contact with the catalyst bed. Under the action of the catalyst, a thermal dechlorination reaction will occur. The chlorine-containing products and hydrogen-rich gas produced by the reaction will be discharged from the reactor outlet and subsequently collected and purified by a separation device. After the reaction is completed, stop feeding and continue to purge the reactor with nitrogen. After the reactor cools down to room temperature, the deactivated catalyst can be recovered and regenerated.
[0025] Working principle: Using biomass straw as a carbon source precursor, a nitrogen-doped porous biochar carrier is constructed through a two-step method combining hydrothermal pre-carbonization and high-temperature calcination. Potassium bicarbonate is used to activate the carbon framework, forming a hierarchical pore structure. Simultaneously, in-situ doping with urea introduces nitrogen atoms into the carbon lattice, creating abundant nitrogen defect sites on the carrier surface. Subsequently, an equal-volume impregnation method is used to uniformly load the iron active component onto the carrier surface and within the pores. Low-temperature calcination decomposes the iron salts to form a highly dispersed iron oxide active phase, which synergistically interacts with the nitrogen doping sites. In the PVC dechlorination and hydrogen production reaction, the porous structure of the carrier provides mass transfer channels between reactants and products. The nitrogen doping sites activate the carbon-chlorine bonds in the PVC molecules, while the iron active phase catalyzes the cracking reaction. Together, they lower the activation energy of the reaction, achieving efficient dechlorination and hydrogen production under low-temperature conditions.
[0026] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention in any way. Those skilled in the art can readily implement the present invention based on the description and drawings above. However, any modifications, alterations, and variations made by those skilled in the art without departing from the scope of the present invention using the disclosed technical content are equivalent embodiments of the present invention. Furthermore, any modifications, alterations, and variations made to the above embodiments based on the essential technology of the present invention are still within the protection scope of the present invention.
Claims
1. A nitrogen-doped biochar-supported iron-based PVC low-temperature dechlorination and hydrogen production catalyst, characterized in that, The total dry basis material is calculated as 100 parts, and the raw materials include 62 parts corn straw powder, 18 parts urea, 15 parts ferric chloride hexahydrate, and 5 parts potassium bicarbonate. The catalyst is prepared by the following steps: raw material pretreatment, hydrothermal precarbonization, high-temperature roasting carrier preparation, equal volume impregnation loading, low-temperature calcination activation, and molding and sieving.
2. The nitrogen-doped biochar-supported iron-based PVC low-temperature dechlorination hydrogen production catalyst according to claim 1, characterized in that, The corn stalk powder has a cellulose content ≥40%, ash content ≤5%, and initial moisture content ≤8%; the urea has a purity ≥99.0% and a total nitrogen content ≥46.0%; the ferric chloride hexahydrate has a purity ≥99.0% and an iron content ≥20.0%; the potassium bicarbonate has a purity ≥99.5% and a particle size D... 50 ≤50μm.
3. The nitrogen-doped biochar-supported iron-based PVC low-temperature dechlorination hydrogen production catalyst according to claim 1, characterized in that, The specific steps of the raw material pretreatment are as follows: corn stalks are rinsed with clean water, dried at 80°C for 6 hours, crushed and passed through an 80-mesh sieve, and the straw powder under the sieve is collected.
4. The nitrogen-doped biochar-supported iron-based PVC low-temperature dechlorination hydrogen production catalyst according to claim 3, characterized in that, The hydrothermal precarbonization step is as follows: weigh straw powder, urea, and potassium bicarbonate according to the ratio, add deionized water and mix for 30 minutes. The material-liquid mass ratio is 1:
10. Transfer the mixed slurry into a hydrothermal reactor and keep it at 180°C for 6 hours. After cooling, wash until the filtrate is neutral and vacuum dry at 80°C for 12 hours to obtain the precarbonized nitrogen-doped precursor.
5. The nitrogen-doped biochar-supported iron-based PVC low-temperature dechlorination hydrogen production catalyst according to claim 4, characterized in that, The specific steps for preparing the high-temperature calcination support are as follows: the pre-carbonized nitrogen-doped precursor is placed in a tube furnace and heated to 600°C at a rate of 5°C / min under a nitrogen atmosphere, held at a constant temperature for 2 hours, and cooled with the furnace to obtain crude biochar; the crude biochar is soaked in 1 mol / L hydrochloric acid for 4 hours, washed until neutral, and then dried to obtain a nitrogen-doped porous biochar support.
6. The nitrogen-doped biochar-supported iron-based PVC low-temperature dechlorination hydrogen production catalyst according to claim 5, characterized in that, The specific steps of the equal-volume impregnation and loading are as follows: ferric chloride hexahydrate is prepared into an aqueous solution and added dropwise to a nitrogen-doped porous biochar support while stirring. After the addition is completed, the solution is sealed and allowed to stand for 12 hours, and then vacuum dried at 70°C for 8 hours to obtain the iron-loaded catalyst precursor.
7. The nitrogen-doped biochar-supported iron-based PVC low-temperature dechlorination hydrogen production catalyst according to claim 6, characterized in that, The specific steps of the low-temperature calcination activation are as follows: the iron-loaded catalyst precursor is placed in a tube furnace and heated to 450°C at a rate of 3°C / min under a nitrogen atmosphere, held at a constant temperature for 1.5 hours, and then cooled with the furnace to obtain the crude catalyst.
8. The nitrogen-doped biochar-supported iron-based PVC low-temperature dechlorination hydrogen production catalyst according to claim 7, characterized in that, The specific steps of the molding and screening process are as follows: the crude catalyst is pressed into tablets under 10MPa pressure for 30s, crushed, and then passed through a double-layer sieve of 20 mesh and 40 mesh to collect particles of intermediate size.