A hydrophobic supported palladium-silver catalyst and its preparation method

By forming a hydrophobic layer on the surface of the C4 fraction hydrogenation catalyst, the problem of water molecules being easily adsorbed on the catalyst is solved, thereby improving the catalyst's resistance to water interference and reaction efficiency, and extending the catalyst's service life.

CN123102422APending Publication Date: 2026-11-17PETROCHINA CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510629381.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-15
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing C4 fraction hydrogenation catalysts are prone to having their active sites occupied by water molecules under high water content conditions, leading to a decrease in reaction rate, uneven mass and heat transfer, poor catalyst stability, and easy coking, which affects reaction efficiency.

Method used

A palladium-silver catalyst was supported by an impregnation method. A hydrophobic layer was formed by spraying water, silane coupling agent and silicate ester solution on the catalyst surface. Perfluoroalkyltriethoxysilane was used to graft organic molecules containing -CF3 onto the catalyst surface to improve hydrophobicity and prevent water molecule cluster adsorption.

Benefits of technology

It achieves long-term stable operation of the catalyst under high water content, reduces coking rate, extends catalyst service life, and maintains good hydrogenation reaction efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005405707930000151
    Figure BDA0005405707930000151
  • Figure BDA0005405707930000161
    Figure BDA0005405707930000161
Patent Text Reader

Abstract

This invention discloses a hydrophobic supported palladium-silver catalyst and its preparation method. The preparation method includes: loading an active component onto a support using an impregnation method to obtain a semi-finished catalyst B; uniformly spraying water onto the semi-finished catalyst B and allowing it to stand; then sequentially spraying a solution of a silane coupling agent, allowing it to stand, washing, and standing; spraying a solution of a silicate ester, allowing it to stand; spraying a solution of perfluoroalkyltriethoxysilane, allowing it to stand, and drying to obtain the hydrophobic supported palladium-silver catalyst. The catalyst of this invention can be used in the selective hydrogenation process of aqueous C4 fractions, exhibiting good resistance to water interference. It can operate stably for a long time when the water content reaches 400-500 μg / g, and the coking rate of the catalyst is reduced by more than 70%, and the catalyst operating cycle is significantly extended.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of C4 hydrogenation catalysts, specifically to a hydrophobic supported palladium-silver catalyst and its preparation method. Background Technology

[0002] C4 fraction refers to a mixture of alkanes, alkenes, dienes, and alkynes containing four carbon atoms. It mainly comes from C4 by-products of secondary oil refining units, C4 by-products of ethylene cracking, C4 by-products of ethane cracking, and C4 by-products of coal-to-olefins cracking. It contains hydrocarbons such as n-butane, isobutane, 1-butene, trans-2-butene, cis-2-butene, isobutene, 1,2-butadiene, 1,3-butadiene, methylacetylene, ethylacetylene, and vinylacetylene. Industrially, it is mainly used to produce 1,3-butadiene, isobutene, and 1-butene.

[0003] 1-Butene is an important chemical raw material, used as a comonomer for linear low-density polyethylene (LLDPE) and a monomer for the polymerization of poly-1-butene, and can also be used to produce various fine chemicals. C4 hydrocarbons contain trace amounts of alkynes and dienes, which can easily polymerize and clog the pores of downstream catalysts under certain conditions. To avoid coking of the etherification catalyst and to improve the purity of the 1-butene product, these must be removed before further processing. Currently, the catalysts used in industrial production for the selective hydrogenation of C4 hydrocarbons to 1-butene are mainly noble metal palladium-based catalysts, such as Pd / Al2O3 catalysts and Pd-Ag / Al2O3 bimetallic catalysts.

[0004] In the hydrogenation reaction of C4 fraction, impurity water mainly exists in the form of water molecule clusters, which can move freely and participate in the reaction, interacting with reactants and catalysts. When there is too much water in the reaction system, water may occupy the active sites of the catalyst, hindering the contact between reactant molecules and the active centers of the catalyst, thereby reducing the reaction rate. In addition, the presence of water may also change the mass and heat transfer processes of the reaction, making the temperature and concentration distribution of the reaction system uneven and affecting the reaction process. On the surface of active metal catalysts, water may form strong chemical bonds with the active centers of the metal, reducing the catalytic activity of the active centers. Furthermore, water may also cause catalyst agglomeration and sintering. The presence of water may also affect the physical properties of the catalyst, such as causing the catalyst support to expand, deform, or pulverize. During the hydrogenation reaction, the catalyst needs to withstand certain conditions such as temperature, pressure, and fluid scouring. If the stability of the catalyst is affected, it may lead to catalyst breakage and loss, thus affecting the reaction process. For example, in a fixed-bed hydrogenation reactor, the breakage of catalyst particles may lead to increased bed resistance, affecting the diffusion of reactants and products and reducing reaction efficiency.

[0005] Furthermore, research has found that during the selective hydrogenation of C4 fractions, diene polymerization easily occurs, generating oligomers with a wide molecular weight range, commonly known as "green oil." Green oil is more likely to adsorb onto the catalyst surface and further form coke, blocking the catalyst pores and preventing reactants from diffusing to the active center surface of the catalyst, thus leading to a decrease in catalyst activity.

[0006] CN116422363A provides a method for preparing a hydrophobic Pd-based catalyst and the hydrophobic Pd-based catalyst. The method includes: adding a Pd precursor and a surfactant to an organic alcohol solvent, then adding an alkaline precipitant to adjust the pH to 9-13; dispersing the reaction system in an appropriate amount of ethanol solution and centrifuging and washing to obtain a Pd nanoparticle solution; mixing the Pd nanoparticle solution with HZ, and then washing, drying, and calcining to obtain PdOx / HZ (0≤x≤2, HZ is a ZSM-5 molecular sieve with a silicon-to-aluminum ratio of 500-2000 or a Y molecular sieve with a silicon-to-aluminum ratio of 500-2000); contacting an organic solution containing a silanizing agent with PdOx / HZ in the form of gas bubble deposition, so that the silanizing agent reacts with the surface of PdOx / HZ to form a SiO2 shell, thereby obtaining a Pd-based catalyst with the structure PdOx / HZ@SiO2. However, the high loading of Pd metal in the above catalysts easily leads to a decrease in the utilization rate of active sites and a deterioration in catalyst stability. CN106732771A discloses a method for preparing a hydrophobic nano-silicon sphere supported palladium-based catalyst, including the following steps: preparing nano-silicon spheres with hydrophobic and reducing groups by copolymerizing methyl orthosilicate and a silane coupling agent; reacting the nano-silicon spheres with palladium salt to obtain the hydrophobic nano-silicon sphere supported palladium-based catalyst. CN113354872A discloses a surface modification method for spherical alumina in superhydrophobic and highly fluid thermally conductive silicone grease. This method uses a mixture of spherical alumina and angular alumina as raw materials, hydrolyzing silane coupling agent 3-glycidyl etheroxypropyltrimethoxysilane, ethanol, and water in a certain proportion to form a hydrolysate, then adding a hydrophobic coupling agent dodecyltriethoxysilane to form a synergistic reaction; during modification, the mixed hydrolysate is sprayed onto the surface of the alumina filler and stirred to achieve the purpose of hydrophobic modification of the support. Jin Dayue et al. from Zhejiang University ("Construction of Short-Chain Fluorocarbon Fluorinated Silane Coupling Agents and Their Hydrophobic Coatings", Fine Chemicals, Vol. 37, No. 2, February 2020, pp. 412-419) prepared a hydrophobic coating substrate by coating a silica sol modified with KH550 onto a glass slide and heat-treating it at 300℃. A silane coupling agent was prepared into a trifluorotoluene solution, and the cured hydrophobic coating substrate was placed in it and assembled at room temperature for 24 hours. Subsequently, the modified glass slide was placed in an oven to obtain the hydrophobic coating.

[0007] Existing methods all involve modifying the catalyst surface, which may result in the active centers being covered or the hydrophobicity not meeting requirements. Modifying the catalyst support can cause irreversible changes to the surface properties of the support, making it difficult to prepare the desired catalyst. For example, the silica particles prepared by CN113354872A reach a scale of 60 nm, which is much larger than the 2-4 nm scale of the catalyst active centers, and the silica may cover the active centers. Summary of the Invention

[0008] The purpose of this invention is to provide a hydrophobic supported palladium-silver catalyst and its preparation method. This catalyst can be used for the selective hydrogenation of hydrous C4 materials, and not only has excellent selective hydrogenation performance, but also good resistance to water interference.

[0009] To achieve the above objectives, the present invention adopts the following technical solution:

[0010] This invention provides a method for preparing a hydrophobic supported palladium-silver catalyst, comprising the following steps:

[0011] The active components are loaded onto the support using an impregnation method to obtain a semi-finished catalyst B; the active components include palladium and silver.

[0012] Water is sprayed evenly onto the semi-finished catalyst B, and left to stand for a first preset time to obtain the semi-finished catalyst C.

[0013] The silane coupling agent solution is sprayed onto the semi-finished catalyst C, left to stand for a second preset time, washed, and then left to stand for a third preset time to obtain the semi-finished catalyst D.

[0014] A silicate solution is sprayed onto the semi-finished catalyst D and left to stand for a fourth preset time to obtain the semi-finished catalyst E.

[0015] A solution of perfluoroalkyltriethoxysilane was sprayed onto the semi-finished catalyst E, allowed to stand for a fifth preset time, and then dried to obtain the hydrophobic supported palladium-silver catalyst.

[0016] According to the preparation method of the present invention, preferably, the preparation process of the semi-finished catalyst B includes:

[0017] The support was impregnated in a Pd precursor salt solution, the pH of the solution was adjusted to 1.8-2.5, and a supersaturated impregnation method was used. After impregnation, the solution was dried and calcined to obtain a semi-finished catalyst A.

[0018] Semi-finished catalyst A was impregnated in a precursor salt solution of Ag using an equal-volume impregnation method. After impregnation, the catalyst was dried and calcined to obtain semi-finished catalyst B.

[0019] In the impregnation loading of the active component, this invention employs a conventional impregnation method, with the impregnation loading of metallic palladium being the same as that of ordinary shell catalyst impregnation techniques. The palladium-silver-based selective hydrogenation catalyst of this invention can be obtained using the preparation method recommended in this invention: impregnating the catalyst support with a palladium and silver solution, wherein palladium and silver are impregnated in a stepwise manner, followed by drying and calcination, to obtain the palladium-silver-based hydrogenation catalyst. The palladium-silver-based hydrogenation catalyst of this invention does not exclude the use of other modifying elements besides palladium and silver.

[0020] In the preferred preparation process of the semi-finished catalyst B, more preferably, the support is impregnated in the Pd precursor salt solution for 0.5 to 3 hours; then dried at 80 to 120°C for 1 to 6 hours, and calcined at 350 to 550°C for 2 to 8 hours.

[0021] In the preferred preparation process of the semi-finished catalyst B, more preferably, after the semi-finished catalyst A is impregnated in the precursor salt solution of Ag, it is dried at 80-120°C for 1-4 hours and calcined at 400-600°C for 2-6 hours.

[0022] In the preferred preparation process of the semi-finished catalyst B, more preferably, the precursor salt of Pd is selected from at least one of palladium nitrate, palladium acetate, and palladium chloride; more preferably, palladium chloride.

[0023] In the preferred preparation process of the semi-finished catalyst B, more preferably, the precursor salt of Ag is silver nitrate.

[0024] According to the preparation method of the present invention, preferably, the carrier is an alumina carrier or a mixed carrier with an alumina mass fraction of more than 80%; other metal oxides in the mixed carrier may be magnesium oxide, silicon oxide, etc.

[0025] More preferably, the alumina in the carrier is in a mixed crystal form.

[0026] According to the preparation method of the present invention, preferably, the first preset time is 10 to 30 minutes.

[0027] According to the preparation method of the present invention, preferably, the second preset time is 10-20 hours.

[0028] According to the preparation method of the present invention, preferably, the third preset time is 5 to 10 hours.

[0029] According to the preparation method of the present invention, preferably, the fourth preset time is 2 to 4 hours.

[0030] According to the preparation method of the present invention, preferably, the spray volume of the water is 75% to 90% of the water absorption rate of the carrier.

[0031] According to the preparation method of the present invention, preferably, the silane coupling agent is triethoxychlorosilane or trimethoxychlorosilane.

[0032] According to the preparation method of the present invention, preferably, the solvent in the solution of the silane coupling agent is a C6-C8 alkane, such as at least one selected from n-hexane, cyclohexane, n-heptane, etc.

[0033] According to the preparation method of the present invention, preferably, the mass content of the coupling agent in the solution of the silane coupling agent is 40% to 50%.

[0034] According to the preparation method of the present invention, preferably, the spray volume of the silane coupling agent solution is 5% to 15% of the water absorption rate of the carrier.

[0035] According to the preparation method of the present invention, preferably, the silicate ester is methyl orthosilicate or ethyl orthosilicate.

[0036] According to the preparation method of the present invention, preferably, the solvent in the silicate ester solution is a lower alcohol and water; the lower alcohol is selected from at least one of methanol, ethanol, propanol, and butanol. More preferably, the mass ratio of the lower alcohol, silicate ester, and water is 10:(3-5):(0.5-1).

[0037] According to the preparation method of the present invention, preferably, the solution preparation process of the silicate ester includes: weighing the silicate ester, lower alcohol and water, mixing them, and slowly stirring at 25-40°C for 30-60 min to obtain the silicate ester solution.

[0038] According to the preparation method of the present invention, preferably, the spray volume of the silicate ester solution is 10% to 20% of the water absorption rate of the carrier.

[0039] According to the preparation method of the present invention, preferably, the perfluoroalkyltriethoxysilane is perfluorooctyltriethoxysilane.

[0040] According to the preparation method of the present invention, preferably, the solvent in the solution of the perfluoroalkyltriethoxysilane is a C6-C8 alkane, such as at least one selected from n-hexane, cyclohexane, n-heptane, etc.

[0041] According to the preparation method of the present invention, preferably, the mass content of the perfluoroalkyltriethoxysilane in the solution of the perfluoroalkyltriethoxysilane is 50% to 70%.

[0042] According to the preparation method of the present invention, preferably, the spray volume of the perfluoroalkyltriethoxysilane solution is 5% to 15% of the water absorption rate of the carrier.

[0043] Water molecule clusters in the material readily adsorb and condense on the alumina surface, forming larger clusters. This is primarily due to the hydrophilicity of the catalyst surface, where aluminum hydroxyl groups can form hydrogen bonds with water molecules. Therefore, by sealing or covering the surface aluminum hydroxyl groups to prevent contact with water molecules, the catalyst surface can be transformed from hydrophilic to hydrophobic. This shortens the residence time of water molecules on the catalyst surface, preventing the formation of large water molecule clusters or their entry into the catalyst pores, thus avoiding interference with the catalytic reaction. In the preparation method of this invention, silica is first deposited on the alumina surface, and then the hydroxyl groups on the silica surface react with the active groups of organic molecules containing -CF3, effectively covering the alumina surface with -CF3-containing organic molecules and improving the hydrophobic effect of the catalyst surface.

[0044] -CF3 exhibits excellent hydrophobic properties, and the more -CF3 contained in the polymer chain, the better its hydrophobic properties. Therefore, this invention selects to graft organic molecules containing -CF3 onto the silica surface to enhance the hydrophobicity of the catalyst. However, after a hydrophobic layer is formed on the alumina surface, there are no exposed aluminum hydroxyl groups, making it difficult to load the Pd active component. Therefore, the preparation process of the catalyst in this invention is designed to first load the active component and then prepare the hydrophobic layer. At the same time, the content of the active component in the C4 hydrogenation catalyst is low, and excessive deposition of silica or polymer may cover the active center of the catalyst, leading to a significant decrease in catalyst activity. Therefore, in the preparation method of this invention: 1) Water is sprayed first, and due to the siphon effect of water, it enters and occupies the inner pores of the catalyst. The active component is mainly located in the shell layer near the outer surface, and the content of the active component in the internal structure of the catalyst is low. Therefore, the prepared hydrophobic layer is mainly located in the region where the active component is concentrated. The water in the inner pores will be removed during subsequent drying. 2) To prevent SiO2 from the decomposition of silicate esters from covering the active sites, after spraying water, a silane coupling agent solution is first uniformly sprayed onto the catalyst surface (the silane coupling agent reacts and connects with the exposed hydroxyl groups on the catalyst surface), followed by the spraying of silicate ester solution. The coupling agent fixes some SiO2 in areas without active components, while the SiO2 that does not react with the coupling agent is washed away, avoiding the loss of catalyst activity. The coverage on the catalyst surface and in the macropores is controlled by adjusting the amount of coupling agent used. 3) The coupling agent containing -CF3 reacts with the SiO2 already fixed on the alumina surface, grafting the -CF3-containing organic molecules onto the SiO2, giving both the shell region where the active components are distributed and the well-developed pore structure good hydrophobicity.

[0045] Another invention provides a hydrophobic supported palladium-silver catalyst, which is obtained by any of the above preparation methods.

[0046] The hydrophobic supported palladium-silver catalyst according to the present invention preferably comprises a support and nano-SiO2 and an organic molecule containing -CF3 supported on the support;

[0047] Based on the catalyst weight of 100%, the palladium content (in elemental form) is 0.2% to 0.5%, more preferably 0.23% to 0.45%; the silver content (in elemental form) is 0.05% to 0.5%, more preferably 0.1% to 0.5%; and the content of the organic molecule containing -CF3 is 1.5% to 5.5%, more preferably 1.5% to 5.0%. Specifically, the organic molecule containing -CF3 is a perfluoroalkyltriethoxysilane, preferably a perfluorooctyltriethoxysilane.

[0048] In the hydrophobic supported palladium-silver catalyst of the present invention, preferably, the particle size of the nano-SiO2 is 2-5 nm.

[0049] The hydrophobic supported palladium-silver catalyst according to the present invention preferably has a specific surface area of ​​60-150 m². 2 / g, more preferably 80-120m 2 / g; pore volume is 0.15-0.6 mL / g, more preferably 0.3-0.45 mL / g.

[0050] To ensure the formation of hydrophobic groups at the desired sites, this invention first grafts a silane coupling agent onto the catalyst surface and its well-developed porous structure. Then, a silicate ester solution is sprayed on; after hydrolysis, individual silicon oxide molecules are formed first, reacting with the remaining active groups of the silane coupling agent, thereby loading silicon oxide onto the catalyst in single-molecule form. Although this region is where the metal active component is concentrated, the silanization reaction only occurs in areas without active components, thus preventing the active component from being covered. After spraying a coupling agent containing -CF3 groups onto the catalyst, fluorine-containing organic molecules are grafted onto the surface of smaller SO2 particles, giving the catalyst excellent hydrophobic properties.

[0051] This invention has found that grafting organic molecules containing -CF3 onto the catalyst surface reduces the coking rate of the catalyst. This may be because the presence of -CF3 improves the hydrophobicity of the catalyst while also improving its oleophobicity, thus shortening the residence time of byproducts generated in the reaction on the catalyst surface and delaying the coking rate of the catalyst.

[0052] The catalyst of this invention can be used in the selective hydrogenation process of aqueous C4 fractions. It has good resistance to water interference and can operate stably for a long time when the water content reaches 400-500 μg / g. Moreover, the coking rate of the catalyst is reduced by more than 70%, and the catalyst operating cycle is significantly extended. Detailed Implementation

[0053] To more clearly illustrate the present invention, the following description, in conjunction with preferred embodiments, further clarifies the invention. Those skilled in the art should understand that the specific descriptions below are illustrative rather than restrictive, and should not be construed as limiting the scope of protection of the present invention.

[0054] All numerical specifications in this invention (e.g., temperature, time, concentration, and weight, including ranges for each) are generally approximate values ​​that can be changed (+) or (-) in increments of 0.1 or 1.0. All numerical specifications are to be understood as being preceded by the term "approximately". In the following examples:

[0055] The contents of Pd and Ag in the catalyst were determined using an atomic absorption spectrometer.

[0056] The organic content loaded on the catalyst was measured using TG.

[0057] IR determination of CF3 group content.

[0058] In the examples, the yield of monoene was calculated using the following formula:

[0059] 1-Butene yield (%) = Product 1-butene · 100 / Feed 1-butene Catalyst coking amount = Catalyst mass after operation - Catalyst mass before operation

[0060] Agilent gas chromatographs measure the composition of reactants and products.

[0061] Example 1

[0062] The preparation of catalyst S1 in this embodiment includes the following steps:

[0063] The catalyst support uses commercially available clover-shaped alumina-magnesium oxide carriers with a diameter of 2.0–2.5 mm, a water absorption rate of 65%, and a specific surface area of ​​97 m². 2 / g. Weigh 100g of the carrier.

[0064] (1) Palladium loading by supersaturation impregnation method: Palladium chloride was prepared into an active component impregnation solution, the pH was adjusted to 2.5, and the carrier was impregnated into the prepared palladium active component solution. After impregnation for 3 hours, it was dried at 100°C for 4 hours and calcined at 380°C for 8 hours to obtain the semi-finished catalyst A1.

[0065] (2) Silver loading by equal volume impregnation method: Silver nitrate was prepared into an active component impregnation solution, and A1 was impregnated into the prepared silver active component solution by equal volume impregnation method. The solution was dried at 110°C for 1 hour and calcined at 450°C for 6 hours to obtain semi-finished catalyst B1.

[0066] (3) Spray distilled water with a carrier water absorption rate of 88% evenly onto the semi-finished catalyst B1, let it stand for 30 minutes, and obtain the semi-finished catalyst C1.

[0067] (4) Trimethoxychlorosilane and cyclohexane are mixed evenly to form a coupling agent solution, wherein the mass content of trimethoxychlorosilane is 40%, and the amount of solution prepared is 15% of the water absorption rate of the support. The solution is sprayed onto the semi-finished catalyst C1, and left to stand for 10 hours. After washing, it is left to stand for 5 hours to obtain the semi-finished catalyst D1.

[0068] (5) Mix the measured methanol, methyl orthosilicate and water, and stir slowly at 25°C for 60 min to obtain a silicate solution. The mass ratio of methanol, methyl orthosilicate and water is 10:4.7:0.8. The amount of solution prepared is 18% of the water absorption rate of the carrier. Spray the solution onto the semi-finished catalyst D1 and let it stand for 2 h to obtain the semi-finished catalyst E1.

[0069] (6) Dissolve perfluorooctyltriethoxysilane in cyclohexane to form a solution, wherein the mass content of perfluorooctyltriethoxysilane is 70%, the amount of solution prepared is 13% of the water absorption rate of the support, spray it onto the semi-finished catalyst E1, let it stand for 30 hours, and dry it at 90°C for 5 hours to obtain catalyst S1.

[0070] Catalyst reduction:

[0071] Before use, place it in a fixed-bed reactor and reduce it for 6 hours at 110°C using a mixed gas with a molar ratio of N2:H2 = 1:2.

[0072] Example 2

[0073] The preparation of catalyst S2 in this embodiment includes the following steps:

[0074] The catalyst support uses commercially available spherical alumina support with a diameter of 3.0–3.5 mm, a water absorption rate of 64%, and a specific surface area of ​​92 m². 2 / g. Weigh 100g of the carrier.

[0075] (1) Palladium loading by supersaturation impregnation method: Palladium acetate was prepared into an active component impregnation solution, the pH was adjusted to 2.4, and the support was impregnated into the prepared palladium active component solution. After impregnation for 1 hour, it was dried at 110°C for 3 hours and calcined at 450°C for 4 hours to obtain the semi-finished catalyst A2.

[0076] (2) Silver loading by equal volume impregnation method: Silver nitrate was prepared into an active component impregnation solution, and A2 was impregnated into the prepared silver active component solution by equal volume impregnation method. The solution was dried at 100°C for 3 hours and calcined at 500°C for 4 hours to obtain semi-finished catalyst B2.

[0077] (3) Spray distilled water with a carrier water absorption rate of 85% evenly onto the semi-finished catalyst B2, let it stand for 25 minutes, and obtain the semi-finished catalyst C2.

[0078] (4) Trimethoxychlorosilane and cyclohexane are mixed evenly to form a coupling agent solution, wherein the mass content of trimethoxychlorosilane is 50% and the amount of solution prepared is 5.5% of the water absorption rate of the support. The solution is sprayed onto the semi-finished catalyst C2, and left to stand for 15 hours. After washing, it is left to stand for 10 hours to obtain the semi-finished catalyst D2.

[0079] (5) Mix the measured ethanol, ethyl orthosilicate and water, and stir slowly at 28°C for 35 min to obtain a silicate solution. The mass ratio of ethanol, ethyl orthosilicate and water is 10:3:0.9. The amount of solution prepared is 13% of the water absorption rate of the carrier. Spray the solution onto the semi-finished catalyst D2 and let it stand for 2.5 h to obtain the semi-finished catalyst E2.

[0080] (6) Dissolve perfluorooctyltriethoxysilane in n-hexane to form a solution, wherein the mass content of perfluorooctyltriethoxysilane is 50%, the amount of solution prepared is 6% of the water absorption rate of the support, spray it onto the semi-finished catalyst E2, let it stand for 20 hours, and dry it at 120°C for 3 hours to obtain catalyst S2.

[0081] Catalyst reduction:

[0082] Before use, place it in a fixed-bed reactor and reduce it for 8 hours at 100°C using a mixed gas with a molar ratio of N2:H2 = 1:2.

[0083] Example 3

[0084] The preparation of catalyst S3 in this embodiment includes the following steps:

[0085] The catalyst support uses commercially available clover-shaped alumina carriers with a diameter of 1.8–2.2 mm, a water absorption rate of 66%, and a specific surface area of ​​96 m². 2 / g. Weigh 100g of the carrier.

[0086] (1) Palladium loading by supersaturation impregnation method: Palladium chloride was prepared into an active component impregnation solution, the pH was adjusted to 2.3, and the support was impregnated into the prepared palladium active component solution. After impregnation for 0.5 h, it was dried at 90 °C for 6 h and calcined at 500 °C for 3 h to obtain semi-finished catalyst A3.

[0087] (2) Silver loading by equal volume impregnation method: Silver nitrate was prepared into an active component impregnation solution, and A3 was impregnated into the prepared silver active component solution by equal volume impregnation method. The solution was dried at 120°C for 1 hour and calcined at 480°C for 4 hours to obtain semi-finished catalyst B3.

[0088] (3) Spray distilled water with a carrier water absorption rate of 82% evenly onto the semi-finished catalyst B3, let it stand for 20 minutes, and obtain the semi-finished catalyst C3.

[0089] (4) Trimethoxychlorosilane and n-hexane are mixed evenly to form a coupling agent solution, wherein the mass content of trimethoxychlorosilane is 48% and the amount of solution prepared is 8% of the water absorption rate of the carrier. The solution is sprayed onto the semi-finished catalyst C3, and left to stand for 20 hours. After washing, it is left to stand for 6 hours to obtain the semi-finished catalyst D3.

[0090] (5) Mix the measured propanol, methyl orthosilicate, and water, and stir slowly at 35°C for 30 min to obtain a silicate solution. The mass ratio of propanol, methyl orthosilicate, and water is 10:3.5:0.6. The amount of solution prepared is 15% of the water absorption rate of the carrier. Spray the solution onto the semi-finished catalyst D3 and let it stand for 3 h to obtain the semi-finished catalyst E3.

[0091] (6) Dissolve perfluorooctyltriethoxysilane in n-hexane to form a solution, wherein the mass content of perfluorooctyltriethoxysilane is 58%, the amount of solution prepared is 9% of the water absorption rate of the support, spray it onto the semi-finished catalyst E3, let it stand for 15 hours, and dry it at 100°C for 2.5 hours to obtain catalyst S3.

[0092] Catalyst reduction:

[0093] Before use, place it in a fixed-bed reactor and reduce it under a hydrogen atmosphere at 80°C for 12 hours.

[0094] Example 4

[0095] The preparation of catalyst S4 in this embodiment includes the following steps:

[0096] The catalyst support uses commercially available spherical alumina support with a diameter of 3.0–3.5 mm, a water absorption rate of 68%, and a specific surface area of ​​10³ m². 2 / g. Weigh 100g of the carrier.

[0097] (1) Palladium loading by supersaturation impregnation method: Palladium chloride was prepared into an active component impregnation solution, the pH was adjusted to 2.2, and the support was impregnated into the prepared palladium active component solution. After impregnation for 1.5 h, it was dried at 80 °C for 6 h and calcined at 550 °C for 2 h to obtain the semi-finished catalyst A4.

[0098] (2) Silver loading by equal volume impregnation method: Silver nitrate was prepared into an active component impregnation solution, and A4 was impregnated into the prepared silver active component solution by equal volume impregnation method. The solution was dried at 90°C for 3 hours and calcined at 550°C for 3 hours to obtain semi-finished catalyst B4.

[0099] (3) Spray distilled water with a carrier water absorption rate of 78% evenly onto the semi-finished catalyst B4, let it stand for 15 minutes, and obtain the semi-finished catalyst C4.

[0100] (4) Triethoxychlorosilane and n-heptane are mixed evenly to form a coupling agent solution, wherein the mass content of triethoxychlorosilane is 42% and the amount of solution prepared is 10% of the water absorption rate of the carrier. The solution is sprayed onto the semi-finished catalyst C4, and left to stand for 12 hours. After washing, it is left to stand for 8 hours to obtain the semi-finished catalyst D4.

[0101] (5) Mix the measured ethanol, ethyl orthosilicate and water, and stir slowly at 32°C for 40 min to obtain a silicate solution. The mass ratio of ethanol, ethyl orthosilicate and water is 10:4:0.7. The amount of solution prepared is 16% of the water absorption rate of the carrier. Spray the solution onto the semi-finished catalyst D4 and let it stand for 3.5 h to obtain the semi-finished catalyst E4.

[0102] (6) Dissolve perfluorooctyltriethoxysilane in n-heptane to form a solution, wherein the mass content of perfluorooctyltriethoxysilane is 60%, the amount of solution prepared is 8% of the water absorption rate of the support, spray it onto the semi-finished catalyst E4, let it stand for 10 hours, and dry it at 150°C for 4 hours to obtain catalyst S4.

[0103] Catalyst reduction:

[0104] Before use, place it in a fixed-bed reactor and reduce it for 5 hours at 110°C using a mixed gas with a molar ratio of N2:H2 = 1:2.

[0105] Example 5

[0106] The preparation of catalyst S5 in this embodiment includes the following steps:

[0107] The catalyst support uses a commercially available five-toothed alumina support with a diameter of 3.0–3.5 mm, a water absorption rate of 67%, and a specific surface area of ​​98 m². 2 / g. Weigh 100g of the carrier.

[0108] (1) Palladium loading by supersaturation impregnation method: Palladium chloride was prepared into an active component impregnation solution, the pH was adjusted to 2, and the carrier was impregnated into the prepared palladium active component solution. After impregnation for 2 hours, it was dried at 120°C for 1 hour and calcined at 480°C for 6 hours to obtain the semi-finished catalyst A5.

[0109] (2) Silver loading by equal volume impregnation method: Silver nitrate was prepared into an active component impregnation solution, and A5 was impregnated into the prepared silver active component solution by equal volume impregnation method. The solution was dried at 80°C for 4 hours and calcined at 580°C for 2 hours to obtain semi-finished catalyst B5.

[0110] (3) Spray distilled water with a carrier water absorption rate of 80% evenly onto the semi-finished catalyst B5, let it stand for 20 minutes, and obtain the semi-finished catalyst C5.

[0111] (4) Triethoxychlorosilane and n-octane are mixed evenly to form a coupling agent solution, wherein the mass content of triethoxychlorosilane is 45% and the amount of solution prepared is 12% of the water absorption rate of the support. The solution is sprayed onto the semi-finished catalyst C5, and left to stand for 17 hours. After washing, it is left to stand for 7 hours to obtain the semi-finished catalyst D5.

[0112] (5) Mix the measured ethanol, ethyl orthosilicate and water, and stir slowly at 40°C for 45 min to obtain a silicate solution. The mass ratio of ethanol, ethyl orthosilicate and water is 10:4.5:0.5. The amount of solution prepared is 19% of the water absorption rate of the carrier. Spray the solution onto the semi-finished catalyst D5 and let it stand for 4 h to obtain the semi-finished catalyst E5.

[0113] (6) Dissolve perfluorooctyltriethoxysilane in n-octane to form a solution, wherein the mass content of perfluorooctyltriethoxysilane is 62%, the amount of solution prepared is 10% of the water absorption rate of the support, spray it onto the semi-finished catalyst E5, let it stand for 25 hours, and dry it at 110°C for 4.5 hours to obtain catalyst S5.

[0114] Catalyst reduction:

[0115] Before use, place it in a fixed-bed reactor and reduce it under a hydrogen atmosphere at 90°C for 10 hours.

[0116] Example 6

[0117] The preparation of catalyst S6 in this embodiment includes the following steps:

[0118] The catalyst support uses commercially available clover-shaped alumina carriers with a diameter of 1.8–2.2 mm, a water absorption rate of 70%, and a specific surface area of ​​112 m². 2 / g. Weigh 100g of the carrier.

[0119] (1) Palladium loading by supersaturation impregnation method: Palladium nitrate was prepared into an active component impregnation solution, the pH was adjusted to 2.1, and the support was impregnated into the prepared palladium active component solution. After impregnation for 2.5 h, it was dried at 100 °C for 2 h and calcined at 420 °C for 5 h to obtain the semi-finished catalyst A6.

[0120] (2) Silver loading by equal volume impregnation method: Silver nitrate was prepared into an active component impregnation solution, and A6 was impregnated into the prepared silver active component solution by equal volume impregnation method. The solution was dried at 100°C for 2 hours and calcined at 520°C for 5 hours to obtain semi-finished catalyst B6.

[0121] (3) Spray distilled water with a carrier water absorption rate of 75% evenly onto the semi-finished catalyst B6, let it stand for 10 minutes, and obtain the semi-finished catalyst C6.

[0122] (4) Trimethoxychlorosilane and n-heptane are mixed evenly to form a coupling agent solution, wherein the mass content of trimethoxychlorosilane is 47% and the amount of solution prepared is 14% of the water absorption rate of the support. The solution is sprayed onto the semi-finished catalyst C6, and left to stand for 13 hours. After washing, it is left to stand for 9 hours to obtain the semi-finished catalyst D6.

[0123] (5) Mix the measured ethanol, methyl orthosilicate and water, and stir slowly at 30°C for 50 min to obtain a silicate solution. The mass ratio of ethanol, methyl orthosilicate and water is 10:5:1. The amount of solution prepared is 20% of the water absorption rate of the carrier. Spray the solution onto the semi-finished catalyst D6 and let it stand for 3 h to obtain the semi-finished catalyst E6.

[0124] (6) Dissolve perfluorooctyltriethoxysilane in n-heptane to form a solution, wherein the mass content of perfluorooctyltriethoxysilane is 65%, the amount of solution prepared is 15% of the water absorption rate of the support, spray it onto the semi-finished catalyst E6, let it stand for 20 hours, and dry it at 130°C for 2 hours to obtain catalyst S6.

[0125] Catalyst reduction:

[0126] Before use, place it in a fixed-bed reactor and reduce it for 8 hours at 110°C using a mixed gas with a molar ratio of N2:H2 = 1:3.

[0127] Comparative Example 1

[0128] Catalyst Z1 was prepared in this comparative example using the same support as in Example 2, and the catalyst preparation conditions were the same as in Example 2, except that the silicate solution was not sprayed.

[0129] The catalyst support uses commercially available spherical alumina support with a diameter of 3.0–3.5 mm, a water absorption rate of 64%, and a specific surface area of ​​92 m². 2 / g. Weigh 100g of the carrier.

[0130] (1) Palladium loading by supersaturation impregnation method: Palladium acetate was prepared into an active component impregnation solution, the pH was adjusted to 2.4, and the support was impregnated into the prepared palladium active component solution. After impregnation for 1 hour, it was dried at 110°C for 3 hours and calcined at 450°C for 4 hours to obtain the semi-finished catalyst F1.

[0131] (2) Silver loading by equal volume impregnation method: Silver nitrate was prepared into an active component impregnation solution, and F1 was impregnated into the prepared silver active component solution by equal volume impregnation method. The solution was dried at 100°C for 3 hours and calcined at 500°C for 4 hours to obtain semi-finished catalyst G1.

[0132] (3) Spray distilled water with a carrier water absorption rate of 85% evenly onto the semi-finished catalyst G1, let it stand for 25 minutes, and obtain the semi-finished catalyst H1.

[0133] (4) Trimethoxychlorosilane and cyclohexane are mixed evenly to form a coupling agent solution, wherein the mass content of trimethoxychlorosilane is 50% and the amount of solution prepared is 5.5% of the water absorption rate of the support. The solution is sprayed onto the semi-finished catalyst H1, and left to stand for 15 hours. After washing, it is left to stand for 10 hours to obtain the semi-finished catalyst K1.

[0134] (5) Dissolve perfluorooctyltriethoxysilane in n-hexane to form a solution, wherein the mass content of perfluorooctyltriethoxysilane is 50%, the amount of solution prepared is 6% of the water absorption rate of the support, spray it onto the semi-finished catalyst K1, let it stand for 20 hours, and dry it at 120°C for 3 hours to obtain catalyst Z1.

[0135] Catalyst reduction:

[0136] Before use, place it in a fixed-bed reactor and reduce it for 8 hours at 100°C using a mixed gas with a molar ratio of N2:H2 = 1:2.

[0137] Comparative Example 2

[0138] The catalyst Z2 in this comparative example was prepared using the same support as in Example 3, except that it was prepared using a conventional method.

[0139] The catalyst support uses commercially available clover-shaped alumina carriers with a diameter of 1.8–2.2 mm, a water absorption rate of 66%, and a specific surface area of ​​96 m². 2 / g. Weigh 100g of the carrier.

[0140] (1) Palladium loading by supersaturation impregnation method: Palladium chloride was prepared into an active component impregnation solution, the pH was adjusted to 2.3, and the support was impregnated into the prepared palladium active component solution. After impregnation for 0.5 h, it was dried at 90 °C for 6 h and calcined at 500 °C for 3 h to obtain the semi-finished catalyst F2.

[0141] (2) Silver loading by equal volume impregnation method: Silver nitrate was prepared into an active component impregnation solution, and F2 was impregnated into the prepared silver active component solution by equal volume impregnation method. The solution was dried at 120°C for 1 hour and calcined at 480°C for 4 hours to obtain catalyst Z2.

[0142] Catalyst reduction:

[0143] Before use, place it in a fixed-bed reactor and reduce it under a hydrogen atmosphere at 80°C for 12 hours.

[0144] Comparative Example 3

[0145] Catalyst Z3 was prepared in this comparative example using the same support as in Example 5, but with the following differences: no coupling agent was added, so SiO2 could not be effectively grafted onto the alumina surface and was easily detached during washing; without sufficient SiO2, the supported organic molecules would be lost during washing. The outer layer of the catalyst had poor hydrophobicity.

[0146] The catalyst support uses a commercially available five-toothed alumina support with a diameter of 3.0–3.5 mm, a water absorption rate of 67%, and a specific surface area of ​​98 m². 2 / g. Weigh 100g of the carrier.

[0147] (1) Palladium loading by supersaturation impregnation method: Palladium chloride was prepared into an active component impregnation solution, the pH was adjusted to 2, and the carrier was impregnated into the prepared palladium active component solution. After impregnation for 2 hours, it was dried at 120°C for 1 hour and calcined at 480°C for 6 hours to obtain the semi-finished catalyst F3.

[0148] (2) Silver was loaded using the equal volume impregnation method: Silver nitrate was prepared into an active component impregnation solution, and F3 was impregnated into the prepared silver active component solution using the equal volume impregnation method. The solution was dried at 80°C for 4 hours and calcined at 580°C for 2 hours to obtain the semi-finished catalyst G3.

[0149] (3) Spray distilled water with a carrier water absorption rate of 80% evenly onto the semi-finished catalyst G3, let it stand for 20 minutes, and obtain the semi-finished catalyst H3.

[0150] (4) Mix the measured ethanol, ethyl orthosilicate and water, and stir slowly at 40°C for 45 min to obtain a silicate solution. The mass ratio of ethanol, ethyl orthosilicate and water is 10:4.5:0.5. The amount of solution prepared is 19% of the water absorption rate of the carrier. Spray the solution onto the semi-finished catalyst H3 and let it stand for 4 h to obtain the semi-finished catalyst K3.

[0151] (5) Dissolve perfluorooctyltriethoxysilane in n-octane to form a solution, wherein the mass content of perfluorooctyltriethoxysilane is 62%, the amount of solution prepared is 10% of the water absorption rate of the support, spray it onto the semi-finished catalyst K3, let it stand for 25 hours, and dry it at 110°C for 4.5 hours to obtain catalyst Z3.

[0152] Catalyst reduction:

[0153] Before use, place it in a fixed-bed reactor and reduce it under a hydrogen atmosphere at 90°C for 10 hours.

[0154] Comparative Example 4

[0155] Catalyst Z3 was prepared in this comparative example using the same support as in Example 6, except that it did not support organic molecules containing -CF3, resulting in poor hydrophobicity of the outer layer of the catalyst.

[0156] The catalyst support uses commercially available clover-shaped alumina carriers with a diameter of 1.8–2.2 mm, a water absorption rate of 70%, and a specific surface area of ​​112 m². 2 / g. Weigh 100g of the carrier.

[0157] (1) Palladium loading by supersaturation impregnation method: Palladium chloride was prepared into an active component impregnation solution, the pH was adjusted to 2.1, and the support was impregnated into the prepared palladium active component solution. After impregnation for 2.5 h, it was dried at 100 °C for 2 h and calcined at 420 °C for 5 h to obtain the semi-finished catalyst F4.

[0158] (2) Silver loading by equal volume impregnation method: Silver nitrate was prepared into an active component impregnation solution, and F4 was impregnated into the prepared silver active component solution by equal volume impregnation method. The solution was dried at 100°C for 2 hours and calcined at 520°C for 5 hours to obtain semi-finished catalyst G4.

[0159] (3) Spray distilled water with a carrier water absorption rate of 75% evenly onto the semi-finished catalyst G4, let it stand for 10 minutes, and obtain the semi-finished catalyst H4.

[0160] (4) Trimethoxychlorosilane and n-heptane are mixed evenly to form a coupling agent solution, wherein the mass content of trimethoxychlorosilane is 47% and the amount of solution prepared is 14% of the water absorption rate of the carrier. The solution is sprayed onto the semi-finished catalyst H4, and left to stand for 13 hours. After washing, it is left to stand for 9 hours to obtain the semi-finished catalyst K4.

[0161] (5) Mix the measured ethanol, methyl orthosilicate and water, and stir slowly at 30°C for 50 min to obtain a silicate solution. The mass ratio of ethanol, methyl orthosilicate and water is 10:5:1. The amount of solution prepared is 20% of the water absorption rate of the carrier. Spray the solution onto the semi-finished catalyst K4 and let it stand for 3 h to obtain the semi-finished catalyst Z4.

[0162] Catalyst reduction:

[0163] Before use, place it in a fixed-bed reactor and reduce it for 8 hours at 110°C using a mixed gas with a molar ratio of N2:H2 = 1:3.

[0164] The content of each component in the catalysts obtained in Examples 1-6 above is shown in Table 1.

[0165] Table 1. Content of each component in the catalyst of the examples (based on catalyst mass of 100%)

[0166]

[0167] The catalyst is used in the selective hydrogenation of C4 fractions to recover 1-butene.

[0168] The catalyst was loaded at a rate of 50 mL in a fixed-bed single-stage reactor, and the mass hourly space velocity (WHSV) of the fresh reactant was 1 h⁻¹. -1 The reaction used FCC C4 (composition shown in Table 2) as the feedstock, with a water content of 417 μg / g. The reaction conditions were: operating pressure 1.0 MPa, hydrogen to butadiene molar ratio in the feedstock 6, and reactor inlet temperature 41 °C. The catalytic results are shown in Table 3.

[0169] Table 2. Composition of FCC C4 materials

[0170] project Isobutane n-Butane transbutene n-Butene Isobutylene maleic butene 1,3-Butadiene mass fraction / % 60.33 7.41 7.32 15.32 7.02 2.14 0.14

[0171] Table 3 Catalyst Evaluation Results

[0172]

[0173] As can be seen from the comparison of catalyst evaluation results in Table 3:

[0174] Data analysis from the examples and comparative examples shows that when the catalyst of the present invention is used for the selective hydrogenation of C4 fraction to recover 1-butene, under the same process conditions, the catalyst of the present invention exhibits superior anti-coking performance, while maintaining a high level of catalyst activity and selectivity.

[0175] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the implementation of the present invention. For those skilled in the art, other variations or modifications can be made based on the above description. It is impossible to exhaustively list all the implementation methods here. All obvious variations or modifications derived from the technical solutions of the present invention are still within the protection scope of the present invention.

Claims

1. A process for the preparation of a hydrophobic supported palladium-silver catalyst, wherein, The preparation method includes the following steps: The active components are loaded onto the support using an impregnation method to obtain a semi-finished catalyst B; the active components include palladium and silver. Water is sprayed evenly onto the semi-finished catalyst B, and left to stand for a first preset time to obtain the semi-finished catalyst C. The silane coupling agent solution is sprayed onto the semi-finished catalyst C, left to stand for a second preset time, washed, and then left to stand for a third preset time to obtain the semi-finished catalyst D. A silicate solution is sprayed onto the semi-finished catalyst D and left to stand for a fourth preset time to obtain the semi-finished catalyst E. A solution of perfluoroalkyltriethoxysilane was sprayed onto the semi-finished catalyst E, allowed to stand for a fifth preset time, and then dried to obtain the hydrophobic supported palladium-silver catalyst.

2. The preparation method according to claim 1, wherein, The preparation process of the semi-finished catalyst B includes: The support was impregnated in a Pd precursor salt solution, the pH of the solution was adjusted to 1.8-2.5, and a supersaturated impregnation method was used. After impregnation, the solution was dried and calcined to obtain a semi-finished catalyst A. Semi-finished catalyst A was impregnated in a precursor salt solution of Ag using an equal-volume impregnation method. After impregnation, the catalyst was dried and calcined to obtain semi-finished catalyst B.

3. The preparation method according to claim 2, wherein, The carrier is immersed in the precursor salt solution of Pd for 0.5 to 3 hours; then dried at 80 to 120°C for 1 to 6 hours, and calcined at 350 to 550°C for 2 to 8 hours.

4. The preparation method according to claim 2, wherein, After the semi-finished catalyst A is impregnated in the precursor salt solution of Ag, it is dried at 80-120°C for 1-4 hours and calcined at 400-600°C for 2-6 hours.

5. The preparation method according to claim 2, wherein, The precursor salt of Pd is selected from at least one of palladium nitrate, palladium acetate, and palladium chloride.

6. The preparation method according to claim 2, wherein, The precursor salt of Ag is silver nitrate.

7. The preparation method according to claim 1 or 2, wherein, The carrier is an alumina carrier or a mixed carrier with an alumina mass fraction of more than 80%; the other metal oxides in the mixed carrier are magnesium oxide and / or silicon oxide.

8. The preparation method according to claim 1, wherein, The first preset time is 10 to 30 minutes. The second preset time is 10-20 hours. The third preset time is 5 to 10 hours. The fourth preset time is 2 to 4 hours.

9. The preparation method according to claim 1, wherein, The spray volume of water is 75% to 90% of the carrier's water absorption rate.

10. The preparation method according to claim 1, wherein, The silane coupling agent is triethoxychlorosilane or trimethoxychlorosilane.

11. The preparation method according to claim 1, wherein, In the solution of the silane coupling agent, the solvent is a C6-C8 alkane, and the mass content of the coupling agent is 40%-50%.

12. The preparation method according to claim 1, wherein, The spray volume of the silane coupling agent solution is 5% to 15% of the water absorption rate of the carrier.

13. The preparation method according to claim 1, wherein, The silicate ester is methyl orthosilicate or ethyl orthosilicate.

14. The preparation method according to claim 1, wherein, In the silicate ester solution, the solvent is a lower alcohol and water; the lower alcohol is selected from at least one of methanol, ethanol, propanol, and butanol. The mass ratio of the lower alcohol, silicate ester and water is 10:(3-5):(0.5-1).

15. The preparation method according to claim 1, wherein, The spray volume of the silicate solution is 10% to 20% of the water absorption rate of the carrier.

16. The preparation method according to claim 1, wherein, The perfluoroalkyltriethoxysilane is perfluorooctyltriethoxysilane.

17. The preparation method according to claim 1, wherein, In the solution of the perfluoroalkyltriethoxysilane, the solvent is a C6-C8 alkane, and the mass content of the perfluoroalkyltriethoxysilane is 50%-70%. The spray volume of the perfluoroalkyltriethoxysilane solution is 5% to 15% of the water absorption rate of the carrier.

18. A hydrophobic supported palladium-silver catalyst, obtained by the preparation method according to any one of claims 1-17.

19. The hydrophobic supported palladium-silver catalyst according to claim 18, wherein, The hydrophobic supported palladium-silver catalyst includes a support and nano-SiO2 and an organic molecule containing -CF3 supported on the support; The catalyst contains 0.2% to 0.5% palladium (in elemental form) and 0.05% to 0.5% silver (in elemental form) by weight of 100%, and the organic molecule containing -CF3 contains 1.5% to 5.5%.

20. The hydrophobic supported palladium-silver catalyst according to claim 19, wherein, The particle size of the nano-SiO2 is 2-5 nm; The specific surface area of the hydrophobic supported palladium-silver catalyst is 60-150 m 2 / g, and the pore volume is 0.15-0.6 mL / g.

Citation Information

Patent Citations

  • Preparation method of hydrophobic silica nano sphere-supported palladium-based catalyst

    CN106732771A

  • Surface modification method of aluminum oxide for super-hydrophobic high-fluidity heat-conducting silicone grease

    CN113354872A