A sulfur-vanadium-nitrate triple-effect FCC additive prepared by co-precipitation-spray granulation method
The sulfur-vanadium-nitrate triple-effect FCC additive prepared by co-precipitation-spray granulation method solves the problems of single function and complex process in the existing technology, realizes efficient removal of sulfur oxides and nitrogen oxides in catalytic cracking flue gas, effectively captures vanadium, and improves the performance of the catalyst.
Patent Information
- Application Number
- CN202611279707.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-21
- Publication Date
- 2026-11-17
AI Technical Summary
Existing FCC flue gas treatment additives have limited functions, complex processes, and insufficient vanadium resistance, making it difficult to simultaneously and efficiently remove sulfur oxides and nitrogen oxides while capturing vanadium.
A sulfur-vanadium-nitrate triple-effect FCC additive was prepared by co-precipitation-spray granulation. The magnesium oxide-aluminum oxide-cerium oxide sulfur transfer active phase, titanium oxide-calcium oxide vanadium-resistant phase, and vanadium oxide denitrification active phase were uniformly distributed in a single microsphere through a six-component synergistic co-precipitation system. Combined with a stepwise pH-controlled co-precipitation process and calcination treatment, the synergistic effect of each functional phase was achieved.
This invention enables a single additive to simultaneously perform sulfur transfer, denitrification, and vanadium capture resistance, simplifying the process, reducing usage costs, and improving catalyst lifespan and product distribution quality.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to a sulfur-vanadium-nitrate triple-effect FCC additive prepared by co-precipitation-spray granulation, and more particularly to a multi-effect additive that can simultaneously remove sulfur oxides and nitrogen oxides from catalytic cracking regenerated flue gas and improve the vanadium resistance of the main catalyst, and its preparation method. Background Technology
[0002] In crude oil processing, catalytic cracking is currently the most important secondary processing technology used in Chinese refineries. While producing large quantities of high-quality light oil products, it also emits a certain amount of sulfur oxides (SOx) and nitrogen oxides (NOx) in its regeneration flue gas, causing environmental pollution and corrosion to the equipment. It is estimated that SOx and NOx emissions from FCC regeneration flue gas account for approximately 6%-7% and 10% of total SOx and NOx emissions into the atmosphere, respectively.
[0003] In recent years, the gasoline and diesel market has been sluggish. In order to reduce costs, refineries have purchased cheap heavy oil. This type of oil has a high content of vanadium, sulfur and nitrogen. Vanadium will seriously damage the catalyst, resulting in increased catalyst usage, poor product distribution, and sulfur and nitrogen further increasing the difficulty of processing.
[0004] Methods to reduce SOx and NOx emissions from FCC regenerators include: 1. Feedstock hydrotreating; 2. Wet flue gas scrubbing; 3. Selective catalytic reduction (SCR); 4. Selective non-catalytic reduction (SNCR); 5. Low-temperature ozone oxidation (LoTOx); and 6. Additive technology. Since additive technology requires almost no equipment investment and has low operating costs, using additives to reduce SOx and NOx emissions from catalytic cracking flue gas has become the best choice for refineries.
[0005] For refineries, they do not want to increase the amount of catalyst used. In addition, even if they add additives, they want to minimize the variety and amount of additives used. Therefore, multifunctional and efficient composite additives have become the first choice.
[0006] CN111420687A discloses a dual-functional additive for reducing NOx and transferring sulfur in FCC regenerated flue gas, and its preparation method. This additive uses a MgF2-modified catalytic cracking equilibrium agent as a carrier, and loads Pb, Sr, and a Group VIII metal using an in-situ isobaric impregnation method. When applied to an FCC industrial simulation unit, it can remove over 85% of NOx and over 75% of SOx. This additive recycles waste catalytic cracking equilibrium agent, has a simple production process, is convenient to use, and offers significant economic benefits.
[0007] CN110787834A discloses a desulfurization and denitrification aid for catalytic cracking flue gas and its preparation method, comprising 50-90 parts of carrier, 10-30 parts of matrix, 1-15 parts of active component, 2-10 parts of binder, and 0-10 parts of active additive; the active component includes a metallic active component and a non-metallic active component, with a weight ratio of metallic active component to non-metallic active component of 1:1-5:1; the method includes the following steps: impregnation, pulping, spray drying, and calcination.
[0008] CN106345488A discloses a copper-manganese-cerium composite oxide FCC regenerated flue gas combustion-supporting and denitrification aid and its preparation method. This combustion-supporting and denitrification aid uses alumina as a carrier and a symbiotic copper-manganese-cerium composite oxide as the active component, with the active component loaded onto the carrier. This invention not only has the dual functions of supporting CO combustion and reducing NOx emissions, but also features a simple, easy-to-implement, and low-cost preparation method.
[0009] CN102962061A discloses a multifunctional catalyst for removing NOx and SOx from catalytic cracking regenerated flue gas and its preparation method. The catalyst is prepared by impregnating alumina microspheres with rare earth-type desulfurization impregnation solution A, rare earth-type denitrification impregnation solution B, and precious metal salt impregnation solution C, followed by drying and calcination. When added to the device at a dosage of 0.5%, the catalyst achieves a NOx removal rate of over 70% and a SOx removal rate of over 40% in the regenerated flue gas, while also exhibiting good CO combustion-supporting effects and increasing propylene yield by over 2.0%.
[0010] CN1480246 discloses a three-effect agent comprising an adsorbent, cerium dioxide and vanadium pentoxide as oxidation catalysts, and cerium fluoride as a structural aid. The oxidation catalyst and structural aid are dispersed in the adsorbent, which has the general formula MgAl2-xFe. x O4· y The MgO spinel-like composite oxide has x in the formula being 0.01–0.5 and y being 0.2–1.2. The rare-earth cerium-containing compound in the three-effect agent uses bastnaesite powder as its raw material. This invention's three-effect agent is used for the efficient adsorption and desorption of sulfur oxides, the combustion enhancement of carbon monoxide, and the reduction of nitrogen oxides in the regenerated flue gas of petroleum refining catalytic cracking. Furthermore, the preparation method of the three-effect agent has a low cost.
[0011] CN104759202A discloses an additive for removing pollutants from catalytic cracking regeneration flue gas and its preparation method. The method involves modifying magnesium aluminum spinel, hydrotalcite-like material, and boehmite with rare earth elements, adding a binder to form a high-solids-content slurry, spray-molding, drying, and calcining to obtain an additive carrier with high hydrothermal stability. Then, a precious metal is impregnated using an equal-volume impregnation method, followed by a second calcination to obtain the final product. The additive of this invention exhibits good hydrothermal stability, good sustained activity and long lifespan; it does not contain vanadium, iron, or other components harmful to catalytic cracking catalysts; and the resulting additive for removing pollutants from catalytic cracking regeneration flue gas has superior performance.
[0012] CN119499846A discloses a denitrification, combustion-promoting, and acid-mist-removing additive. The method involves reacting a precisely proportioned mixture of ferric chloride, magnesium chloride, aluminum chloride, and sodium hydroxide aqueous solution to generate a crosslinking agent solution. This solution is then mixed with modified magnesium saponite and subjected to a heating and holding process to form a crosslinked structure. Subsequently, the crosslinked magnesium saponite is impregnated in a solution containing multiple metal salts and calcined to obtain the final additive. The modified magnesium saponite is prepared using polyethylene glycol ether and sodium aluminosilicate, optimizing the pore structure and thermal stability. Compared with existing technologies, the additive of this invention effectively reduces SOx and NOx emissions, especially sulfur trioxide emissions, during catalytic cracking, improves combustion efficiency, reduces pollutant generation, and avoids the use of toxic substances, thus reducing environmental pollution and demonstrating significant environmental and economic benefits.
[0013] CN119972064A discloses a three-effect additive for desulfurization, denitrification, and combustion improvement, its preparation method, and its application. The three-effect additive comprises: 30%-60% magnesium oxide, 20%-50% aluminum oxide, 8%-15% cerium oxide, 2%-5% vanadium pentoxide, 2%-10% modified metal components (calculated as oxides), and 0.01%-0.1% noble metal elements (calculated as elemental). The magnesium oxide is provided by a first magnesium source and a magnesium-aluminum matrix material, and the aluminum oxide is provided by a first aluminum source and a magnesium-aluminum matrix material. The mass of the magnesium-aluminum matrix material is 5%-30% of the total mass of the raw materials of the three-effect additive. The magnesium-aluminum matrix material is obtained by crystallizing a mixture of a second aluminum source and a second magnesium source after sol-gel treatment, and the magnesium-aluminum matrix material comprises magnesium oxide and aluminum oxide in a mass ratio of 0.2-0.8:1.
[0014] Catalytic cracking units mostly use flue gas sulfur transfer aids, denitrification agents, and CO combustion aids. Many units use two or even three of these functional aids simultaneously. Because these aids have limited functions and complicated addition processes, the use of certain functional aids is restricted when emissions meet standards, resulting in resource waste and environmental pollution. Summary of the Invention
[0015] The technical problem to be solved by this invention is to address the shortcomings of existing FCC flue gas treatment additives, such as single function, complex process, and insufficient vanadium resistance. This invention provides a sulfur-vanadium-nitrate triple-effect FCC additive prepared by co-precipitation-spray granulation and its preparation method. This additive integrates three functions, namely sulfur transfer, denitrification and vanadium capture resistance, in a single microsphere. The functional phases are uniformly distributed, the preparation process is simple, and it can effectively capture vanadium on the balancer, thereby improving the distribution of catalytic cracking products.
[0016] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows:
[0017] A three-way FCC additive, the chemical composition of which, based on oxides, comprises:
[0018] Magnesium oxide 15-30wt%, aluminum oxide 25-45wt%, cerium oxide 5-12wt%, titanium oxide 8-20wt%, vanadium oxide 2-7wt%, calcium oxide 3-10wt%.
[0019] Among them, magnesium oxide, aluminum oxide and cerium oxide together constitute the sulfur transfer active phase, titanium oxide and calcium oxide together constitute the vanadium-resistant phase, and vanadium oxide constitutes the denitrification active phase. Each phase is uniformly distributed in the microspheres.
[0020] The unique feature of this invention is:
[0021] (1) Design of a six-component synergistic coprecipitation system and functional phases: This invention is the first to integrate a magnesium oxide-aluminum oxide-cerium oxide sulfur transfer active phase, a titanium oxide-calcium oxide vanadium-resistant phase, and a vanadium oxide denitrification active phase into a single coprecipitation system. Unlike the stepwise loading mode of "carrier + impregnated active components" used in the prior art, this invention achieves uniform mixing of six metal oxides at the molecular / atomic level through one-step coprecipitation, avoiding the problems of uneven distribution of active components and limited loading in the impregnation method. In particular, this invention organically integrates the vanadium-resistant phase (calcium titanate phase), sulfur transfer phase (magnesium aluminum cerium phase), and denitrification phase (vanadium oxide phase), achieving the dual goals of "aiding pollution control and aiding vanadium capture".
[0022] (2) Stepwise pH-controlled coprecipitation process: In this invention, a stepwise alkali addition strategy of "one-third-pause-two-thirds-pause-final pH" is adopted in the coprecipitation process. In this stepwise coprecipitation process, trivalent aluminum ions preferentially precipitate in the pH range of 5.0-6.0, followed by magnesium and cerium ions in the pH range of 7.0-8.0, and finally titanium and calcium ions in the pH range of 8.5-10.0. This ensures the orderly formation of magnesium-aluminum-cerium solid solution and avoids the calcium titanate phase being encapsulated and unable to expose active sites. It allows different metal ions to precipitate in an orderly manner according to the difference in solubility product, avoiding component segregation caused by local supersaturation and ensuring the uniform coexistence of various oxide phases in the final product. This process is different from the conventional one-time alkali addition coprecipitation method and can effectively control the synergistic formation of magnesium-aluminum-cerium solid solution and calcium titanate crystal phase.
[0023] (3) Existing vanadium-containing FCC additives all use a post-impregnation method to load vanadium onto the surface of the oxide support. The vanadium species are unevenly dispersed and easily accumulate locally, leading to poisoning of the main catalyst. In this application, the vanadium species are not doped into the magnesium aluminum spinel lattice, but are dispersed as an independent active phase at the interface of each oxide phase. At the same time, they achieve functional coupling with the calcium titanate anti-vanadium phase, which is fundamentally different from the existing spinel doped vanadium technical solution.
[0024] Furthermore, the magnesium oxide, aluminum oxide, and cerium oxide are derived from the co-precipitation products of magnesium salts, aluminum salts, and cerium salts, which form a magnesium-aluminum-cerium composite oxide solid solution in the additive. This magnesium-aluminum-cerium composite oxide solid solution possesses excellent alkaline surface properties and oxygen storage capacity, enabling it to efficiently capture SO2 in the regenerator and convert it into sulfate. Under a reducing atmosphere, it releases SO2 to achieve sulfur transfer.
[0025] Furthermore, the titanium dioxide and calcium oxide are derived from the co-precipitation products of titanium and calcium salts, forming a calcium titanate crystalline phase during the calcination of the additives. The calcium titanate crystalline phase is structurally stable at high temperatures, and its perovskite lattice exhibits selective adsorption capacity for vanadium species, making it a key structure for achieving vanadium trapping resistance.
[0026] Furthermore, the vanadium oxide is derived from metavanadate, which is highly dispersed at the interfaces of various oxide phases in the additive. During the co-precipitation process, metavanadate can be uniformly embedded in other metal hydroxide precipitates, and after calcination, it forms highly dispersed V2O5 or magnesium vanadate / aluminum vanadate species, which are distributed at the interfaces of various phases. This is beneficial to the NOx catalytic reduction reaction and avoids catalyst poisoning due to local enrichment.
[0027] Furthermore, the particle size distribution of the additive microspheres is 40-150 micrometers, and the bulk density is 0.7-0.9 g / ml, which meets the requirements of the FCC device for additive particle size and fluidization performance.
[0028] This invention also provides a method for preparing the above-mentioned triple-effect FCC adjuvant, comprising the following steps:
[0029] (1) Prepare a mixed acidic solution containing magnesium salt, aluminum salt, cerium salt, titanium salt, calcium salt and vanadium salt;
[0030] (2) The mixed acidic solution and alkaline precipitant are added to the reactor in parallel under high-speed stirring. When one-third and two-thirds of the alkaline precipitant are added, the reaction is stopped for 5-10 minutes. The final pH value is controlled to 8.5-10.0 to carry out the coprecipitation reaction and obtain a coprecipitation slurry containing various metal hydroxides and / or oxides.
[0031] (3) After aging, filtering and washing, the co-precipitated slurry is re-watered and pulped, and silica sol accounting for 3-10 wt% of the slurry solid content and a certain proportion of hydrochloric acid are added and stirred evenly.
[0032] (4) Spray dry the slurry obtained in step (3) with an inlet air temperature of 300-400℃ and an outlet air temperature of 110-160℃ to obtain microspheres;
[0033] (5) The microspheres are calcined at 500-650℃ for 1-2 hours to obtain the triple-effect FCC additive.
[0034] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0035] (1) The additive of the present invention integrates the three functions of sulfur transfer, denitrification and anti-vanadium capture. A single additive can replace multiple functional additives, simplifying the addition process, reducing the cost of use and reducing resource waste.
[0036] (2) The co-precipitation method makes each active component uniformly distributed at the molecular level, and the synergistic effect of each functional phase is significantly better than that of the additives prepared by the impregnation method, and the utilization rate of active components is high.
[0037] (3) The calcium titanate anti-vanadium capturing phase in the additive can effectively capture vanadium species from the balancer, thereby reducing the vanadium content on the main catalyst, thus improving the distribution of catalytic cracking products, reducing the yield of oil slurry and coke, and extending the service life of the catalyst.
[0038] (4) Vanadium oxide is both an active component and can be captured and utilized by the additive itself, forming a "vanadium capture-denitrification" synergy, while avoiding the poisoning of the main catalyst by vanadium.
[0039] (5) The preparation process is simple and does not require cumbersome steps such as impregnation and multiple roasting, making it suitable for large-scale industrial production. Detailed Implementation
[0040] The present invention will be further illustrated below with specific embodiments and comparative examples, but the present invention is not limited to these embodiments.
[0041] Raw material description
[0042] Magnesium sulfate (MgSO4·7H2O, analytical grade)
[0043] Aluminum sulfate (Al2(SO4)3·18H2O, analytical grade)
[0044] Cerium nitrate (Ce(NO3)3·6H2O, analytical grade)
[0045] Titanium oxysulfate (TiOSO4, analytical grade)
[0046] Calcium chloride (CaCl2·2H2O, analytical grade)
[0047] Ammonium metavanadate (NH4VO3, analytical grade)
[0048] Silica sol (SiO2 content 30wt%, analytical grade)
[0049] Ammonia (25 wt%, analytical grade) was used as an alkaline precipitant.
[0050] Hydrochloric acid (36 wt%, analytical grade)
[0051] Balancer and Oil Instructions
[0052] Balancer: Industrial FCC balancer catalyst, mainly composed of Y-type molecular sieve (33wt%), kaolin matrix (39wt%), and binder (28wt%), with vanadium content of 7500μg / g.
[0053] Oil products: vacuum residue + wax oil, properties are shown in Table 1.
[0054] Table 1 Evaluation of oil properties
[0055]
[0056] Methods for evaluating the performance of additives:
[0057] Evaluation was conducted using a small riser evaluation device at a reaction temperature of 515℃, a reagent-to-oil ratio of 6, a reaction time of 3.5 seconds, and a regeneration temperature of 710℃. SOx (as SO2) and NOx (as NO) concentrations in the regenerated flue gas were measured using an online flue gas analyzer. The products were distilled and split into dry gas (C1-C2), liquefied petroleum gas (C3-C4), gasoline, diesel (200-350℃), oil slurry (>350℃), and raw coke, with yields (wt%, dry basis) calculated for each.
[0058] Example 1
[0059] Preparation steps: (1) Dissolve 126.5g magnesium sulfate, 333.8g aluminum sulfate, 86.8g cerium nitrate, 101.9g titanium oxysulfate, 44.4g calcium chloride, and 9.2g ammonium metavanadate in 2L of deionized water, add dilute hydrochloric acid to adjust the pH to 1.5-2.0, and prepare a mixed acidic solution; (2) Pump the mixed acidic solution into the reactor, turn on the high-speed stirring (800r / min), and add 25wt% ammonia water in parallel at a flow rate of 300mL / min. Stop adding alkali when 1 / 3 of the total amount of ammonia water has been added, and stir for 5 minutes; continue adding until 2 / 3 is added, and stop stirring for 8 minutes; finally adjust the pH to 9.0, continue stirring for 30 minutes, and obtain a coprecipitated slurry; (3) Age the slurry at 60℃ for 4 hours, filter, and wash with deionized water. Add water to the filter cake and slurry it to a solid content of 35wt%. Add silica sol (accounting for 6wt% of solid content) and hydrochloric acid to adjust the pH to 3.5-4.0 and stir evenly. (4) Spray drying: inlet air temperature 350℃, outlet air temperature 130℃, atomization pressure 2.5MPa. (5) Calcine the obtained microspheres at 600℃ for 1.5 hours to obtain the additive of Example 1.
[0060] Example 1: Properties of the adjuvant:
[0061]
[0062] Example 2
[0063] Preparation steps: (1) Dissolve 95.2g magnesium sulfate, 401.2g aluminum sulfate, 112.3g cerium nitrate, 82.4g titanium oxysulfate, 66.6g calcium chloride, and 5.5g ammonium metavanadate in 2L of deionized water, add dilute hydrochloric acid to adjust the pH to 1.5-2.0, and prepare a mixed acidic solution; (2) Add 25wt% ammonia water in parallel under high-speed stirring (800r / min). Stop for 5 minutes when the volume is 1 / 3, stop for 10 minutes when the volume is 2 / 3, and finally adjust the pH to 9.5; (3) Aging the slurry for 4 hours, filter and wash, and then slurry until the solid content is 35wt%. Add silica sol (accounting for 4wt% of the solid content) and hydrochloric acid to adjust the pH to 4.0; (4) Spray drying: inlet air temperature 320℃, outlet air temperature 120℃; (5) Calcination at 600℃ for 1.5 hours.
[0064] Example 2: Properties of the adjuvant:
[0065]
[0066] Example 3
[0067] Preparation steps: (1) Dissolve 158.6g magnesium sulfate, 278.4g aluminum sulfate, 52.0g cerium nitrate, 132.6g titanium oxysulfate, 29.6g calcium chloride, and 12.8g ammonium metavanadate in 2L of deionized water, and add dilute hydrochloric acid to adjust the pH to 1.5-2.0; (2) Add 25wt% ammonia water in parallel under high-speed stirring (800r / min). Stop for 8 minutes when 1 / 3 of the volume is reached, and stop for 6 minutes when 2 / 3 of the volume is reached, and finally adjust the pH to 8.8; (3) Aging the slurry for 3 hours, filtering and washing, and then slurrying to a solid content of 38wt%, adding silica sol (accounting for 8wt% of the solid content) and hydrochloric acid to adjust the pH to 3.8; (4) Spray drying: inlet air temperature 380℃, outlet air temperature 150℃; (5) Calcination at 550℃ for 2 hours.
[0068] Example 3: Properties of the adjuvant:
[0069]
[0070] Comparative Example 1
[0071] A denitrification and desulfurization dual-function additive was prepared according to the formula of the published patent CN110787834A:
[0072] Take 750g of alumina carrier and 200g of kaolin matrix, add 12g of mixed active components of copper nitrate, manganese oxide and cerium nitrate (CuO:MnO2:CeO2 mass ratio = 1:1:1), add 50g of aluminum sol as binder and 5g of modifier;
[0073] All components were mixed and pulped to form a uniform slurry with a solid content of 35 wt%. The slurry was spray-dried to obtain microspheres, which were then calcined at 700℃ for 3 hours to obtain a traditional impregnated copper-manganese-cerium-based desulfurization and denitrification dual-function additive.
[0074] Evaluation Experiment
[0075] The following four sets of experiments were conducted in a small riser evaluation device:
[0076] Blank experiment: using only the balancing agent (without any additives).
[0077] Example 1 Experiment: Balancing agent + 3wt% Example 1 adjuvant
[0078] Example 2 Experiment: Balancing agent + 3wt% Example 2 adjuvant
[0079] Example 3 Experiment: Balancing agent + 3wt% Example 3 adjuvant
[0080] Comparative Example 1 Experiment: Balancing agent + 3wt% Comparative Example 1 additive
[0081] The oils listed in Table 1 were used in each experiment, and the reaction conditions were consistent (reaction temperature 515℃, agent-to-oil ratio 6, reaction time 3.5s, regeneration temperature 710℃). SOx and NOx concentrations in the regenerated flue gas were measured using an online analyzer. The yield was calculated by distillation and fractionation of the products.
[0082] Table 2 Comparison of product distribution (wt%, dry basis)
[0083]
[0084] Table 3 Comparison of regenerated flue gas composition (ppm, dry basis)
[0085]
[0086] In summary, the sulfur-vanadium-nitrate triple-effect FCC additive prepared by the co-precipitation-spray granulation method of this invention achieves efficient removal of SOx and NOx from flue gas through the synergistic effect of the magnesium-aluminum-cerium sulfur transfer phase, the calcium titanate anti-vanadium capturing phase, and the vanadium oxide denitrification phase. At the same time, it effectively captures vanadium on the balancer and improves the distribution of catalytic cracking products, showing significant technical advantages and application prospects.
Claims
1. A three-way FCC additive, the chemical composition of which, based on oxides, comprises: Magnesium oxide 15-30wt%, aluminum oxide 25-45wt%, cerium oxide 5-12wt%, titanium oxide 8-20wt%, vanadium oxide 2-7wt%, calcium oxide 3-10wt%.
2. Among them, Magnesium oxide, aluminum oxide, and cerium oxide together constitute the sulfur transfer active phase, titanium oxide and calcium oxide together constitute the vanadium-resistant phase, and vanadium oxide constitutes the denitrification active phase. Each phase is uniformly distributed in the microspheres.
3. The triple-effect FCC additive according to claim 1, characterized in that: The magnesium oxide, aluminum oxide, and cerium oxide are derived from the co-precipitation products of magnesium salts, aluminum salts, and cerium salts, which form a magnesium-aluminum-cerium composite oxide solid solution in the additive.
4. The triple-effect FCC additive according to claim 1, characterized in that: The titanium oxide and calcium oxide are derived from the co-precipitation products of titanium salt and calcium salt, and form a perovskite-type CaTiO3 crystal phase during the calcination of the additives.
5. The triple-effect FCC additive according to claim 1, characterized in that: The vanadium oxide is derived from vanadium pentoxide obtained by the decomposition of metavanadate. It is highly dispersed in the interface of each oxide phase in the additive, and the particle size of the vanadium species is controlled between 2-5 nm.
6. The triple-effect FCC additive according to claim 1, characterized in that: The particle size distribution of the additive microspheres is 40-150 micrometers, and the bulk density is 0.7-0.9 g / mL.
7. The method for preparing the triple-effect FCC adjuvant according to any one of claims 1-5, characterized in that... Includes the following steps: (1) Prepare a mixed acidic solution containing divalent magnesium salt, trivalent aluminum salt, trivalent cerium salt, tetravalent titanium salt, divalent calcium salt and pentavalent vanadium salt, and add dilute hydrochloric acid to adjust the pH to 1.5-2.0 to ensure that all metal ions are completely dissolved and no precipitate is formed; (2) The mixed acidic solution and alkaline precipitant are added to the reactor in parallel under high-speed stirring. When one-third and two-thirds of the alkaline precipitant are added, the reaction is stopped for 5-10 minutes. The final pH value is controlled to 8.5-10.0 to carry out the coprecipitation reaction and obtain a coprecipitation slurry containing various metal hydroxides and / or oxides. (3) After aging, filtering and washing, the co-precipitated slurry is re-watered and pulped, and silica sol accounting for 3-10 wt% of the slurry solid content and a certain proportion of hydrochloric acid are added and stirred evenly. (4) Spray dry the slurry obtained in step (3) with an inlet air temperature of 300-400℃ and an outlet air temperature of 110-160℃ to obtain microspheres; (5) The microspheres are calcined at 500-650℃ for 1-2 hours to obtain the triple-effect FCC additive.
Citation Information
Patent Citations
Multifunctional catalyst for removing NOX and SOX in catalytic cracking regeneration flue gas and preparation method of multifunctional catalyst
CN102962061A
Additive of removing catalytic-cracking regenerated flue gas pollutant and preparation method of same
CN104759202A
Copper-manganese-cerium composite oxide FCC regenerated flue gas combustion-supporting denitration auxiliary agent and preparation method thereof
CN106345488A
Catalytic cracking flue gas desulfurization and denitration auxiliary agent, and preparation method thereof
CN110787834A
Bifunctional additive for reducing NOx and sulfur transfer in FCC regenerated flue gas and preparation method thereof