A method for regenerating a hydrogenation catalyst
By using a mixture of hydrogen and hydrogen sulfide gas to treat the deactivated distillate oil hydrotreating catalyst in a fixed-bed regeneration reactor, the problems of incomplete carbon removal and sulfur loss were solved, achieving efficient catalyst regeneration and cost savings.
Patent Information
- Application Number
- CN202510622821.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-15
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies for regenerating distillate oil hydrogenation catalysts suffer from incomplete removal of carbon deposits and loss of sulfur-containing species, resulting in a complex, costly, and time-consuming regeneration process.
A fixed-bed regeneration reactor is used to treat the deactivated catalyst at low temperature by using a mixture of hydrogen and hydrogen sulfide gas. Combined with the activation effect of the noble metal catalyst, carbon deposits are removed while sulfur-containing species are retained, thus avoiding the loss of sulfur during high-temperature oxidation.
It effectively removes carbon deposits, maintains catalyst activity, shortens the start-up cycle, reduces economic and time costs, and improves the efficiency of oil refining enterprises.
Smart Images

Figure CN123102425A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of distillate oil hydrogenation, specifically, it is a method for regenerating deactivated light distillate oil hydrogenation catalysts. Background Technology
[0002] The lifespan of distillate oil hydrotreating catalysts and hydrocracking catalysts is generally 3–5 years, while that of residue oil hydrotreating catalysts is generally 1–2 years. Residue oil hydrotreating catalysts that have deactivated generally do not undergo regeneration due to their high metal deposition, high carbon content, and low hydrogen-to-carbon atomic ratio. Except for residue oil hydrotreating catalysts, other hydrotreating catalysts can be regenerated 1–2 times after one cycle of industrial application. This is because deactivation of hydrotreating catalysts is mainly caused by carbon deposition, and carbon deposition-induced catalyst deactivation is a reversible process, thus its activity can be restored through regeneration.
[0003] Currently, the industrial method for regenerating deactivated catalysts in distillate oil hydrotreating is carbon burning regeneration. Under an oxygen and nitrogen atmosphere, carbon deposits on the catalyst are burned off, restoring the pore volume and specific surface area of the catalyst to the standard for use with fresh catalysts, thereby restoring the activity of the deactivated catalyst.
[0004] CN114682265 B discloses a method for regenerating a Co-Mo type jet fuel hydrogenation catalyst. This method involves treating the deactivated catalyst with carbon, followed by organic acid treatment, roasting, and impregnation, effectively restoring the catalyst's activity. However, this method has multiple regeneration steps and a complex process.
[0005] CN1122574C discloses a method for regenerating a hydrogenation catalyst. This method involves treating a deactivated catalyst at different temperature ranges by carbon burning, sulfur burning, and metal removal, followed by cooling and vibration screening to obtain a regenerated catalyst. This regeneration method can effectively remove impurities from the surface of the deactivated catalyst, restoring the deactivated catalyst to the level of a fresh catalyst.
[0006] The aforementioned patents and current industrial methods for regenerating deactivated catalysts using carbon burning effectively remove carbon deposits. However, the sulfur that maintains catalyst activity is also burned off during regeneration, and sulfur-containing gases are released. Furthermore, the regenerated catalyst requires further sulfidation treatment before reuse, increasing both the time and economic costs of catalyst regeneration. Therefore, there is an urgent need to develop a regeneration method that can retain sulfur on the catalyst while effectively removing carbon deposits. Summary of the Invention
[0007] To address the shortcomings of existing technologies, this invention provides a method for regenerating hydrogenation catalysts. This method, through the coordination of the catalyst and the process flow, can effectively remove carbon deposits on deactivated catalysts while retaining sulfur-containing species on the deactivated catalysts.
[0008] The method for regenerating the hydrogenation catalyst of the present invention includes the following: a fixed-bed regeneration reactor consisting of a noble metal catalyst bed and a deactivated hydrogenation catalyst bed from top to bottom;
[0009] (1) Hydrogen gas is continuously introduced from the top of the reactor and flows out from the bottom of the reactor, so that the entire reactor is in a hydrogen atmosphere and the tail gas is discharged from the bottom of the reactor.
[0010] (2) Heat the reactor to 150℃~170℃ and continuously introduce a mixture of hydrogen and hydrogen sulfide gas between the noble metal catalyst bed and the deactivated hydrogenation catalyst bed. The mixture gas passes through the lower bed catalyst and is discharged from the bottom of the reactor.
[0011] (3) Continue to heat the reactor to 230℃~260℃, maintain the temperature for a period of time, and discharge the regeneration tail gas from the bottom of the reactor;
[0012] (4) Continue to heat the reactor to 300℃~350℃, maintain the temperature for a period of time, and discharge the regeneration tail gas from the bottom of the reactor.
[0013] (5) Cool the reactor to 150℃~170℃, stop the flow of mixed gas, let it cool naturally to room temperature, stop the flow of hydrogen from the top of the reactor, and the regeneration of the deactivated catalyst is complete.
[0014] In the method of this invention, the noble metal catalyst can be a commercially available noble metal catalyst. Such catalysts have a strong ability to dissociate hydrogen and can activate hydrogen at relatively low temperatures. The HDO-18 catalyst developed by FRIPP is preferred. Noble metal catalysts generally use alumina as a support and Pt and / or Pd as active components. The content of the active component in the catalyst, by weight, is not less than 0.1%, and generally ranges from 0.1% to 1.5%.
[0015] In the method of this invention, the deactivated hydrogenation catalyst refers to a catalyst that has been partially deactivated or fails to meet reaction requirements due to carbon deposition during the hydrotreating of distillate oils. The deactivated hydrogenation catalyst generally uses alumina or modified alumina as a support, and molybdenum and / or tungsten, nickel and / or cobalt as active metal components. Deactivated hydrogenation catalysts include deactivated naphtha hydrogenation catalysts, deactivated kerosene hydrogenation catalysts, and deactivated diesel hydrogenation catalysts.
[0016] In the method of the present invention, the reactor conditions in step (1) are: at room temperature and at a pressure of 1.0 MPa to 8.0 MPa.
[0017] In the method of the present invention, based on the total amount of catalyst loaded in the regeneration reactor, the amount of noble metal catalyst bed loaded is 1% to 20%, preferably 5% to 15%; the amount of deactivated hydrogenation catalyst bed loaded is 80% to 99%, preferably 85% to 95%.
[0018] In the method of the present invention, the volume ratio of hydrogen to deactivated catalyst in step (1) is 50 to 300, preferably 80 to 200.
[0019] In the method of the present invention, the volume fraction of hydrogen sulfide in the mixed gas of hydrogen sulfide and hydrogen in step (2) is 0.1% to 0.3%, and the hydrogen sulfide content is sufficient to prevent sulfur loss during the regeneration of the deactivated catalyst. In the method of the present invention, the flow rate of the mixed gas to the volume ratio of the deactivated catalyst in step (2) is 10 to 200, preferably 50 to 150.
[0020] In the method of the present invention, the isothermal regeneration time in step (3) is 4h to 12h; the isothermal regeneration time in step (4) is 4h to 12h.
[0021] In the method of the present invention, the heating or cooling rate of each step is generally 10℃~15℃ / h.
[0022] In this invention, hydrogen enters from the top of the reactor and passes through the noble metal catalyst bed at the top. At a certain temperature, some of the hydrogen dissociates on the noble metal catalyst, becoming active hydrogen, which diffuses through the surface into the deactivated catalyst bed below the regeneration reactor. The carbon deposits on the deactivated hydrogenation catalyst undergo hydrogenation and cracking reactions under the action of the active hydrogen, transforming into hydrocarbon species with higher hydrogen content and smaller molecular weight. These are then removed by hydrogen purging, thereby restoring the hydrogenation activity of the deactivated catalyst.
[0023] To prevent the loss of sulfur-containing species from the deactivated hydrogenation catalyst and to prevent the reduction of the sulfided catalyst, a gas containing hydrogen sulfide (a mixture of hydrogen sulfide and hydrogen) is introduced from the middle of the reactor. This ensures the deactivated hydrogenation catalyst remains in a sulfided state and does not experience sulfur loss. Because carbon deposits are effectively removed and the sulfided state is maintained, the deactivated catalyst does not require sulfidation upon reuse after regeneration, saving on startup costs for sulfiding agents and shortening the startup cycle. Therefore, this invention is not only more environmentally friendly but also saves on economic and time costs, significantly improving the economic efficiency of refineries.
[0024] This invention, through the combination of catalyst and process flow, can effectively remove carbon deposits on deactivated catalysts at lower regeneration temperatures while retaining sulfur-containing species on the deactivated catalyst. Compared to traditional regeneration by burning carbon in an oxygen-containing atmosphere, the regeneration conditions of this invention are more moderate, sulfur-containing species are not burned off, and no sulfidation treatment is required after the deactivated catalyst is regenerated, saving time and economic costs during startup. Attached Figure Description
[0025] Figure 1This is a schematic diagram of a method for regenerating a hydrogenated deactivated catalyst according to the present invention.
[0026] Among them, 1-hydrogen; 2-mixed gas of hydrogen and hydrogen sulfide; 3-noble metal catalyst bed (upper bed); 4-deactivated hydrogenation catalyst bed (lower bed); 5-regenerated tail gas. Detailed Implementation
[0027] The present invention will now be described in detail with reference to embodiments and comparative examples, but this does not limit the scope of the invention.
[0028] Example 1
[0029] A 100 mL fixed-bed regeneration reactor was used. The upper bed of the noble metal catalyst was packed with 10 mL of HDO-18 noble metal catalyst, the properties of which are shown in Table 1. The lower bed of the deactivated hydrogenation catalyst was packed with 90 mL of deactivated coking gasoline hydrodediolefin catalyst S. The regeneration conditions were: regeneration pressure 2.0 MPa, hydrogen flow rate 9.0 L / h, hydrogen sulfide content in the mixed gas 0.2%, mixed gas flow rate 9.0 L / h, isothermal regeneration at 230℃ for 8 h, and isothermal regeneration at 300℃ for 8 h. After the catalyst S was regenerated, its activity was evaluated. The properties of the regenerated catalyst and the experimental evaluation results are shown in Table 2.
[0030] Example 2
[0031] A 100 mL fixed-bed regeneration reactor was used. The upper bed of the noble metal catalyst was packed with 10 mL of HDO-18 noble metal catalyst, and the lower bed of the deactivated hydrogenation catalyst was packed with 90 mL of deactivated kerosene hydrogenation catalyst F. The regeneration conditions were: regeneration pressure 2.0 MPa, hydrogen flow rate 12.0 L / h, hydrogen sulfide content in the mixed gas 0.2%, mixed gas flow rate B 9.0 L / h, isothermal regeneration at 240℃ for 8 h, and isothermal regeneration at 310℃ for 8 h. After catalyst regeneration, the activity of catalyst F was evaluated. The properties of the regenerated catalyst and the experimental evaluation results are shown in Table 3.
[0032] Example 3
[0033] A 100 mL fixed-bed regeneration reactor was used. The upper bed of the noble metal catalyst was loaded with 10 mL of HDO-18 noble metal catalyst, and the lower bed of the deactivated hydrogenation catalyst was loaded with 90 mL of deactivated diesel hydrogenation catalyst U. The regeneration conditions were: regeneration pressure 2.0 MPa, hydrogen flow rate 15.0 L / h, hydrogen sulfide content in the mixed gas 0.2%, mixed gas flow rate 9.0 L / h, isothermal regeneration at 250℃ for 8 h, and isothermal regeneration at 320℃ for 8 h. After catalyst regeneration, the activity of catalyst U was evaluated. The properties of the regenerated catalyst and the experimental evaluation results are shown in Table 4.
[0034] Comparative Example 1
[0035] A 100 mL fixed-bed regeneration reactor was used. The upper bed of the noble metal catalyst was packed with 10 mL of quartz sand (which has no dissociation activity for hydrogen), and the lower bed of the deactivated hydrotreating catalyst was packed with 90 mL of deactivated coking gasoline hydrodediolefin catalyst S. The regeneration conditions were: regeneration pressure 2.0 MPa, hydrogen flow rate 9.0 L / h, hydrogen sulfide content in the mixed gas 0.2%, mixed gas flow rate 9.0 L / h, isothermal regeneration at 230℃ for 8 h, and isothermal regeneration at 300℃ for 8 h. After catalyst regeneration, the activity of catalyst S was evaluated. The properties of the regenerated catalyst and the experimental evaluation results are shown in Table 2. This illustrates the regeneration effect of deactivated catalyst S when the noble metal catalyst without a noble metal bed is activated by hydrogen dissociation.
[0036] Comparative Example 2
[0037] A 100 mL fixed-bed regeneration reactor was used. The upper bed of the noble metal catalyst was packed with 10 mL of HDO-18 noble metal catalyst, and the lower bed of the deactivated hydrogenation catalyst was packed with 90 mL of deactivated kerosene hydrogenation catalyst F. Regeneration conditions were: regeneration pressure 2.0 MPa, hydrogen flow rate 12.0 L / h, mixed gas free of hydrogen sulfide (i.e., pure hydrogen with a volume concentration greater than 99.9%), mixed gas flow rate 9.0 L / h, isothermal regeneration at 240℃ for 8 h, and isothermal regeneration at 310℃ for 8 h. After catalyst regeneration, the activity of catalyst F was evaluated. The properties of the regenerated catalyst and the experimental evaluation results are shown in Table 3. This illustrates the regeneration effect of deactivated catalyst F when there is no hydrogen sulfide in the mixed gas.
[0038] Comparative Example 3
[0039] A 100 mL fixed-bed regeneration reactor was used. The upper bed of the precious metal catalyst was packed with 10 mL of HDO-18 precious metal catalyst, and the lower bed of the deactivated hydrogenation catalyst was packed with 90 mL of deactivated diesel hydrogenation catalyst U. The regeneration conditions were: regeneration pressure 2.0 MPa, hydrogen flow rate 15.0 L / h, mixed gas flow rate 0.0 L / h, isothermal regeneration at 250℃ for 8 h, and isothermal regeneration at 320℃ for 8 h. After catalyst regeneration, the activity of catalyst U was evaluated. The properties of the regenerated catalyst and the experimental evaluation results are shown in Table 4. This table illustrates the regeneration effect of deactivated catalyst U when no mixed gas is introduced.
[0040] Table 1. Physicochemical properties of catalysts
[0041]
[0042]
[0043] Table 2. Catalyst properties and experimental evaluation results before and after catalyst S regeneration.
[0044]
[0045] Table 2 shows that the deactivated coking gasoline hydrodediolefin catalyst S can be regenerated, and the pore volume and specific surface area of the regenerated S can be restored to the level of the fresh catalyst. Using the present invention, the carbon removal rate on the catalyst is 95.68%, and the sulfur retention rate on the catalyst is close to 100%. The experimental evaluation results show that the diene removal rate of the deactivated S is 2.8%, and the diene removal rate of the regenerated S after regeneration in Example 1 is 96.60%, which is also 96.60% of the fresh catalyst. This indicates that the catalytic activity of the catalyst can be completely restored using the method of the present invention. The carbon content of the S regenerated catalyst in Comparative Example 1 is still as high as 4.78%, and the specific surface area and pore volume are slightly increased. This indicates that when the upper bed of the regeneration reactor is filled with quartz sand, the carbon deposits on the catalyst cannot be effectively removed. The experimental evaluation data of the S regenerated catalyst in Comparative Example 1 also show that when the upper bed of the regeneration reactor is filled with quartz sand, the diene removal activity of the regenerated catalyst cannot be effectively restored.
[0046] Table 3. Catalyst properties and experimental evaluation results before and after catalyst F regeneration.
[0047]
[0048] Table 3 shows that the deactivated kerosene hydrotreating catalyst F can be regenerated. The F regenerator in Example 2 can effectively achieve deep hydrodesulfurization and denitrification. The activity of the F regenerator in Example 2 is comparable to that of the new F regenerator, and the sulfur and nitrogen content of the refined kerosene from both are less than 1 mg / kg. The catalyst regeneration results and evaluation data of Comparative Example 2 show that when the mixed gas does not contain hydrogen sulfide during regeneration, the carbon deposits on the catalyst can be effectively removed, but a large amount of sulfur will be lost from the catalyst, with a sulfur loss rate of over 50%. After regeneration, the hydrodesulfurization and denitrification activity of the catalyst cannot be effectively restored. As shown in Example 2 and Comparative Example 2, using the present invention, the deactivated catalyst can effectively remove carbon deposits without sulfur loss.
[0049] Table 4. Catalyst properties and experimental evaluation results before and after catalyst U regeneration.
[0050]
[0051]
[0052] Table 4 shows that the diesel hydrodeactivation catalyst of this invention can effectively remove carbon deposits. The evaluation data of the U regenerator in Example 3 shows that the activity of the U regenerator can be completely restored to the level of the fresh catalyst. Comparative Example 3 shows that during the regeneration process, when no mixed gas is introduced, a large amount of sulfur on the catalyst is still lost, with a sulfur loss rate of over 50%, and carbon deposits remain on the catalyst after regeneration. The U regenerator in Comparative Example 3 cannot achieve effective regeneration of the deactivated catalyst.
[0053] In summary, this invention can effectively remove carbon deposits from deactivated catalysts in distillate oil hydrotreating while retaining sulfur-containing species on the deactivated catalyst. Using this invention, the deactivated catalyst can be effectively regenerated. It is worth noting that this invention is only applicable to reversible deactivation caused by catalyst carbon deposits; deactivation caused by metal deposition, etc., is not applicable to this invention.
Claims
1. A method for regenerating a hydrogenation catalyst, characterized in that... The following contents are included: The fixed bed regeneration reactor consists of a precious metal catalyst bed and a deactivated hydrogenation catalyst bed from top to bottom; (1) Hydrogen gas is continuously introduced from the top of the reactor and flows out from the bottom of the reactor, so that the entire reactor is in a hydrogen atmosphere and the tail gas is discharged from the bottom of the reactor; (2) The reactor is heated to 150℃~170℃, and a mixture of hydrogen and hydrogen sulfide gas is continuously introduced from between the precious metal catalyst bed and the deactivated hydrogenation catalyst bed. The mixture passes through the lower bed catalyst and is discharged from the bottom of the reactor; (3) The reactor is heated to 230℃~260℃ and regenerated at a constant temperature for a period of time. The regenerated tail gas is discharged from the bottom of the reactor; (4) The reactor is heated to 300℃~350℃ and regenerated at a constant temperature for a period of time. The regenerated tail gas is discharged from the bottom of the reactor; (5) The reactor is cooled to 150℃~170℃, the mixture is stopped, and the reactor is allowed to cool naturally to room temperature. The hydrogen gas introduced from the top of the reactor is stopped, and the deactivated catalyst regeneration is completed.
2. The regeneration method according to claim 1, characterized in that: The noble metal catalyst uses alumina as a support and Pt and / or Pd as active components. The content of the active components in the catalyst by weight is not less than 0.1%, preferably 0.1% to 1.5%.
3. The regeneration method according to claim 1, characterized in that: The deactivated hydrogenation catalyst refers to a catalyst that is partially deactivated or fails to meet reaction requirements due to carbon deposition during the hydrotreating of distillate oil. The deactivated hydrogenation catalyst uses alumina or modified alumina as a support and molybdenum and / or tungsten, nickel and / or cobalt as active metal components.
4. The regeneration method according to claim 1, characterized in that: The conditions for the reactor in step (1) are: at room temperature and at a pressure of 1.0 MPa to 8.0 MPa.
5. The regeneration method according to claim 1, characterized in that: Based on the total catalyst loading in the regeneration reactor, the loading of the precious metal catalyst bed is 1% to 20%, preferably 5% to 15%; the loading of the deactivated hydrogenation catalyst bed is 80% to 99%, preferably 85% to 95%.
6. The regeneration method according to claim 1, characterized in that: The volume ratio of hydrogen to deactivated catalyst in step (1) is 50 to 300, preferably 80 to 200.
7. The regeneration method according to claim 1, characterized in that: In the mixture of hydrogen sulfide and hydrogen described in step (2), the volume fraction of hydrogen sulfide is 0.1% to 0.3%.
8. The regeneration method according to claim 1, characterized in that: The ratio of the mixed gas flow rate to the deactivated catalyst volume in step (2) is 10 to 200, preferably 50 to 150.
9. The regeneration method according to claim 1, characterized in that: The isothermal regeneration time in step (3) is 4h to 12h; the isothermal regeneration time in step (4) is 4h to 12h.
10. The regeneration method according to claim 1, characterized in that: The heating or cooling rate for each step is 10℃~15℃ / h.
Citation Information