A method for regenerating a deactivated hydrogenation catalyst

By combining a fixed-bed regeneration reactor with hydrogen, hexane solvent (a sulfurizing agent), the problems of incomplete carbon removal and sulfur loss in deactivated distillate oil hydrogenation catalysts were solved, achieving efficient regeneration and low-cost catalyst recovery.

CN123102426APending Publication Date: 2026-11-17CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202510622825.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-15
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies for the regeneration of deactivated distillate oil hydrogenation catalysts suffer from incomplete removal of carbon deposits and loss of sulfides, resulting in high regeneration costs and extended regeneration time.

Method used

A fixed-bed regeneration reactor is used to wash and regenerate the deactivated catalyst at different temperatures using hydrogen and hexane solvent containing sulfides. By utilizing the activation effect of the noble metal catalyst and the use of an appropriate amount of sulfides, carbon deposits are effectively removed while retaining sulfur-containing species on the catalyst.

Benefits of technology

It achieves effective removal of carbon deposits at lower temperatures, preserves the sulfidation state of the catalyst, shortens the start-up cycle, reduces regeneration costs, and restores catalyst activity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102426A_ABST
    Figure CN123102426A_ABST
Patent Text Reader

Abstract

This invention discloses a method for regenerating a deactivated hydrogenation catalyst, comprising: a fixed-bed regeneration reactor with first and second catalyst beds arranged from top to bottom, wherein the first bed is filled with a noble metal catalyst and the second bed is filled with a deactivated hydrogenation catalyst; the specific regeneration process is as follows: (1) under normal temperature and certain pressure conditions, hydrogen gas is introduced from the top of the reactor; (2) the reactor is heated to 150℃~170℃, and n-hexane solvent containing a sulfiding agent is introduced between the first and second beds; (3) the reactor is heated to the first regeneration temperature and regenerated by constant temperature flushing; (4) the reactor is heated to the second regeneration temperature and regenerated by constant temperature flushing, and the catalyst is regenerated. This method, through the combination of catalyst and process flow, can effectively remove carbon deposits on the deactivated catalyst while retaining sulfur-containing species on the deactivated catalyst. This regeneration method can also avoid the emission of sulfur-containing gases during the conventional deactivated catalyst regeneration process, making it more environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for regenerating a hydrogenation catalyst for distillate oil, specifically a method for regenerating a deactivated hydrogenation catalyst for light distillate oil. Background Technology

[0002] The lifespan of distillate oil hydrotreating catalysts and hydrocracking catalysts is generally 3–5 years, while that of residue oil hydrotreating catalysts is generally 1–2 years. Residue oil hydrotreating catalysts that have deactivated generally do not undergo regeneration due to their high metal deposition, high carbon content, and low hydrogen-to-carbon atomic ratio. Except for residue oil hydrotreating catalysts, other hydrotreating catalysts can be regenerated 1–2 times after one cycle of industrial application. This is because deactivation of hydrotreating catalysts is mainly caused by carbon deposition, and carbon deposition-induced catalyst deactivation is a reversible process, thus its activity can be restored through regeneration.

[0003] Currently, the industrial method for regenerating deactivated catalysts in distillate oil hydrotreating is carbon burning regeneration. Under an oxygen and nitrogen atmosphere, carbon deposits on the catalyst are burned off, restoring the pore volume and specific surface area of ​​the catalyst to the standard for use with fresh catalysts, thereby restoring the activity of the deactivated catalyst.

[0004] CN114682265 B discloses a method for regenerating a Co-Mo type jet fuel hydrogenation catalyst. This method involves treating the deactivated catalyst with carbon, followed by organic acid treatment, roasting, and impregnation, effectively restoring the catalyst's activity. However, this method has multiple regeneration steps and a complex process.

[0005] CN1122574C discloses a method for regenerating a hydrogenation catalyst. This method involves treating a deactivated catalyst at different temperature ranges by carbon burning, sulfur burning, and metal removal, followed by cooling and vibration screening to obtain a regenerated catalyst. This regeneration method can effectively remove impurities from the surface of the deactivated catalyst, restoring the deactivated catalyst to the level of a fresh catalyst.

[0006] The aforementioned patents and current industrial methods for regenerating deactivated catalysts using carbon burning effectively remove carbon deposits. However, the sulfur that maintains catalyst activity is also burned off during regeneration, and sulfur-containing gases are released. Furthermore, the regenerated catalyst requires further sulfidation treatment before reuse, increasing both the time and economic costs of catalyst regeneration. Therefore, there is an urgent need to develop a regeneration method that can retain sulfur on the catalyst while effectively removing carbon deposits. Summary of the Invention

[0007] To address the shortcomings of existing technologies, this invention provides a method for regenerating deactivated hydrogenation catalysts. This method, through the coordination of the catalyst and the process flow, can effectively remove carbon deposits on the deactivated catalyst while retaining sulfur-containing species. This regeneration method also avoids the emission of sulfur-containing gases during conventional deactivated catalyst regeneration processes, making it more environmentally friendly.

[0008] The method for regenerating the deactivated hydrogenation catalyst of the present invention includes the following:

[0009] The fixed-bed regeneration reactor consists of a first catalyst bed and a second catalyst bed arranged from top to bottom. The first catalyst bed is filled with a noble metal catalyst, and the second catalyst bed is filled with a deactivated hydrogenation catalyst. The specific regeneration process is as follows:

[0010] (1) Under certain pressure conditions, hydrogen gas is introduced from the top of the reactor to make the reactor a hydrogen atmosphere;

[0011] (2) Heat the reactor to 150℃~170℃ and introduce n-hexane solvent containing sulfiding agent between the first catalyst bed and the second catalyst bed;

[0012] (3) Heat the reactor to the first regeneration temperature and perform constant temperature flushing and regeneration;

[0013] (4) Heat the reactor to the second regeneration temperature and continue constant temperature rinsing and regeneration to regenerate the catalyst.

[0014] In the method of this invention, the deactivated hydrogenation catalyst refers to a catalyst that has been partially deactivated or fails to meet reaction requirements due to carbon deposition during the hydrotreating of distillate oils. The deactivated hydrogenation catalyst generally uses alumina or modified alumina as a support, and molybdenum and / or tungsten, nickel and / or cobalt as active metal components. Deactivated hydrogenation catalysts include deactivated naphtha hydrogenation catalysts, deactivated kerosene hydrogenation catalysts, and deactivated diesel hydrogenation catalysts.

[0015] In the method of this invention, the noble metal catalyst can be a commercially available noble metal catalyst. Such catalysts have a strong ability to dissociate hydrogen and can activate hydrogen at relatively low temperatures. Noble metal catalysts generally use alumina as a support and Pt and / or Pd as the active component. The content of the active component in the catalyst, by weight, is not less than 0.1%, and generally 0.1% to 1.5%. Preferably, the HDO-18 catalyst developed by FRIPP is used.

[0016] In the method of the present invention, based on the total amount of catalyst loaded in the regeneration reactor, the catalyst loading amount of the first catalyst bed is 1% to 20%, preferably 5% to 15%; and the catalyst loading amount of the second catalyst bed is 80% to 99%, preferably 85% to 95%.

[0017] In the method of the present invention, the pressure in step (1) is 1.0 MPa to 8.0 MPa, the volume ratio of hydrogen (under standard conditions) to the generating agent is 100 to 200, and step (1) is generally performed at room temperature (5℃ to 40℃).

[0018] In the method of this invention, the content of the sulfiding agent in the hexane solvent containing the sulfiding agent is 0.02% to 0.05% of the mass fraction of hexane, calculated as elemental sulfur. Injecting too much sulfiding agent will result in waste, while injecting too little will cause desulfurization of the catalyst. The volume hourly space velocity (VHSV) for rinsing with the hexane solvent is 1.0 h⁻¹. -1 ~10.0h -1 The volume hourly space velocity of the solvent flush can be adjusted according to the degree of deactivation due to carbon deposition in the catalyst.

[0019] In the method of the present invention, the first regeneration temperature in step (3) is 230℃~260℃, and the constant temperature rinsing and regeneration time is 4~12 hours.

[0020] In the method of the present invention, the second regeneration temperature in step (3) is 300℃~350℃, and the constant temperature rinsing and regeneration time is 4~12 hours.

[0021] In the method of this invention, the heating and cooling rates are generally 10℃~15℃ / h, except for natural cooling.

[0022] In the method of the present invention, after step (4) is completed, the temperature is generally lowered to 150℃~170℃, the introduction of n-hexane solvent containing sulfiding agent is stopped, and then the reactor is naturally cooled to room temperature (generally 5℃~40℃), the introduction of hydrogen is stopped, and the regeneration of deactivated catalyst is completed.

[0023] This invention, through the coordination of catalyst and process flow, can effectively remove carbon deposits on deactivated catalysts at lower regeneration temperatures. First, hydrogen gas enters from the top of the reactor. A hexane solvent containing a sulfiding agent is introduced between the first and second catalyst beds. Some of the hydrogen dissociates on the noble metal catalyst, becoming active hydrogen, which diffuses into the second catalyst bed via surface diffusion. Under the action of the active hydrogen, the carbon deposits on the deactivated hydrogenation catalyst undergo hydrogenation and cracking reactions, transforming into hydrocarbon species with higher hydrogen content and smaller molecular weights. Simultaneously, these are removed by the rinsing action of the hexane solvent containing the sulfiding agent, thus regenerating the catalyst. To prevent the loss of sulfur-containing species from the deactivated catalyst in the lower bed and to prevent the reduction of the sulfided catalyst, a small amount of sulfiding agent is injected into the hexane solvent. This ensures that the deactivated catalyst in the lower bed remains in a sulfided state, preventing sulfur loss. Because the carbon deposits are effectively removed while retaining the sulfur-containing species on the deactivated catalyst, the sulfided state is maintained. Therefore, after the deactivated catalyst is regenerated, it does not need to be sulfided when it is reused, thus saving the cost of using sulfiding agents at the start-up and shortening the start-up cycle. Attached Figure Description

[0024] Figure 1 This is a schematic diagram of a method for regenerating a hydrogenated deactivated catalyst according to the present invention.

[0025] The mixture consists of: 1-hexane solvent; 2-hydrogen; 3-sulfurizing agent; 4-first catalyst bed (upper bed); 5-second catalyst bed (lower bed); and 6-a mixture of hexane solvent flushing solution and hydrogen.

[0026] The implementing party

[0027] The present invention will now be described in detail with reference to embodiments and comparative examples, but this does not limit the scope of the invention.

[0028] Example 1

[0029] A 100 mL fixed-bed regeneration reactor was used. The first catalyst bed (upper bed) was packed with 10 mL of HDO-18 noble metal catalyst, the properties of which are shown in Table 1. The second catalyst bed (lower bed) was packed with 90 mL of A coking gasoline hydrodediolefin deactivation catalyst. The regeneration conditions were: hydrogen flow rate to the upper bed of 12.0 L / h, regeneration pressure of 2.0 MPa, and hexane solvent space velocity of 4.0 h⁻¹. -1 FSA-55 environmentally friendly sulfurizing agent was injected into n-hexane. The mass fraction of FSA-55 was 0.09% (equivalent to 0.05% sulfur content in n-hexane solvent). The catalyst was regenerated by constant temperature flushing at 230℃ for 8 hours, and then by constant temperature flushing at 300℃ for 8 hours. After the catalyst regeneration was completed, the activity of catalyst A was evaluated. The properties of the regenerated catalyst and the experimental evaluation results are shown in Table 2.

[0030] Example 2

[0031] A 100 mL fixed-bed regeneration reactor was used. The first catalyst bed (upper bed) was packed with 10 mL of HDO-18 noble metal catalyst, and the second catalyst bed (lower bed) was packed with 90 mL of B kerosene hydrodeactivation catalyst. The regeneration conditions were: hydrogen flow rate to the upper bed of 12.0 L / h, regeneration pressure of 2.0 MPa, and hexane solvent hourly space velocity of 4.0 h⁻¹. -1 FSA-55 environmentally friendly sulfurizing agent was injected into n-hexane. The mass fraction of FSA-55 was 0.09% (equivalent to 0.05% sulfur content in n-hexane solvent). The catalyst was regenerated by constant temperature flushing at 240℃ for 8 hours, and then by constant temperature flushing at 310℃ for 8 hours. After the catalyst regeneration was completed, the activity of catalyst B was evaluated. The properties of the regenerated catalyst and the experimental evaluation results are shown in Table 3.

[0032] Example 3

[0033] A 100 mL fixed-bed regeneration reactor was used. The first catalyst bed (upper bed) was packed with 10 mL of HDO-18 noble metal catalyst, and the second catalyst bed (lower bed) was packed with 90 mL of C diesel hydrodeactivation catalyst. The regeneration conditions were: hydrogen flow rate to the upper bed of 12.0 L / h, regeneration pressure of 2.0 MPa, and n-hexane solvent hourly space velocity of 4.0 h⁻¹. -1 FSA-55 environmentally friendly sulfurizing agent was injected into n-hexane. The mass fraction of FSA-55 was 0.09% (equivalent to 0.05% sulfur content in n-hexane solvent). The catalyst was regenerated by constant temperature flushing at 250℃ for 8 hours, and then by constant temperature flushing at 320℃ for 8 hours. After the catalyst regeneration was completed, the activity of the C catalyst was evaluated. The properties of the regenerated catalyst and the experimental evaluation results are shown in Table 4.

[0034] Comparative Example 1

[0035] A 100 mL fixed-bed regeneration reactor was used. The first catalyst bed (upper bed) was packed with 10 mL of silica sand (which has no dissociation activity for hydrogen), and the second catalyst bed (lower bed) was packed with 90 mL of A coking gasoline hydrodediolefin deactivation catalyst. The regeneration conditions were: hydrogen flow rate to the upper bed of 12.0 L / h, regeneration pressure of 2.0 MPa, and n-hexane solvent hourly space velocity of 4.0 h⁻¹. -1FSA-55 environmentally friendly sulfurizing agent was injected into n-hexane. The mass fraction of FSA-55 was 0.09% (equivalent to 0.05% sulfur content in n-hexane solvent). The catalyst was regenerated by constant temperature flushing at 230℃ for 8 hours, and then by constant temperature flushing at 300℃ for 8 hours. After catalyst regeneration, the activity of catalyst A was evaluated. The properties of the regenerated catalyst and the experimental evaluation results are shown in Table 2. This is used to illustrate the regeneration effect of deactivated catalyst A when hydrogen is dissociated and activated without a first bed of noble metal catalyst.

[0036] Comparative Example 2

[0037] A 100 mL fixed-bed regeneration reactor was used. The first catalyst bed (upper bed) was packed with 10 mL of HDO-18 noble metal catalyst, and the second catalyst bed (lower bed) was packed with 90 mL of B kerosene hydrodeactivation catalyst. The regeneration conditions were: hydrogen flow rate to the upper bed of 12.0 L / h, regeneration pressure of 2.0 MPa, and hexane solvent hourly space velocity of 4.0 h⁻¹. -1 Without injecting any sulfiding agent into the hexane, the catalyst was regenerated by constant-temperature flushing at 240℃ for 8 hours, and then by constant-temperature flushing at 310℃ for 8 hours. After the catalyst regeneration was completed, the activity of catalyst B was evaluated. The properties of the regenerated catalyst and the experimental evaluation results are shown in Table 3. This is used to illustrate the regeneration effect of deactivated catalyst B when no sulfiding agent is injected into the hexane flushing solvent.

[0038] Comparative Example 3

[0039] A 100 mL fixed-bed regeneration reactor was used. The first catalyst bed (upper bed) was packed with 10 mL of HDO-18 noble metal catalyst, and the second catalyst bed (lower bed) was packed with 90 mL of C diesel hydrodeactivation catalyst. The regeneration conditions were: hydrogen flow rate to the upper bed of 12.0 L / h, regeneration pressure of 2.0 MPa, and hexane solvent space velocity of 0 h⁻¹. -1 The FSA-55 sulfiding agent injection mass flow rate was the same as in Example 3. The catalyst was regenerated by constant-temperature flushing at 250°C for 8 hours, and then by constant-temperature flushing at 320°C for 8 hours. After catalyst regeneration, the activity of the C catalyst was evaluated. The properties of the regenerated catalyst and the experimental evaluation results are shown in Table 4. This illustrates the regeneration effect of the deactivated C catalyst when hexane solvent is not introduced for solvent flushing of the deactivated catalyst in the lower bed.

[0040] Table 1. Physicochemical properties of catalysts

[0041] Catalyst number HDO-18 Metal composition Pt-Pd Physical properties Pore ​​volume, mL / g ≮0.45 <![CDATA[specific surface area, m 2 / g]]> ≮170 Compressive strength ≮90 shape cylindrical bar

[0042] Table 2A Catalyst Properties and Experimental Evaluation Results Before and After Regeneration

[0043]

[0044]

[0045] As shown in Table 2, using the regenerated catalyst of this invention, the deactivated catalyst A for the hydrodeolefinization of coking gasoline can be regenerated, and the pore volume and specific surface area of ​​the regenerated catalyst A can be restored to the level of the fresh catalyst. Using this invention, the carbon removal rate on the catalyst is 95.68%, and the sulfur retention rate on the catalyst is close to 100%. Experimental evaluation results show that the diene removal rate of the deactivated catalyst A is 2.8%, while the diene removal rate of the regenerated catalyst A after regeneration in Example 1 is 96.60%, the same as the fresh catalyst. This indicates that using the regenerated catalyst A of this invention, the catalytic activity of the catalyst can be completely restored. The carbon content of the regenerated catalyst A in Comparative Example 1 is still as high as 4.78%, and the specific surface area and pore volume are slightly reduced, indicating that when the upper bed of the regeneration reactor is filled with quartz sand, the carbon deposits on the catalyst cannot be effectively removed. The experimental evaluation data of the regenerated catalyst A in Comparative Example 1 also show that when the upper bed of the regeneration reactor is filled with quartz sand, the diene removal activity of the regenerated catalyst cannot be effectively restored.

[0046] Table 3B Catalyst properties and experimental evaluation results before and after regeneration

[0047]

[0048]

[0049] Table 3 shows that using the regenerated catalyst of this invention, the deactivated catalyst B for kerosene hydrotreating can be regenerated. The regenerator B in Example 2 can effectively achieve deep hydrotreating desulfurization and denitrification. The activity of the regenerator B in Example 2 is comparable to that of the new catalyst B, and the sulfur and nitrogen content of the refined kerosene from both is less than 1 mg / kg. The catalyst regeneration results and evaluation data of Comparative Example 2 show that when the hexane washing solvent does not contain sulfur during regeneration, the carbon deposits on the catalyst can be effectively removed, but a large amount of sulfur will be lost from the catalyst, with a sulfur loss rate of over 50%. After regeneration, the hydrotreating desulfurization and denitrification activity of the catalyst cannot be effectively restored. As shown in Example 2 and Comparative Example 2, using this invention, the deactivated catalyst can effectively remove carbon deposits without sulfur loss.

[0050] Table 4. Catalyst properties and experimental evaluation results before and after C regeneration.

[0051]

[0052]

[0053] Table 4 shows that the diesel hydrodeactivation catalyst of the present invention can effectively remove carbon deposits. The evaluation data of the C regenerator in Example 3 indicates that the present invention does not exhibit desulfurization, and the activity of the C regenerator can be fully restored to the level of the fresh catalyst. Comparative Example 3 illustrates that during the regeneration process, when hexane solvent is not introduced to rinse the deactivated catalyst in the lower bed, the carbon deposits on the deactivated catalyst cannot be effectively removed by solvent rinsing, and the catalyst activity cannot be effectively restored.

[0054] In summary, this invention can effectively remove carbon deposits from deactivated catalysts in distillate oil hydrotreating while retaining sulfur-containing species on the deactivated catalyst. Using this invention, the deactivated catalyst can be effectively regenerated. It is worth noting that this invention is only applicable to reversible deactivation caused by catalyst carbon deposits; deactivation caused by metal deposition, etc., is not applicable to this invention.

Claims

1. A method for regenerating a deactivated hydrogenation catalyst, characterized in that... The following contents are included: The fixed bed regeneration reactor is provided with a first catalyst bed and a second catalyst bed from top to bottom, wherein the first catalyst bed is filled with a noble metal catalyst and the second catalyst bed is filled with a deactivated hydrogenation catalyst; The specific regeneration process is as follows: (1) Under certain pressure conditions, hydrogen gas is introduced from the top of the reactor to make the reactor in a hydrogen atmosphere; (2) The reactor is heated to 150℃~170℃ and n-hexane solvent containing sulfiding agent is introduced between the first catalyst bed and the second catalyst bed; (3) The reactor is heated to the first regeneration temperature and is regenerated by constant temperature flushing; (4) The reactor is heated to the second regeneration temperature and is regenerated by constant temperature flushing, and the catalyst is regenerated.

2. The regeneration method according to claim 1, characterized in that: The deactivated hydrogenation catalyst refers to a catalyst that is partially deactivated or fails to meet reaction requirements due to carbon deposition during the hydrotreating of distillate oil; the deactivated hydrogenation catalyst uses alumina or modified alumina as a support, and molybdenum and / or tungsten, nickel and / or cobalt as active metal components.

3. The regeneration method according to claim 1, characterized in that: The noble metal catalyst uses alumina as a support and Pt and / or Pd as active components, with the content of the active components in the catalyst being not less than 0.1% by weight.

4. The regeneration method according to claim 1, characterized in that: Based on the total catalyst loading in the regeneration reactor, the catalyst loading of the first catalyst bed is 1% to 20%, preferably 5% to 15%; the catalyst loading of the second catalyst bed is 80% to 99%, preferably 85% to 95%.

5. The regeneration method according to claim 1, characterized in that: The pressure mentioned in step (1) is 1.0MPa to 8.0MPa, and the volume ratio of hydrogen to the pre-generated agent under standard conditions is 100 to 200.

6. The regeneration method according to claim 1, characterized in that: In the n-hexane solvent containing a sulfiding agent, the sulfiding agent content, calculated as elemental sulfur, accounts for 0.02% to 0.05% of the mass fraction of n-hexane.

7. The regeneration method according to claim 1, characterized in that: The volume space velocity of the n-hexane solvent flushing was 1.0 h -1 ~ 10.0 h -1 .

8. The regeneration method according to claim 1, characterized in that: The first regeneration temperature in step (3) is 230℃~260℃, and the constant temperature rinsing and regeneration time is 4~12 hours.

9. The regeneration method according to claim 1, characterized in that: The second regeneration temperature in step (3) is 300℃~350℃, and the constant temperature rinsing and regeneration time is 4~12 hours.

10. The regeneration method according to claim 1, characterized in that: After step (4) is completed, the temperature is first lowered to 150℃~170℃, the flow of n-hexane solvent containing sulfiding agent is stopped, and then the reactor is allowed to cool down naturally to room temperature. The flow of hydrogen is then stopped, and the deactivated catalyst regeneration is completed.

Citation Information

Patent Citations

  • Process for regenerating hydrocatalyst

    CN1122574C