A method for removing arsenic and enriching tungsten from waste vanadium-tungsten-titanium SCR denitration catalyst
By combining choline chloride pre-adsorption, in-situ carbonization under nitrogen atmosphere, and alkaline oxygen leaching, the problems of arsenic removal and tungsten component stability during the regeneration of waste vanadium-tungsten-titanium SCR denitrification catalysts were solved, achieving efficient catalyst regeneration and stability restoration.
Patent Information
- Application Number
- CN202611298177.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-25
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to simultaneously and effectively remove arsenic contaminants and maintain the stability of tungsten components during the regeneration of spent vanadium-tungsten-titanium SCR denitration catalysts, leading to decreased catalyst activity and loss of tungsten components.
A method combining choline chloride pre-adsorption, in-situ carbonization under nitrogen atmosphere, and alkaline-oxygen leaching was adopted. Choline chloride pre-adsorption enhanced the retention capacity of tungsten and vanadium components, a carbonization modification layer was formed under nitrogen atmosphere, and ultrasonic treatment under alkaline-oxygen system achieved efficient removal of arsenic and stable retention of tungsten.
It achieves significant inhibition of tungsten migration and loss while removing arsenic, improves catalyst regeneration efficiency and long-term stability, and restores catalyst denitrification performance.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of catalyst regeneration technology, specifically relating to a method for removing arsenic and enriching tungsten in a waste vanadium-tungsten-titanium SCR denitrification catalyst. Background Technology
[0002] Waste vanadium-tungsten-titanium SCR denitrification catalysts typically use TiO2 as a support and are loaded with active or co-catalytic components such as WO3 and V2O5. They are widely used in thermal power generation, waste incineration, and other industrial flue gas denitrification applications. With prolonged service life, these catalysts are susceptible to poisoning and deactivation by harmful components such as arsenic in the flue gas, leading to a decrease in their denitrification activity. Since these catalysts still retain functional components such as tungsten and vanadium, as well as the TiO2 support, maintaining the stability of key functional components while removing arsenic pollutants is beneficial for restoring the catalyst's denitrification performance and achieving high-value regeneration and reuse of waste SCR denitrification catalysts. However, arsenic in the flue gas not only causes poisoning and deactivation of active components, but it also accumulates on the catalyst surface and interacts with the active components on the catalyst surface, thus increasing the difficulty of catalyst regeneration and reuse.
[0003] To overcome the regeneration challenge caused by arsenic surface enrichment, existing wet arsenic removal processes often require highly alkaline, oxidizing, or complexing treatment conditions to enhance the removal effect. However, while these harsh conditions remove surface arsenic contamination, they also easily trigger the simultaneous dissolution or loss of tungsten co-catalyst components. Especially in alkaline leaching environments, tungsten components are easily converted into tungstates or polytungstates and enter the liquid phase, causing irreversible tungsten loss, which severely degrades the activity recovery level and long-term stability of the regenerated catalyst.
[0004] Therefore, in order to suppress the loss of tungsten components and improve the selectivity of arsenic removal, it is necessary to develop a regeneration method that can effectively reduce the residual amount of As in the catalyst while achieving stable retention of tungsten components, in order to solve the problem that it is difficult to simultaneously achieve arsenic removal and tungsten component retention during the regeneration of existing waste vanadium-tungsten-titanium SCR denitrification catalysts.
[0005] It should be noted that the above statements are only used to provide background information related to this application and do not necessarily constitute prior art. Summary of the Invention
[0006] In view of this, the purpose of this invention is to provide a method for removing arsenic and enriching tungsten from waste vanadium-tungsten-titanium SCR denitration catalysts. The preparation method provided by this invention combines choline chloride pre-adsorption, in-situ carbonization under a nitrogen atmosphere, and alkaline-oxygen leaching to reduce tungsten migration and loss while removing arsenic from the waste SCR denitration catalyst. This method, through a three-step synergistic process of choline chloride pre-adsorption, in-situ carbonization under a nitrogen atmosphere, and alkaline-oxygen leaching, aims to achieve efficient arsenic removal from the catalyst while significantly inhibiting tungsten migration and dissolution, reducing its loss, thereby achieving the dual objectives of arsenic removal and tungsten enrichment.
[0007] Specifically, this invention provides a method for removing arsenic and enriching tungsten from waste vanadium-tungsten-titanium SCR denitration catalyst, comprising the following steps: S1. Add the waste vanadium-tungsten-titanium SCR denitration catalyst to an aqueous solution of choline chloride, allow it to stand or shake at room temperature for adsorption, and filter to obtain the pre-adsorbed catalyst. S2. The pre-adsorbed catalyst is placed in a nitrogen atmosphere, heated and kept at that temperature, and then cooled to room temperature to obtain a carbonized modified catalyst. S3. The carbonized modified catalyst is impregnated in a mixed solution containing an alkaline oxygen system and subjected to ultrasonic reaction. After filtration and washing until neutral, an arsenic-removing and tungsten-rich catalyst is obtained.
[0008] In some specific embodiments of the present invention, the concentration of the choline chloride aqueous solution in S1 is 0.01~0.5mol / L.
[0009] In some specific embodiments of the present invention, the solid-liquid ratio of the waste vanadium-tungsten-titanium SCR denitration catalyst in S1 to the aqueous choline chloride solution is 1:(2-5)g / mL.
[0010] In some specific embodiments of the present invention, the static or oscillating adsorption time in S1 is 5 to 60 minutes.
[0011] In some specific embodiments of the present invention, the heating and holding process described in S2 is as follows: heating to 350-600 ℃ at a heating rate of 3-10 ℃ / min, and holding for 30-180 min.
[0012] In some specific embodiments of the present invention, the mixed solution of the alkaline oxygen system described in S3 contains NaOH and H2O2.
[0013] In some specific embodiments of the present invention, the mass fraction of NaOH in the mixed solution of the alkali-oxygen system is 1.5-10%, and the mass fraction of H2O2 in the mixed solution of the alkali-oxygen system is 1.5-7%.
[0014] In some specific embodiments of the present invention, the solid-liquid ratio of the mixed solution of the waste vanadium-tungsten-titanium SCR denitration catalyst in S1 and the alkaline oxygen-containing system in S3 is 1:(3-8)g / mL.
[0015] In some specific embodiments of the present invention, the ultrasonic reaction method is as follows: using 100-300W ultrasonic waves for 5-80 minutes for ultrasonic reaction.
[0016] The present invention also provides the application of the arsenic removal and tungsten enrichment method of the waste vanadium-tungsten-titanium SCR denitration catalyst as described in any of the preceding claims in the regeneration of the waste vanadium-tungsten-titanium SCR denitration catalyst.
[0017] The present invention has the following significant advantages and effects compared with the prior art: The present application provides a method that enhances the retention capacity of tungsten and vanadium components in the spent catalyst system of SCR denitrification catalyst through choline chloride pre-adsorption, inhibiting the migration and loss of the above-mentioned effective components in subsequent treatment processes. Subsequent nitrogen atmosphere heat treatment forms a stable carbonized modified layer on the catalyst surface, which can further protect the tungsten components. Through the combination of alkaline oxygen system and ultrasonic treatment, efficient removal of arsenic from the spent catalyst can be achieved. In addition, under the action of ultrasound, the carbonized layer formed can promote the activation of oxidant and the generation of hydroxyl radicals to a certain extent, further improving the oxidation effect in the subsequent alkaline oxygen leaching process. Detailed Implementation
[0018] This invention discloses a method for removing arsenic and enriching tungsten from waste vanadium-tungsten-titanium SCR denitration catalyst. Those skilled in the art can refer to the content of this document and appropriately modify the process parameters to achieve the desired result. It is particularly important to note that all similar substitutions and modifications are obvious to those skilled in the art and are considered to be included in this invention. The methods and applications of this invention have been described through preferred embodiments. Those skilled in the art can clearly modify or appropriately change and combine the methods and applications described herein without departing from the content, spirit, and scope of this invention to realize and apply the technology of this invention.
[0019] The following specific embodiments illustrate the solution of this application. It should be noted that these embodiments are for illustrative purposes only and should not be considered as limiting the scope of this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be obtained commercially. Example 1
[0020] Step 1: Take 8 g of waste vanadium-tungsten-titanium SCR denitration catalyst (with an As content of 0.1592 wt% and a W content of 4.0873 wt%), add it to 24 mL of 0.02 mol / L choline chloride aqueous solution, let it stand at room temperature for 10 min for adsorption, and filter to obtain the pre-adsorbed catalyst.
[0021] Step 2: Place the pre-adsorbed catalyst in a tube furnace and heat it to 420 °C at a heating rate of 3 °C / min under a nitrogen atmosphere. Hold the temperature for 10 min and allow it to cool naturally to room temperature to obtain the carbonized modified catalyst.
[0022] Step 3: Add the carbonized modified catalyst to 24 mL of a mixed solution containing 7 wt% NaOH and 5 wt% H2O2, treat it under ultrasonic assistance at 200 W for 15 min, filter it, and wash it with deionized water until the pH of the washing solution is close to 7 to obtain the arsenic-removed and tungsten-rich catalyst.
[0023] The elemental composition of the catalyst samples before and after treatment was analyzed using X-ray fluorescence spectrometry (XRF), and the mass percentages of As and W in the samples were determined. The residual As content was 0.041 wt%, and the W retention rate was 96.7%.
[0024] This application employs a process route of "choline chloride pre-adsorption - in-situ carbonization under nitrogen atmosphere - alkaline oxygen leaching". The mechanism is as follows: In the pre-adsorption stage, choline chloride preferentially adsorbs onto the surface of the spent vanadium-tungsten-titanium SCR denitrification catalyst. Through electrostatic association and phase transfer, it forms stable ion pairs or salt structures with anions such as tungstate, metavanadate, and polytungstate present in the catalyst, thereby enhancing the retention capacity of tungsten and vanadium components in the spent catalyst system and inhibiting the migration and loss of these effective components during subsequent treatment. Furthermore, this effect is mainly based on electrostatic attraction rather than chelation, thus maintaining good stability under pH conditions of 8–14. In addition, the long organic chain structure of choline chloride can also promote the retention and dispersion of tungsten and vanadium anions, reducing their tendency to migrate into the liquid phase, which is beneficial for retaining the effective components of tungsten and vanadium during the arsenic removal pretreatment process.
[0025] Secondly, in-situ carbonization via nitrogen atmosphere heat treatment causes the organic components adsorbed on the catalyst surface to undergo pyrolysis and in-situ carbonization, forming a stable carbonized modified layer on the catalyst surface. During the subsequent alkaline-oxygen leaching process, the oxidant component helps remove arsenic, while this carbonized modified layer can reduce the direct effect of the leachate on the tungsten component to a certain extent. Furthermore, under the action of an ultrasonic field, the carbonized layer can also enhance the local cavitation effect, promote the sonication of water molecules, and improve interfacial mass transfer, which helps to increase the generation of hydroxyl radicals (·OH) in the system, thereby strengthening the oxidative activation ability of H2O2 and improving the oxidative removal effect of arsenic. Therefore, the synergistic effect of arsenic removal and tungsten preservation can be further achieved in the ultrasonic field. Comparative Example 1
[0026] Take 8 g of waste vanadium-tungsten-titanium SCR denitration catalyst, add it to 24 mL of 0.02 mol / L tetramethylammonium chloride aqueous solution, let it stand at room temperature for 10 min for adsorption, and filter to obtain the pre-adsorbed catalyst; The above-mentioned pre-adsorbed catalyst was placed in a tube furnace and heated to 420 °C at a heating rate of 3 °C / min under a nitrogen atmosphere, held at that temperature for 10 min, and then naturally cooled to room temperature to obtain the carbonized modified catalyst. The carbonized modified catalyst was added to 24 mL of a mixed solution containing 7 wt% NaOH and 5 wt% H2O2, and treated with ultrasound at 200 W for 15 min. The solution was then filtered and washed with deionized water until the pH of the washing solution was close to 7 to obtain the treated sample.
[0027] Using the same detection and analysis method as in Example 1, the catalyst sample obtained in this comparative example had a residual As element content of 0.0569 wt% and a W element retention rate of 91.1%. Comparative Example 2
[0028] Take 8 g of waste vanadium-tungsten-titanium SCR denitration catalyst, add it to 24 mL of 0.02 mol / L tetramethylammonium bromide aqueous solution, let it stand at room temperature for 10 min for adsorption, and filter to obtain the pre-adsorbed catalyst; The above-mentioned pre-adsorbed catalyst was placed in a tube furnace and heated to 420 °C at a heating rate of 3 °C / min under a nitrogen atmosphere, held at that temperature for 10 min, and then naturally cooled to room temperature to obtain the carbonized modified catalyst. The above-mentioned carbonized modified catalyst was added to 24 mL of a mixed solution containing 7 wt% NaOH and 5 wt% H2O2, and treated for 15 min under ultrasonic assistance at 200 W. The solution was filtered and washed with deionized water until the pH of the washing solution was close to 7 to obtain the treated sample. Using the same detection and analysis method as in Example 1, the catalyst sample obtained in this comparative example had a residual As content of 0.0572 wt% and a W retention rate of 87.8%.
[0029] Example 1 of this application uses choline chloride as an organic protective agent. Although choline chloride may have slightly weaker initial electrostatic binding ability, its molecule contains a hydroxyethyl structure, which provides better hydrophilic dispersibility and higher effective carbon content. Under appropriate heat treatment conditions, it is easier to carbonize and form a continuous, dense amorphous carbon layer, which can more effectively coat tungsten-related species and weaken their contact with the alkaline leaching medium, thereby reducing the migration and loss of tungsten in subsequent treatment processes. In contrast, Comparative Examples 1 and 2 use common quaternary ammonium salts such as tetramethylammonium chloride and tetramethylammonium bromide as organic protective agents. These have a strong electrostatic binding ability to tungstate ions and can also play a role in protecting tungsten to some extent. However, due to the short carbon chain and few carbonizable components, it is difficult to form a stable carbon protective layer after heat treatment, resulting in a relatively poor tungsten protection effect.
[0030] Based on experimental data and considering the synergistic effect of "adsorption enrichment-pyrolysis carbonization-alkali leaching protection", the choline chloride used in this application is more suitable as an organic protective agent for the removal of arsenic and enrichment of tungsten from waste vanadium-tungsten-titanium SCR denitrification catalysts than other common low-carbon quaternary ammonium salts (tetramethylammonium chloride, tetramethylammonium bromide). Comparative Example 3
[0031] Take 8 g of waste vanadium-tungsten-titanium SCR denitration catalyst, add it to 24 mL of 0.02 mol / L choline chloride aqueous solution, let it stand at room temperature for 10 min for adsorption, and filter to obtain the pre-adsorbed catalyst.
[0032] The pre-adsorbed catalyst obtained by filtration was added to 24 mL of a mixed solution containing 7 wt% NaOH and 5 wt% H2O2, and treated with ultrasound at 200 W for 15 min. After filtration, the solution was washed with deionized water until the pH of the washing solution was close to 7, thus obtaining the arsenic-free tungsten-rich catalyst.
[0033] Using the same detection and analysis method as in Example 1, the catalyst sample obtained in this comparative example had a residual As content of 0.0682 wt% and a W retention rate of 88.3%.
[0034] Although the present invention has been described with reference to the above embodiments, it should be understood that the present invention may be further modified and varied without departing from the spirit of the present invention, and all such modifications and variations are within the protection scope of the present invention.
Claims
1. A method for removing arsenic and enriching tungsten from waste vanadium-tungsten-titanium SCR denitration catalyst, characterized in that, Includes the following steps: S1. Add the waste vanadium-tungsten-titanium SCR denitration catalyst to an aqueous solution of choline chloride, allow it to stand or shake at room temperature for adsorption, and filter to obtain the pre-adsorbed catalyst. S2. The pre-adsorbed catalyst is placed in a nitrogen atmosphere, heated and kept at that temperature, and then cooled to room temperature to obtain a carbonized modified catalyst. S3. The carbonized modified catalyst is impregnated in a mixed solution containing an alkaline oxygen system and subjected to ultrasonic reaction. After filtration and washing until neutral, an arsenic-removing and tungsten-rich catalyst is obtained.
2. The method for removing arsenic and enriching tungsten from waste vanadium-tungsten-titanium SCR denitration catalyst as described in claim 1, characterized in that, The concentration of the choline chloride aqueous solution in S1 is 0.01~0.5 mol / L.
3. The method for removing arsenic and enriching tungsten from waste vanadium-tungsten-titanium SCR denitration catalyst as described in claim 1, characterized in that, The solid-liquid ratio of the waste vanadium-tungsten-titanium SCR denitration catalyst in S1 to the aqueous choline chloride solution is 1:(2-5)g / mL.
4. The method for removing arsenic and enriching tungsten from waste vanadium-tungsten-titanium SCR denitration catalyst as described in any one of claims 1-3, characterized in that, The static or oscillating adsorption time described in S1 is 5-60 min.
5. The method for removing arsenic and enriching tungsten from waste vanadium-tungsten-titanium SCR denitration catalyst as described in claim 1, characterized in that, The heating and holding process described in S2 is as follows: heating to 350-600 ℃ at a heating rate of 3-10 ℃ / min, and holding for 30-180 min.
6. The method for removing arsenic and enriching tungsten from waste vanadium-tungsten-titanium SCR denitration catalyst as described in claim 1, characterized in that, The mixed solution of the alkaline oxygen system described in S3 contains NaOH and H2O2.
7. The method for removing arsenic and enriching tungsten from waste vanadium-tungsten-titanium SCR denitration catalyst as described in claim 6, characterized in that, The mass fraction of NaOH in the mixed solution of the alkaline oxygen system is 1.5-10%, and the mass fraction of H2O2 in the mixed solution of the alkaline oxygen system is 1.5-7%.
8. The method for removing arsenic and enriching tungsten from waste vanadium-tungsten-titanium SCR denitration catalyst as described in claim 1, characterized in that, The solid-liquid ratio of the mixed solution of the waste vanadium-tungsten-titanium SCR denitration catalyst in S1 and the alkaline oxygen-containing system in S3 is 1:(3-8)g / mL.
9. The method for removing arsenic and enriching tungsten from waste vanadium-tungsten-titanium SCR denitration catalyst as described in any one of claims 1-8, characterized in that, The ultrasonic reaction method is as follows: use 100-300W ultrasonic waves for 5-80 minutes for ultrasonic reaction.
10. The application of the method for removing arsenic and enriching tungsten from waste vanadium-tungsten-titanium SCR denitration catalyst as described in any one of claims 1-8 in the regeneration of waste vanadium-tungsten-titanium SCR denitration catalyst.