A method for graded and classified utilization of coal gasification slag
By using a graded and quality-based utilization method, the problem of low overall utilization efficiency of coal gasification slag has been solved, achieving efficient resource recovery and environmentally friendly utilization of coal gasification slag, improving the comprehensive utilization rate and reducing the production cost of building materials.
Patent Information
- Application Number
- CN202611206065.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-10
- Publication Date
- 2026-11-17
AI Technical Summary
The existing methods for utilizing coal gasification slag are inefficient, result in serious resource waste, and fail to fully consider the differences in characteristics of coal gasification slag of different particle sizes, leading to low comprehensive utilization rate and serious environmental pollution problems.
A graded and graded utilization method is adopted, including drying, grading and screening, flotation and calcination, to recover residual carbon components, prepare calcium oxide and use it for building materials, taking advantage of the characteristics of coal gasification slag of different particle sizes.
It has achieved efficient and comprehensive utilization of coal gasification slag, increasing the comprehensive utilization rate to over 95%, solving the problems of environmental pollution and resource waste, reducing the production cost of building materials, and the prepared calcium oxide is used for flue gas desulfurization and sewage treatment.
Smart Images

Figure CN123102490A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of solid waste resource utilization technology, specifically relating to a method for graded and quality-based utilization of coal gasification slag. Background Technology
[0002] Coal gasification is the leading technology in coal chemical industry, playing a vital role in the efficient and clean utilization of coal. However, some raw coal fails to be fully converted during the gasification process due to insufficient high-temperature residence time, abnormal material flow paths, and uneven temperatures within the furnace. This results in solid products rich in unburned carbon and minerals, including fine-particle fly ash and coarse-particle bottom ash (coal gasification slag).
[0003] Currently, the primary method for disposing of coal gasification slag is landfill storage. This approach not only exacerbates the depletion of land resources but also creates dual environmental pressures due to the particulate matter dispersion caused by long-term open-air accumulation. Furthermore, when coal gasification slag comes into contact with water, the heavy metals and toxic components it contains are prone to migration and release, potentially triggering a chain reaction of water and soil pollution and posing a potential risk to ecological security and public health.
[0004] Although researchers have studied the characteristics and resource utilization of coal gasification slag, most existing technologies adopt a holistic approach, failing to fully consider the significant differences in composition, structure, and performance among different particle sizes of coal gasification slag. This results in low comprehensive utilization rates and insufficient high-value utilization of coal gasification slag. For example, directly using coal gasification slag with high residual carbon content in building materials reduces the strength and durability of the materials; while mixing coal gasification slag with high calcium content with other coal gasification slag wastes valuable calcium resources.
[0005] Therefore, developing a graded and graded utilization method that can fully utilize the characteristics of coal gasification slag of different particle sizes is of great significance for improving the comprehensive utilization rate of coal gasification slag, reducing environmental pollution, and realizing resource recycling. Summary of the Invention
[0006] The technical problem to be solved by the present invention is to provide a method for graded and quality-based utilization of coal gasification slag, so as to solve the problems of low efficiency and serious resource waste in the existing overall utilization of coal gasification slag.
[0007] The technical solution adopted to achieve the above objectives is to provide a method for the graded and graded utilization of coal gasification slag, including the following steps: (1) After drying, the coal gasification slag is graded and screened to obtain coal gasification slag with particle sizes of <60 mesh, 60~200 mesh and >200 mesh respectively; (2) The coal gasification slag with a particle size of <60 mesh is subjected to flotation treatment to recover the residual carbon components; (3) Use coal gasification slag with a particle size of 60~200 mesh as raw and auxiliary materials for building materials; (4) Calcium oxide is prepared by calcining coal gasification slag with a particle size >200 mesh.
[0008] Preferably, the grading and screening process in step (1) yields coal gasification slag of <20 mesh, 20~40 mesh, 40~60 mesh, 60~80 mesh, 80~100 mesh, 100~200 mesh and >200 mesh respectively.
[0009] Preferably, the coal gasification slag is the bottom ash produced by a circulating fluidized bed coal gasification furnace.
[0010] Preferably, the drying in step (1) is carried out at room temperature, and the moisture content of the dried coal gasification slag is <0.5%.
[0011] More preferably, the moisture content of the dried coal gasification slag is 0.25%.
[0012] Preferably, in step (2), kerosene is used as the collector and pine oil is used as the frother in the flotation process; the flotation time is 5~10 min and the temperature is 20~30℃.
[0013] More preferably, the amount of kerosene used is 800~1200g / t; the amount of pine oil used is 200~300g / t; the flotation time is 7.5min; and the temperature is 25℃.
[0014] More preferably, the amount of kerosene used is 1000g / t; the amount of pine oil used is 250g / t.
[0015] Preferably, in step (3), the raw materials used as building materials include concrete additives; when coal gasification slag with a particle size of 60-200 mesh is used as a concrete additive, the mass percentage of the additive is 10-30%.
[0016] More preferably, when coal gasification slag with a particle size of 60-200 mesh is used as a concrete additive, the mass percentage of the slag is 20%.
[0017] Preferably, in step (4), the calcination heating rate is 5~10℃ / min, the calcination temperature is 800~1000℃, and the time is 1~3h.
[0018] More preferably, in step (4), the calcination treatment heating rate is 7.5℃ / min, the calcination temperature is 900℃, and the time is 2h.
[0019] The present invention also provides a system for the graded and graded utilization of coal gasification slag, comprising a drying device, a screening device, a flotation device, a calcination device and a building material mixing device connected in sequence.
[0020] The drying device includes a preheating and insulation shell, on the surface of which are connected an inlet, a temperature and humidity sensor, a diversion return air inlet, and an outlet; a feed baffle is provided at the bottom of the inlet; a dust filter is provided on the diversion return air inlet; a support tray is provided inside the preheating and insulation shell, and a ventilation device is provided at the bottom of the support tray, with air ducts and multiple ventilation openings arranged sequentially on the ventilation device; The screening device 2 is a vibrating screen, including a feed inlet and discharge outlets for each particle size on the surface of the screening device, as well as a motor, eccentric wheel and support at the bottom of the screening device; the screening device is equipped with screen fixing bars and standard screens of each grade inside the screening device. The flotation device is a flotation machine, including a collector feeder, a frother feeder, a foam scraper and a residual carbon discharge port located at the top of the flotation cell, an air blower and a bottom ash discharge port located at the bottom of the flotation cell, a circulating pump located outside the flotation cell, and a motor, agitator and a temperature control heat exchanger located inside the flotation cell. The motor is connected to the agitator, and the collector feeder is also provided with a feed inlet. The calcining device is a rotary calcining kiln, including a feed inlet, temperature sensor and discharge outlet set on the surface of the refractory insulation layer, a kiln cylinder rotation drive device and trolley set at the bottom of the refractory insulation layer, a rotary calcining kiln cylinder and segmented burners set inside the refractory insulation layer, and a cooler set on the discharge outlet. The building material mixing device is a concrete mixer, which includes a feed inlet at the top of the concrete mixer body and a discharge outlet at the bottom, a mixer inside the concrete mixer body, and a discharge valve on the discharge outlet.
[0021] The beneficial effects of the above technical solution adopted in this invention are as follows: the drying device is used for drying coal gasification slag, the feed baffle is used to control the feed speed, the multi-point ventilation port is connected to the air duct to form uniform heat exchange, the preheating and heat preservation shell is used to improve temperature stability and reduce environmental impact, the temperature and humidity sensor is used to monitor the internal state of the device, and the dust removal filter is used to dry the coal gasification slag to obtain dry coal gasification slag. The screening device is used for the graded screening of dried coal gasification slag. Each level of standard screen forms screening channels corresponding to BA1~BA7. The eccentric wheel is used to adjust the vibration amplitude. The screen fixing strip ensures that the screen is tight and prevents it from loosening. The flotation unit is used for flotation treatment to recover residual carbon components; the circulating pump is used for in-tank circulation to improve the uniformity of reagent dispersion; the blower aerator is used to form foam; and the foam scraper is used to scrape the foam to the residual carbon recovery channel. The calcination unit is used for calcination treatment to prepare calcium oxide; when coal gasification slag is used as a concrete additive, the building material mixing unit is used to mix the coal gasification slag with other building materials.
[0022] More preferably, the screening device is a standard sieve with different particle sizes.
[0023] The present invention has the following beneficial effects: (1) This invention realizes the efficient recovery and utilization of different components in coal gasification slag. The residual carbon recovered from coal gasification slag with a particle size <60 mesh can be used as fuel or gasification raw material; coal gasification slag with a particle size of 60~200 mesh can be directly used in the building materials field, which can replace part of the cement and reduce the production cost of building materials; high-purity calcium oxide products prepared from coal gasification slag with a particle size >200 mesh can be used in the fields of flue gas desulfurization and sewage treatment, realizing the high-value utilization of bottom slag.
[0024] (2) Based on the compositional and structural characteristics and thermal weight loss behavior differences of the bottom ash produced by circulating fluidized bed coal gasifiers of different particle sizes, this invention realizes graded and quality-based utilization, increases the comprehensive utilization rate of coal gasification ash to over 95%, and solves the environmental and resource waste problems caused by existing landfill disposal.
[0025] (3) The process of this invention is simple, requires no complicated modification treatment, requires little equipment investment, has low operating costs, and is easy to promote and apply in industrial applications. Attached Figure Description
[0026] Figure 1 This is an equipment diagram of the method for graded and classified utilization of coal gasification slag according to the present invention; Figure 2 A graph showing the mass percentage of coal gasification slag with different particle sizes; Figure 3 XRD patterns of coal gasification slag with different particle sizes; Figure 4 Infrared spectra of coal gasification slag with different particle sizes; Figure 5 The images show the apparent morphology of coal gasification slag with different particle sizes. Among them, (a) is a magnified view of region A in (b) at 2 μm; (b) is the apparent morphology of BA1 at 1 mm; (c) is a magnified view of region B in (b) at 2 μm; (d) is a magnified view of region A in (e) at 2 μm; (e) is the apparent morphology of BA2 at 1 mm; and (f) is the apparent morphology of region B in (e) at 2 μm. Figure 6 The images show the apparent morphology of coal gasification slag with different particle sizes; (a) shows the apparent morphology of BA3 at 2 μm; (b) shows the apparent morphology of BA3 at 300 μm; (c) shows the apparent morphology of BA4 at 2 μm; (d) shows the apparent morphology of BA4 at 300 μm; (e) shows the apparent morphology of BA5 at 2 μm; and (f) shows the apparent morphology of BA5 at 200 μm. Figure 7The images show the apparent morphology of coal gasification slag with different particle sizes; (a) shows the apparent morphology of BA6 at 2 μm; (b) shows the apparent morphology of BA6 at 200 μm; (c) shows the apparent morphology of BA7 at 2 μm; and (d) shows the apparent morphology of BA7 at 50 μm. Figure 8 TG curves of coal gasification slag with different particle sizes under an inert atmosphere; Figure 9 TG curves of coal gasification slag with different particle sizes under an oxidizing atmosphere; The components include: 1. Drying device; 2. Screening device; 3. Flotation device; 4. Calcination device; 5. Building material mixing device; 11. Feed inlet; 12. Feed baffle; 13. Supporting tray; 14. Air duct; 15. Multi-point ventilation outlet; 16. Preheating and insulation shell; 17. Temperature and humidity sensor; 18. Discharge outlet; 19. Diversion return air outlet; 110. Dust collector filter; 21. Feed inlet; 22A~22G, standard sieves of various grades; 23. Motor; 24. Eccentric wheel; 25. Support; 26. Screen fixing strip; 27A~27G, discharge outlets of various particle sizes; 31. Flotation tank; 32. Agitator; 33. 34. Circulating pump; 35. Collector feeder; 36. Foaming agent feeder; 37. Blower aerator; 38. Foam scraper; 39. Temperature control heat exchanger; 30. Residual carbon outlet; 310. Bottom ash outlet; 311. Feed inlet; 312. Motor; 41. Rotary calcining kiln; 42. Kiln rotation drive device; 43. Tractor; 44. Feed inlet; 45. Discharge outlet; 46A~46B. Segmented burners; 47. Refractory insulation layer; 48. Temperature sensor; 49. Cooler; 51. Concrete mixer body; 52. Feed inlet; 53. Agitator; 54. Discharge valve; 55. Discharge outlet. Detailed Implementation
[0027] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are only for explaining the invention and are not intended to limit the invention; that is, the described embodiments are only a part of the embodiments of this invention, and not all of them.
[0028] Therefore, the following detailed description of the embodiments of the present invention is not intended to limit the scope of the claimed invention, but merely to illustrate selected embodiments of the invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.
[0029] The features and performance of the present invention will be further described in detail below with reference to embodiments. The coal gasification slag used in this application originates from the bottom ash produced by a circulating fluidized bed coal gasification furnace in the Zhundong region of Xinjiang. The following embodiments utilize a system for the graded and graded utilization of coal gasification slag; specific equipment is described in [link to specific equipment description]. Figure 1 .
[0030] The system for graded and graded utilization of coal gasification slag includes a drying device 1, a screening device 2, a flotation device 3, a calcination device 4, and a building material mixing device 5 connected in sequence.
[0031] The drying device 1 includes a preheating and insulation shell 16, on the surface of which are connected an inlet 11, a temperature and humidity sensor 17, a diversion return air port 19, and an outlet 18; an inlet baffle 12 is provided at the bottom of the inlet 11; a dust removal filter 110 is provided on the diversion return air port 19; a support tray 13 is provided inside the preheating and insulation shell 16, and a ventilation device is provided at the bottom of the support tray 13, with an air guide duct 14 and a multi-point ventilation port 15 arranged in sequence on the ventilation device; The screening device 2 is a vibrating screen, including a feed inlet 21, discharge outlets 27A~27G for each particle size, a motor 23, an eccentric wheel 24 and a support 25 at the bottom of the screening device; the screening device is equipped with screen fixing strips 26 and standard screens 22A~22G for each particle size. The flotation device 3 is a flotation machine, including a collector feeder 34, a frother feeder 35, a foam scraper 37 and a residual carbon outlet 39 installed on the upper part of the flotation tank 31, an air blower 36 and a bottom slag outlet 310 installed at the bottom of the flotation tank 31, a circulating pump 33 installed outside the flotation tank 31, and a motor 312, an agitator 32 and a temperature control heat exchanger 38 installed inside the flotation tank 31. The motor 312 is connected to the agitator 32, and the collector feeder 34 is also provided with a feed inlet 311. The calcining device 4 is a rotary calcining kiln, including a feed inlet 44, a temperature sensor 48 and a discharge outlet 45 disposed on the surface of the refractory insulation layer 47, a kiln cylinder rotation drive device 42 and a trolley 43 disposed at the bottom of the refractory insulation layer 47, a rotary calcining kiln cylinder 41 disposed inside the refractory insulation layer 47 and segmented burners 46A~46B, and a cooler 49 disposed on the discharge outlet 45; The building material mixing device 5 is a concrete mixer, including a feed inlet 52 at the top of the concrete mixer body 51 and a discharge outlet 55 at the bottom, a mixer 53 inside the concrete mixer body 51, and a discharge valve 54 on the discharge outlet 55.
[0032] Example 1 A method for graded and differentiated utilization of coal gasification slag includes the following steps: (1) 100 kg of coal gasification slag was dried for 24 hours under air and room temperature conditions. The moisture content of the dried coal gasification slag was 0.28%. Then, it was graded and screened by a vibrating screener to obtain coal gasification slag with 7 different particle sizes, specifically: <20 mesh coal gasification slag (BA1) 23.23 kg, 20~40 mesh coal gasification slag (BA2) 4.02 kg, 40~60 mesh coal gasification slag (BA3) 5.36 kg, 60~80 mesh coal gasification slag (BA4) 42.70 kg, 80~100 mesh coal gasification slag (BA5) 17.56 kg, 100~200 mesh coal gasification slag (BA6) 6.45 kg, and >200 mesh coal gasification slag (BA7) 0.35 kg. (2) 32.61 kg of coal gasification slag (BA1~BA3) with a particle size <60 mesh (carbon content 3.5%) was added to a flotation machine. 800 g / t of kerosene was added as a collector and 200 g / t of pine oil was added as a frother for flotation treatment. The flotation temperature was 20℃ and the time was 10 min. 1.02 kg of residual carbon component was recovered, and the residual carbon recovery rate was 89.47%. (3) 66.71 kg of coal gasification slag (BA4~BA6) with a particle size of 60~200 mesh was directly added to the concrete mixer as a concrete additive, accounting for 10% of the mass of the concrete; (4) Place 0.35 kg of coal gasification slag (BA7) with a particle size > 200 mesh in a rotary kiln, raise the temperature to 800°C at a heating rate of 5°C / min, calcine for 3 hours, and cool to room temperature to obtain 0.29 kg of calcium oxide with a purity of 92.3%.
[0033] Example 2 A method for graded and differentiated utilization of coal gasification slag includes the following steps: (1) 100 kg of coal gasification slag was dried for 24 hours under air and room temperature conditions. The moisture content of the dried coal gasification slag was 0.32%. Then, it was graded and screened by a vibrating screener to obtain 7 coal gasification slags with different particle sizes, specifically: <20 mesh coal gasification slag (BA1) 22.56 kg, 20~40 mesh coal gasification slag (BA2) 4.15 kg, 40~60 mesh coal gasification slag (BA3) 5.67 kg, 60~80 mesh coal gasification slag (BA4) 43.18 kg, 80~100 mesh coal gasification slag (BA5) 17.57 kg, 100~200 mesh coal gasification slag (BA6) 5.72 kg, and >200 mesh coal gasification slag (BA7) 0.58 kg. (2) 32.38 kg of coal gasification slag (BA1~BA3) with a particle size <60 mesh (carbon content 3.5%) was added to a flotation machine. 1200 g / t of kerosene was added as a collector and 300 g / t of pine oil was added as a frother for flotation treatment. The flotation temperature was 30℃ and the time was 5 min. 1.01 kg of residual carbon component was recovered, and the residual carbon recovery rate was 89.14%. (3) 66.47 kg of coal gasification slag (BA4~BA6) with a particle size of 60~200 mesh was directly added to the concrete mixer as a concrete additive, accounting for 30% of the mass of the concrete; (4) Place 0.58 kg of coal gasification slag (BA7) with a particle size > 200 mesh in a rotary kiln, raise the temperature to 1000℃ at a heating rate of 10℃ / min, calcine for 1 h, and cool to room temperature to obtain 0.31 kg of calcium oxide with a purity of 95.6%.
[0034] Example 3 A method for graded and differentiated utilization of coal gasification slag includes the following steps: (1) 100 kg of coal gasification slag was dried in air and at room temperature for 24 hours. The moisture content of the dried coal gasification slag was 0.25%. Then, it was graded and screened by a vibrating screener to obtain coal gasification slag with 7 different particle sizes, specifically: <20 mesh coal gasification slag (BA1) 23.48 kg, 20~40 mesh coal gasification slag (BA2) 4.86 kg, 40~60 mesh coal gasification slag (BA3) 5.02 kg, 60~80 mesh coal gasification slag (BA4) 42.67 kg, 80~100 mesh coal gasification slag (BA5) 17.75 kg, 100~200 mesh coal gasification slag (BA6) 5.82 kg, and >200 mesh coal gasification slag (BA7) 0.35 kg. (2) 33.36 kg of coal gasification slag (BA1~BA3) with a particle size <60 mesh (carbon content 3.5%) was added to a flotation machine. 1000 g / t of kerosene was added as a collector and 250 g / t of pine oil was added as a frother for flotation treatment. The flotation temperature was 25℃ and the time was 7.5 min. 1.05 kg of residual carbon component was recovered, and the residual carbon recovery rate was 89.74%. (3) Add 66.24 kg of coal gasification slag (BA4~BA6) with a particle size of 60~200 mesh directly to the concrete mixer as a concrete additive, accounting for 20% of the mass of the concrete; (4) Place 0.35 kg of coal gasification slag (BA7) with a particle size > 200 mesh in a rotary kiln, raise the temperature to 900°C at a heating rate of 7.5°C / min, calcine for 2 hours, and cool to room temperature to obtain 0.30 kg of calcium oxide with a purity of 94.1%.
[0035] The flowchart of the method for graded and classified utilization of coal gasification slag of this invention is as follows: Figure 1 .
[0036] Comparative Example 1 A method for graded and graded utilization of coal gasification slag, compared with Example 3, does not perform grading and screening treatment, but directly uses 100kg of coal gasification slag as a concrete additive, with a mass percentage of 20% in the concrete.
[0037] Comparative Example 2 A method for classifying and utilizing coal gasification slag, compared with Example 3, does not perform classification and screening. Instead, 100 kg of coal gasification slag is directly added to a flotation machine, 1000 g / t of kerosene is added as a collector, and 250 g / t of pine oil is added as a frother for flotation treatment. The flotation temperature is 25°C and the time is 7.5 min.
[0038] Comparative Example 3 A method for graded and graded utilization of coal gasification slag, compared with Example 3, does not perform graded screening treatment, but directly places 100kg of coal gasification slag in a rotary kiln, raises the temperature to 900℃ at a heating rate of 7.5℃ / min, and calcines for 2h.
[0039] Example 1: Characterization and Analysis of Coal Gasification Slag 1.1 Quality Proportion Analysis To illustrate the mass distribution of coal gasification slag with different particle sizes, 100g of coal gasification slag was weighed, dried, and sieved using a small laboratory mesh sieve according to the particle size specified in Example 3. The sieved slag was then weighed, and the mass percentage of bottom slag with different particle sizes was calculated. The results are as follows: Figure 2 As shown.
[0040] from Figure 2 As can be seen, the particle size distribution of BA exhibits significant non-uniformity. Large particles (BA1, BA2) account for 27.87% of the total mass, while small particles (BA3~BA6) account for the highest proportion at 71.75%, and powder (BA7) accounts for only 0.38%.
[0041] 1.2 Characterization Analysis The seven coal gasification slags with different particle sizes obtained after grading and sieving in step (1) of Example 3 were subjected to industrial analysis, ash analysis, XRD analysis, infrared spectroscopy analysis, morphological characterization and thermogravimetric analysis.
[0042] 1.2.1 Industrial Analysis According to the testing specifications of the national standard GB / T 212-2008, the moisture, ash and volatile matter contents of BA samples were determined, and the fixed carbon content was calculated by the difference method. The results are shown in Table 1.
[0043] Table 1. Industrial Analysis Results of Coal Gasification Slag
[0044] Note: M ad : Moisture (air-dried basis) mass percentage; A ad Ash content (dry basis) as a percentage by mass; VM ad : Percentage of volatile substances by mass; FC ad : Percentage of fixed carbon by mass.
[0045] from Figure 1 The results show that BA1 has the highest fixed carbon content, at 3.68%; the ash content of BA4 to BA6 is all greater than 100%, which is due to the oxidation reaction of some metal elements during the roasting process, which leads to an increase in the oxygen content in the sample; BA7 has the highest volatile matter content, at 17.82%.
[0046] 1.2.2 Ash content analysis The gray composition of the samples was analyzed by X-ray fluorescence spectrometry (XRF, Thermo Scientific ARL Perform'X, USA). The test method was pellet method, and the results are presented in the form of oxides. The results are shown in Table 2.
[0047] Table 2 Ash content analysis results of coal gasification slag
[0048] Note: All values in the table are percentages by mass. As can be seen from the results in Table 2, the coal gasification slag of different particle sizes is mainly composed of five elements: Si, Al, Fe, Ca, and Mg, with the sum of their contents all exceeding 85%. Among them, the calcium oxide content in BA7 is as high as 85.82%, indicating that the Ca element in the bottom slag is mainly enriched in the fine powder particles.
[0049] 1.2.3 XRD Analysis The samples were examined using a Bruker D8 ADVANCE X-ray diffractometer (Germany) at 40 kV and 40 mA. The diffractometer was equipped with a Cu Kα radiation source (wavelength λ = 1.5406), and the scanning range was set to 5–80 ° with a scanning rate of 0.02 ° / min. The results are as follows: Figure 3 As shown.
[0050] from Figure 3 As can be seen, BA1 contains crystalline phase components mainly composed of quartz or aluminosilicates; BA2 to BA6 have low contents of crystalline structural components and are mainly composed of amorphous inorganic components; BA7 has obvious Ca(OH)2 characteristic diffraction peaks.
[0051] 1.2.4 Infrared Spectroscopy Analysis The study used a Bruker EQUINOX-55 Fourier transform infrared spectrometer (resolution 0.4 cm⁻¹). -1 Wavenumber accuracy 0.01 cm -1 The sample was analyzed. At room temperature, the sample was mixed with spectrally pure KBr at a mass ratio of 1:100, ground, compressed into a pellet, and placed in a sample chamber at 500-4000 cm⁻¹. -1 The measurement was performed within the specified range. Results are as follows: Figure 4 As shown.
[0052] from Figure 4 As can be seen from this, 3644 cm -1 The -OH stretching peak (Ca(OH)2) indicates that Ca mainly exists as Ca(OH)2; 1630 cm⁻¹ -1 The peak at 1020 cm⁻¹ is related to C=O. -1 and 920 / 844 / 515 / 458 cm -1 Reflecting the structure of aluminosilicates and quartz; BA7 at 1467, 1415, and 873 cm⁻¹ -1 The characteristic peak of CaCO3 appears.
[0053] 1.2.5 Morphological Characterization Scanning electron microscopy (SEM) was used to analyze the surface of the samples, and to explore the similarities and differences in the surface characteristics of coal gasification slag of different particle sizes and their variation patterns. SEM images were obtained under the test conditions of 10 kV acceleration voltage and InLens signal.
[0054] The results are as follows Figures 5-7 As shown, BA1 and BA2 exhibit irregular shapes, BA3 to BA6 are spherical particles, and BA7 is a flocculent powder. This is due to the turbulence and surface tension during the gasification process.
[0055] 1.2.6 Thermogravimetric Analysis Using a STA 2500 / Hitachi TG / DTA7300 thermogravimetric analyzer, high-purity nitrogen was selected as the inert carrier gas and air as the oxidizing carrier gas. The samples were heated from room temperature to 1000 °C at a heating rate of 10 °C / min to systematically study their thermogravimetric behavior. The results are as follows: Figures 8-9 As shown.
[0056] from Figures 8-9 As can be seen, under an inert atmosphere, the weight loss rates of BA1 and BA7 were 2.87% and 18.20%, respectively, indicating poor thermal stability; BA4 to BA6 showed low weight loss rates and high thermal stability. Under an oxidizing atmosphere, the weight loss rates of BA1 and BA7 were 10.58% and 18.24%, respectively; BA4 to BA6 showed almost no weight loss and extremely low loss on ignition.
[0057] Experiment Example 2 Performance Evaluation The various products obtained by the methods of Example 3 and Comparative Examples 1-3 were evaluated, and the results are shown in Table 3. The concrete used in the concrete compressive strength test was prepared with PO 42.5 cement, manufactured sand, and continuously graded crushed stone with a particle size of 5-31.5 mm in a mass ratio of 1:1.5:3. The concrete compressive strength was tested using the methods in GB / T 50081-2019 "Standard for Test Methods of Physical and Mechanical Properties of Concrete".
[0058] Table 3 Comparison of product performance under different process conditions
[0059] As shown in Table 1, the comprehensive utilization rate of the bottom slag in Example 3 of this invention is as high as 95.2%, which is much higher than that of Comparative Examples 2 and 3. Compared with Comparative Example 1, the concrete prepared by this invention has higher compressive strength because the bottom slag of BA4~BA6 has high ash content, good thermal stability, and does not contain high residual carbon components, thus not adversely affecting the strength and durability of the concrete. Compared with Comparative Example 3, the calcium oxide product prepared by this invention has higher purity because the calcium oxide content in the bottom slag of BA7 is as high as 85.82%, and a high-purity calcium oxide product can be obtained through simple calcination.
[0060] The present invention has been described according to the above embodiments. It should be understood that the above embodiments do not limit the present invention in any way. All technical solutions obtained by equivalent substitution or equivalent transformation fall within the scope of the present invention.
Claims
1. A method for graded and differentiated utilization of coal gasification slag, characterized in that, Includes the following steps: (1) After drying, the coal gasification slag is graded and screened to obtain coal gasification slag with particle sizes of <60 mesh, 60~200 mesh and >200 mesh respectively; (2) The coal gasification slag with a particle size of <60 mesh is subjected to flotation treatment to recover the residual carbon components; (3) Use coal gasification slag with a particle size of 60~200 mesh as raw and auxiliary materials for building materials; (4) Calcium oxide is prepared by calcining coal gasification slag with a particle size >200 mesh.
2. The method for graded and differentiated utilization of coal gasification slag as described in claim 1, characterized in that, The coal gasification slag is the bottom ash produced by a circulating fluidized bed coal gasifier.
3. The method for graded and differentiated utilization of coal gasification slag as described in claim 1, characterized in that, In step (1), the drying is carried out at room temperature, and the moisture content of the dried coal gasification slag is <0.5%.
4. The method for graded and differentiated utilization of coal gasification slag as described in claim 3, characterized in that, The moisture content of the dried coal gasification slag is 0.25%.
5. The method for graded and differentiated utilization of coal gasification slag as described in claim 1, characterized in that, In step (2), kerosene is used as the collector and pine oil is used as the frother in the flotation process; the flotation time is 5-10 min and the temperature is 20-30℃.
6. The method for graded and differentiated utilization of coal gasification slag as described in claim 5, characterized in that, The amount of kerosene used is 800~1200g / t; the amount of pine oil used is 200~300g / t; the flotation time is 7.5min and the temperature is 25℃.
7. The method for graded and differentiated utilization of coal gasification slag as described in claim 1, characterized in that, In step (3), the raw materials used as building materials include concrete additives; when the coal gasification slag with a particle size of 60~200 mesh is used as a concrete additive, the mass percentage of the additive is 10~30%.
8. The method for graded and classified utilization of coal gasification slag as described in claim 7, characterized in that, When the coal gasification slag with a particle size of 60-200 mesh is used as a concrete additive, the mass percentage of the slag is 20%.
9. The method for graded and classified utilization of coal gasification slag as described in claim 1, characterized in that, In step (4), the calcination treatment has a heating rate of 5~10℃ / min, a calcination temperature of 800~1000℃, and a time of 1~3h.