A method for applying epoxy self-coating primer to transformer plate heat sinks
By using an epoxy self-electrophoretic primer method, combined with shot blasting or zinc phosphate phosphating processes and overhead chain hoist dip coating technology, the problem of insufficient powder coating penetration in transformer finned radiator powder coating was solved, achieving efficient corrosion protection and low-cost production.
Patent Information
- Application Number
- CN202611209322.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-11
- Publication Date
- 2026-11-17
AI Technical Summary
Existing powder coating for transformer finned radiators has problems such as powder not being able to penetrate the gaps between reinforcing ribs, leading to rust, yellow water flow, and oil leakage in the gaps. In addition, electrophoresis or hot-dip galvanizing equipment is expensive, and construction costs and energy consumption are high.
The epoxy self-electrophoretic primer method is adopted, including pretreatment, pre-drying, dip coating of HD-147 epoxy self-electrophoretic primer and electrostatic powder coating. The surface is prepared by shot blasting or zinc phosphate process, combined with suspension hoist dip coating and high temperature drying technology to ensure the coating's penetration and anti-corrosion ability.
It improves the corrosion resistance of transformer finned radiators, reduces production costs and energy waste, solves the problem of incomplete coating in the gaps of powder coating reinforcing ribs, and enhances the corrosion resistance of weak points in the equipment.
Abstract
Description
Technical Field
[0001] This invention relates to the field of anti-corrosion coating technology for non-galvanized transformer finned radiators, specifically to a method for applying an epoxy self-electrophoretic primer to transformer finned radiators. Background Technology
[0002] There are three main types of powder coating for existing transformer finned heat sinks.
[0003] 1. Direct pretreatment (shot blasting or pickling and phosphating) followed by electrostatic powder coating (direct spraying of polyester powder or epoxy base powder plus polyester powder). 2. Electrophoresis followed by electrostatic powder coating (direct spraying of polyester powder or epoxy base powder plus polyester powder). 3. Electrostatic powder coating after hot-dip galvanizing (directly spraying polyester powder or epoxy base powder plus polyester powder). This application addresses the problems and shortcomings of traditional processes: 1. This solves the problem that in direct powder coating, the powder cannot penetrate the gaps between reinforcing ribs, resulting in incomplete sealing and coating, leading to rust, yellow water leakage, and oil leakage in the gaps.
[0004] 2. Solve the problems of high equipment costs, construction costs, and energy consumption associated with electrophoresis or hot-dip galvanizing. Summary of the Invention
[0005] To overcome the shortcomings and deficiencies of existing technologies, the present invention aims to provide a method for applying an epoxy self-coating primer to transformer finned radiators. This method solves the problems of missed coating in the reinforcing rib seams of transformer finned radiators during powder coating, and the high cost of applying powder coating after electrophoresis and hot-dip galvanizing. It effectively improves the corrosion resistance of transformer finned radiators, reduces production costs, and minimizes energy waste.
[0006] The objective of this invention is achieved through the following technical solution: a method for applying an epoxy self-coating primer to a transformer plate heat sink, comprising the following steps: (1) Pretreatment: The surface of the radiator is free of oil stains and other contaminants, and free of oxide scale, yellow rust, etc.; (2) Pre-drying: Thoroughly remove moisture from the weld to fundamentally eliminate shrinkage cavities, pinholes, and fish eyes; hot air drying, 50-60℃ wind box drying for 1 hour; (3) Dip coating HD-147 epoxy self-electrophoretic primer; The workpiece is transported by a suspension hoist and a transfer line by dipping. The viscosity of HD-147 epoxy self-electrophoretic primer is adjusted to 19-23S with thinner. The workpiece is transported to the position of HD-147 epoxy self-electrophoretic primer tool and immersed in HD-147 epoxy self-electrophoretic primer tool. One layer of HD-147 epoxy self-electrophoretic primer is dipped on the surface of the workpiece. After immersion for 8-12 minutes, the oil droplets on the surface of the workpiece are cleaned with a roller soaked in thinner. The surface of the workpiece is allowed to dry naturally for 1 hour and then dried at 150-180℃ for 30-15 minutes. (4) Electrostatic spraying of powder coating: After drying, the workpiece is transferred to the spray booth. The humidity of the spray booth is controlled at 40%-70%, and the temperature is controlled at 18-30℃. HD-1001 epoxy conductive base powder, JM-2005 conductive intermediate powder, or JM-5001 high weather-resistant polyester powder are applied by manual or automatic electrostatic spraying. The high temperature is maintained at 180-200℃ for 15-25 minutes.
[0007] As an improvement to the epoxy self-electrophoretic primer method for transformer plate heat sinks of the present invention: the pretreatment in step (1) is shot blasting or zinc phosphate phosphating; The shot blasting process steps are as follows: a. Pre-treatment: The exterior of the workpiece is cleaned by manual grinding to remove welding slag, spatter, sharp corners and weld beads, and the oil outlet of the workpiece is sealed. b. Degreasing: Use high-temperature degreasing or alkaline spraying to remove oil stains from the surface of the workpiece; c. Suspended loading: The workpiece is suspended by a hanger and fed into the shot blasting machine for automatic shot blasting. d. Automatic shot blasting: Steel shot, ceramic shot or other particles with a diameter of 0.2-3.0 mm are shot at high speed onto the surface of the workpiece through a shot blasting machine. The impact and abrasion action are used to clean the oxide scale, rust, welding slag and other impurities on the surface of the workpiece. At the same time, the stress state of the workpiece surface is changed, and the fatigue strength and coating adhesion of the workpiece are improved. e. Shot blasting effect test: Test the removal effect of impurities such as oxide scale, rust, and welding slag on the surface of the workpiece. If the result is qualified, it will proceed to the next process. The zinc phosphating process steps are as follows: a. Pre-inspection of the material before loading, and cleaning of the workpiece surface to remove welding slag, spatter, sharp corners and weld beads; b. Pre-degreasing: 3% alkaline degreasing agent, total alkalinity 20-28pt, temperature 50-55℃, spray pressure 0.18-0.22MPa, to remove thick oil and dust from the surface of the workpiece by spraying. c. Main degreasing: Temperature 50-60℃, soak in alkaline washing tank for 5-8 minutes, stir at the bottom, alkalinity 25-35pt, skim off the floating oil on the liquid surface at regular intervals, and the water film on the surface of the workpiece after washing is continuous and unbroken. If the water film does not break within 30 seconds, the degreasing is considered successful. d. First bipolar water wash; e. Pickling to remove rust; f. Second bipolar water wash; g. Neutralization: This is done in a phosphoric acid solution tank. The phosphoric acid in the tank is 8-12 ml / L industrial phosphoric acid with a pH of 4.0-5.0 and a temperature of 20-25℃. Soak for 60-90 seconds. After neutralization, rinse the workpiece with running tap water for 30-60 seconds. The pH of the tap water is 6-7. Rinse until there are no white alkali marks or soap residues on the surface of the workpiece. h. Surface conditioning; This is done in a titanium-based surface conditioning solution bath with a pH value of 8.0-9.5. Immerse in the titanium-based surface conditioning solution bath at room temperature for 30-60 seconds. i. Phosphating; j. Third bipolar water wash.
[0008] As an improvement to the epoxy self-coating primer method for transformer plate heat sinks of the present invention: the selection of powder coating in step (4) is configured according to the anti-corrosion level and required thickness of the workpiece; To meet the C3M anti-corrosion requirements, spray 80-90um of JM-5001 high weather-resistant polyester powder, HD-147 epoxy self-electrophoretic primer with a thickness of 20-30um, and the total thickness of HD-147 epoxy self-electrophoretic primer and JM-5001 high weather-resistant polyester powder is 100-120um. To meet the C4M anti-corrosion requirements, spray 130-150um of JM-5001 high weather-resistant polyester powder, HD-147 epoxy self-electrophoretic primer thickness is 20-30um, and the total thickness of HD-147 epoxy self-electrophoretic primer and JM-5001 high weather-resistant polyester powder is 150-180um. To meet the C5M anti-corrosion requirements, spray 100-130um of JM-5001 high weather-resistant polyester powder and 80-100um of JM-2005 conductive intermediate powder, and the thickness of HD-147 epoxy self-electrophoretic primer is 20-30um. The total thickness of HD-147 epoxy self-electrophoretic primer, JM-5001 high weather-resistant polyester powder and JM-2005 conductive intermediate powder is 200-260um.
[0009] The beneficial effects of this invention are as follows: This invention solves the current problems of missed coating in the reinforcing rib seams of transformer radiator powder coating, and the high cost of powder coating after electrophoresis and hot-dip galvanizing. It effectively improves the corrosion resistance of transformer radiator powder coating, reduces production costs, and minimizes energy waste. The coating scheme of HD-147 epoxy self-coating primer with matching powder completely solves the problem of missed coating, greatly improving the corrosion resistance of weak points in transformer radiator powder coating; HD-147 epoxy self-coating primer requires low equipment investment and does not cause additional energy consumption during production. Detailed Implementation
[0010] To facilitate understanding by those skilled in the art, the present invention will be further described below with reference to embodiments. The content mentioned in the embodiments is not intended to limit the present invention.
[0011] Example 1
[0012] A method for applying an epoxy self-coating primer to a transformer plate heat sink includes the following steps: (1) Pretreatment: The surface of the radiator is free of oil and other contaminants, and free of oxide scale, yellow rust, etc.; the pretreatment adopts shot blasting process. The shot blasting process steps are as follows: a. Pre-treatment: The exterior of the workpiece is cleaned by manual grinding to remove welding slag, spatter, sharp corners and weld beads, and the oil outlet of the workpiece is sealed. b. Degreasing: Use high-temperature degreasing or alkaline spraying to remove oil stains from the surface of the workpiece; c. Suspended loading: The workpiece is suspended by a hanger and fed into the shot blasting machine for automatic shot blasting. d. Automatic shot blasting: Steel shot, ceramic shot or other particles with a diameter of 0.2-3.0 mm are shot at high speed onto the surface of the workpiece through a shot blasting machine. The impact and abrasion action are used to clean the oxide scale, rust, welding slag and other impurities on the surface of the workpiece. At the same time, the stress state of the workpiece surface is changed, and the fatigue strength and coating adhesion of the workpiece are improved. e. Shot blasting effect test: Test the removal effect of impurities such as oxide scale, rust, and welding slag on the surface of the workpiece. If the result is qualified, it will proceed to the next process. (2) Pre-drying: Thoroughly remove moisture from the weld to fundamentally eliminate shrinkage cavities, pinholes, and fish eyes; hot air drying, 50-60℃ wind box drying for 1 hour; (3) Dip coating HD-147 epoxy self-electrophoretic primer; The workpiece is transported by a suspension hoist and a transfer line by dipping. The viscosity of HD-147 epoxy self-electrophoretic primer is adjusted to 19-23S with thinner. The workpiece is transported to the position of HD-147 epoxy self-electrophoretic primer tool and immersed in HD-147 epoxy self-electrophoretic primer tool. One layer of HD-147 epoxy self-electrophoretic primer is dipped on the surface of the workpiece. After immersion for 8-12 minutes, the oil droplets on the surface of the workpiece are cleaned with a roller soaked in thinner. The surface of the workpiece is allowed to dry naturally for 1 hour and then dried at 150-180℃ for 30-15 minutes. (4) Electrostatic powder coating; after drying, the workpiece is transferred to the spray booth, the humidity of the spray booth is controlled at 40%-70%, the temperature is controlled at 18-30℃, manual or automatic electrostatic spraying is used, and after spraying, the workpiece is kept at a high temperature of 180-200℃ for 15-25 minutes. The selection of powder coatings is based on the corrosion resistance level and required thickness of the workpiece; To meet the C3M anti-corrosion requirements, spray 80-90um of JM-5001 high weather-resistant polyester powder, HD-147 epoxy self-electrophoretic primer with a thickness of 20-30um, and the total thickness of HD-147 epoxy self-electrophoretic primer and JM-5001 high weather-resistant polyester powder is 100-120um. To meet the C4M anti-corrosion requirements, spray 130-150um of JM-5001 high weather-resistant polyester powder, HD-147 epoxy self-electrophoretic primer thickness is 20-30um, and the total thickness of HD-147 epoxy self-electrophoretic primer and JM-5001 high weather-resistant polyester powder is 150-180um. To meet the C5M anti-corrosion requirements, spray 100-130um of JM-5001 high weather-resistant polyester powder and 80-100um of JM-2005 conductive intermediate powder, and the thickness of HD-147 epoxy self-electrophoretic primer is 20-30um. The total thickness of HD-147 epoxy self-electrophoretic primer, JM-5001 high weather-resistant polyester powder and JM-2005 conductive intermediate powder is 200-260um.
[0013] Example 2
[0014] A method for applying an epoxy self-coating primer to a transformer plate heat sink includes the following steps: (1) Pretreatment: The surface of the radiator is free of oil and other contaminants, and free of oxide scale, yellow rust, etc.; the pretreatment adopts the zinc phosphate process. The zinc phosphate phosphating process steps are as follows: a. Pre-inspection of the material before loading, and cleaning of the workpiece surface to remove welding slag, spatter, sharp corners and weld beads; b. Pre-degreasing: 3% alkaline degreasing agent, total alkalinity 20-28pt, temperature 50-55℃, spray pressure 0.18-0.22MPa, to remove thick oil and dust from the surface of the workpiece by spraying. c. Main degreasing: Temperature 50-60℃, soak in alkaline washing tank for 5-8 minutes, stir at the bottom, alkalinity 25-35pt, skim off the floating oil on the liquid surface at regular intervals, and the water film on the surface of the workpiece after washing is continuous and unbroken. If the water film does not break within 30 seconds, the degreasing is considered successful. d. First bipolar water wash; e. Pickling to remove rust; f. Second bipolar water wash; g. Neutralization: This is done in a phosphoric acid solution tank. The phosphoric acid in the tank is 8-12 ml / L industrial phosphoric acid with a pH of 4.0-5.0 and a temperature of 20-25℃. Soak for 60-90 seconds. After neutralization, rinse the workpiece with running tap water for 30-60 seconds. The pH of the tap water is 6-7. Rinse until there are no white alkali marks or soap residues on the surface of the workpiece. h. Surface conditioning; This is done in a titanium-based surface conditioning solution bath with a pH value of 8.0-9.5. Immerse in the titanium-based surface conditioning solution bath at room temperature for 30-60 seconds. i. Phosphating; j. Third bipolar water wash; after water wash, proceed to the next process; (2) Pre-drying: Thoroughly remove moisture from the weld to fundamentally eliminate shrinkage cavities, pinholes, and fish eyes; hot air drying, 50-60℃ wind box drying for 1 hour; (3) Dip coating HD-147 epoxy self-electrophoretic primer; The workpiece is transported by a suspension hoist and a transfer line by dipping. The viscosity of HD-147 epoxy self-electrophoretic primer is adjusted to 19-23S with thinner. The workpiece is transported to the position of HD-147 epoxy self-electrophoretic primer tool and immersed in HD-147 epoxy self-electrophoretic primer tool. One layer of HD-147 epoxy self-electrophoretic primer is dipped on the surface of the workpiece. After immersion for 8-12 minutes, the oil droplets on the surface of the workpiece are cleaned with a roller soaked in thinner. The surface of the workpiece is allowed to dry naturally for 1 hour and then dried at 150-180℃ for 30-15 minutes. (4) Electrostatic powder coating; after drying, the workpiece is transferred to the spray booth, the humidity of the spray booth is controlled at 40%-70%, the temperature is controlled at 18-30℃, manual or automatic electrostatic spraying is used, and after spraying, the workpiece is kept at a high temperature of 180-200℃ for 15-25 minutes. The selection of powder coatings is based on the corrosion resistance level and required thickness of the workpiece; To meet the C3M anti-corrosion requirements, spray 80-90um of JM-5001 high weather-resistant polyester powder, HD-147 epoxy self-electrophoretic primer with a thickness of 20-30um, and the total thickness of HD-147 epoxy self-electrophoretic primer and JM-5001 high weather-resistant polyester powder is 100-120um. To meet the C4M anti-corrosion requirements, spray 130-150um of JM-5001 high weather-resistant polyester powder, HD-147 epoxy self-electrophoretic primer thickness is 20-30um, and the total thickness of HD-147 epoxy self-electrophoretic primer and JM-5001 high weather-resistant polyester powder is 150-180um. To meet the C5M anti-corrosion requirements, spray 100-130um of JM-5001 high weather-resistant polyester powder and 80-100um of JM-2005 conductive intermediate powder, and the thickness of HD-147 epoxy self-electrophoretic primer is 20-30um. The total thickness of HD-147 epoxy self-electrophoretic primer, JM-5001 high weather-resistant polyester powder and JM-2005 conductive intermediate powder is 200-260um.
[0015] The above embodiments are preferred implementations of the present invention. In addition, the present invention can be implemented in other ways. Any obvious substitutions without departing from the concept of the present invention are within the protection scope of the present invention.
Claims
1. A method for applying an epoxy self-coating primer to a transformer finned radiator, characterized in that: Includes the following steps: (1) Pretreatment: The surface of the radiator is free of oil and other contaminants, and free of oxide scale and yellow rust; (2) Pre-drying: Thoroughly remove moisture from the weld seam to eliminate shrinkage cavities, pinholes, and fish eyes; hot air drying, 50-60℃ air box drying for 1 hour; (3) Dip coating HD-147 epoxy self-electrophoretic primer; The workpiece is transported by a suspension hoist and a transfer line by dipping. The viscosity of HD-147 epoxy self-electrophoretic primer is adjusted to 19-23S with thinner. The workpiece is transported to the position of HD-147 epoxy self-electrophoretic primer tool and immersed in HD-147 epoxy self-electrophoretic primer tool. One layer of HD-147 epoxy self-electrophoretic primer is dipped on the surface of the workpiece. After immersion for 8-12 minutes, the oil droplets on the surface of the workpiece are cleaned with a roller soaked in thinner. The surface of the workpiece is allowed to dry naturally for 1 hour and then dried at 150-180℃ for 30-15 minutes. (4) Electrostatic spraying of powder coating: After drying, the workpiece is transferred to the spray booth. The humidity of the spray booth is controlled at 40%-70%, and the temperature is controlled at 18-30℃. HD-1001 epoxy conductive base powder, JM-2005 conductive intermediate powder, or JM-5001 high weather-resistant polyester powder are applied by manual or automatic electrostatic spraying. The high temperature is maintained at 180-200℃ for 15-25 minutes.
2. The method for applying an epoxy self-coating primer to a transformer finned radiator according to claim 1, characterized in that: The pretreatment described in step (1) is shot blasting or zinc phosphating; The shot blasting process steps are as follows: a. Pre-treatment: The exterior of the workpiece is cleaned by manual grinding to remove welding slag, spatter, sharp corners and weld beads, and the oil outlet of the workpiece is sealed. b. Degreasing: Use high-temperature degreasing or alkaline spraying to remove oil stains from the surface of the workpiece; c. Suspended loading: The workpiece is suspended by a hanger and fed into the shot blasting machine for automatic shot blasting. d. Automatic shot blasting: Steel shot, ceramic shot or other particles with a diameter of 0.2-3.0 mm are shot at high speed onto the surface of the workpiece through a shot blasting machine. The impact and abrasion action are used to clean the oxide scale, rust, welding slag and other impurities on the surface of the workpiece. At the same time, the stress state of the workpiece surface is changed, and the fatigue strength and coating adhesion of the workpiece are improved. e. Shot blasting effect test: Test the removal effect of impurities such as oxide scale, rust, and welding slag on the surface of the workpiece. If the result is qualified, it will proceed to the next process. The zinc phosphating process steps are as follows: a. Pre-inspection of the material before loading, and cleaning of the workpiece surface to remove welding slag, spatter, sharp corners and weld beads; b. Pre-degreasing: 3% alkaline degreasing agent, total alkalinity 20-28pt, temperature 50-55℃, spray pressure 0.18-0.22MPa, to remove thick oil and dust from the surface of the workpiece by spraying. c. Main degreasing: Temperature 50-60℃, soak in alkaline washing tank for 5-8 minutes, stir at the bottom, alkalinity 25-35pt, skim off the floating oil on the liquid surface at regular intervals, and the water film on the surface of the workpiece after washing is continuous and unbroken. If the water film does not break within 30 seconds, the degreasing is considered successful. d. First bipolar water wash; e. Pickling to remove rust; f. Second bipolar water wash; g. Neutralization; The process is completed in a phosphoric acid solution tank with 8-12 ml / L industrial phosphoric acid, pH 4.0-5.0, and a phosphoric acid temperature of 20-25℃. The soaking time is 60-90 seconds. After neutralization, the workpiece is rinsed with running tap water for 30-60 seconds with a pH of 6-7 until there are no white alkali marks or soap residues on the surface of the workpiece. h. Surface conditioning; This is done in a titanium-based surface conditioning solution bath with a pH value of 8.0-9.
5. Immerse in the titanium-based surface conditioning solution bath at room temperature for 30-60 seconds. i. Phosphating; j. Third bipolar water wash.
3. The method for applying an epoxy self-coating primer to a transformer finned radiator according to claim 1, characterized in that: The selection of powder coating in step (4) is based on the corrosion resistance level and required thickness of the workpiece; To meet the C3M anti-corrosion requirements, spray 80-90um of JM-5001 high weather-resistant polyester powder, HD-147 epoxy self-electrophoretic primer with a thickness of 20-30um, and the total thickness of HD-147 epoxy self-electrophoretic primer and JM-5001 high weather-resistant polyester powder is 100-120um. To meet the C4M anti-corrosion requirements, spray 130-150um of JM-5001 high weather-resistant polyester powder, HD-147 epoxy self-electrophoretic primer thickness is 20-30um, and the total thickness of HD-147 epoxy self-electrophoretic primer and JM-5001 high weather-resistant polyester powder is 150-180um. To meet the C5M anti-corrosion requirements, spray 100-130um of JM-5001 high weather-resistant polyester powder and 80-100um of JM-2005 conductive intermediate powder, and the thickness of HD-147 epoxy self-electrophoretic primer is 20-30um. The total thickness of HD-147 epoxy self-electrophoretic primer, JM-5001 high weather-resistant polyester powder and JM-2005 conductive intermediate powder is 200-260um.