A low-grade copper oxide waste rock heavy medium-strong magnetic combined closed-circuit tailings enrichment process

By combining three-stage closed-circuit crushing and screening with 0.5mm precision hydraulic classification, heavy medium hydrocyclone and vertical ring high gradient strong magnetic separation, the sorting problem of low-grade high-calcium and magnesium copper oxide waste rock was solved, realizing efficient recovery of copper minerals and environmentally friendly utilization of resources.

CN123102716APending Publication Date: 2026-11-17SHENYANG RES INST OF NONFERROUS METALS +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611519209.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-29
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies cannot effectively process low-grade, high-calcium-magnesium copper oxide waste rock from mining areas in the Democratic Republic of Congo, leading to resource waste, environmental pollution, and high production costs.

Method used

A combined closed-circuit tailings removal enrichment process is adopted, which combines three-stage closed-circuit crushing and screening, 0.5mm precision hydraulic classification, and heavy medium hydrocyclone with vertical ring high gradient strong magnetic separation, to achieve the removal of coarse-grained calcium magnesium gangue and the recovery of fine-grained copper oxide minerals.

Benefits of technology

It significantly improved copper grade and metal recovery rate, reduced production costs and acid consumption, and achieved efficient resource utilization and environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention belongs to the field of non-ferrous metal mineral processing technology, specifically relating to a closed-circuit tailings enrichment process for low-grade copper oxide waste rock using a combined heavy media-strong magnetic separation method. The enrichment process steps are as follows: Step 1: Pre-treatment of the low-grade copper oxide waste rock through three-stage closed-circuit crushing and screening to obtain uniformly sized material ≤10mm; Step 2: Hydraulic classification of the ≤10mm material to obtain coarse and fine particles; Step 3: The coarse particles enter a heavy media separation process to obtain a heavy media enriched concentrate; Step 4: The fine particles enter a strong magnetic separation process to obtain a magnetic concentrate; Step 5: The heavy media enriched concentrate and the magnetic concentrate are combined to obtain the enriched raw material. This process uses physical separation, achieving precise separation of coarse and fine minerals through differentiated classification, significantly removing calcium and magnesium gangue impurities, improving copper grade, reducing acid consumption and production costs in subsequent acid leaching processes, and realizing the efficient resource utilization of stockpiled waste rock.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of non-ferrous metal mineral processing technology, specifically relating to a closed-circuit tailings enrichment process for low-grade copper oxide waste rock using a combined heavy medium-strong magnetic field method. Background Technology

[0002] The mining areas in the Democratic Republic of Congo contain a vast amount of low-grade copper oxide waste rock. This type of ore is generally characterized by low copper grade and extremely high calcium and magnesium impurity content, making it a typical difficult-to-process copper oxide mineral resource in the region.

[0003] Currently, the mainstream recovery process for copper oxide ore in the industry is acid leaching. However, this process has significant technical and economic drawbacks when applied to ore from the Democratic Republic of Congo: First, the large amount of calcium and magnesium alkaline impurities in the ore will neutralize with the leaching acid, resulting in extremely high acid consumption and high reagent operating costs; second, the low copper grade leads to low copper metal recovery rates after acid leaching, resulting in extremely poor overall production economic efficiency; third, long-term large-scale acid leaching operations are prone to causing water and soil pollution in the mining area, putting significant environmental pressure on the environment. Due to these technical bottlenecks, this type of low-grade, high-calcium and magnesium copper oxide waste rock cannot be effectively utilized for a long time and can only be stored in the open, which not only occupies a large amount of land resources and causes serious waste of copper metal mineral resources, but also poses problems such as landslides, dust pollution, and resource idleness and loss.

[0004] In existing mineral processing technologies, neither single heavy media separation nor single magnetic separation processes can be adapted to this type of complex ore: single heavy media separation cannot effectively recover fine-grained copper oxide minerals, resulting in severe loss of fine-grained metals; single strong magnetic separation is ineffective in removing coarse-grained gangue impurities, and the concentrate enrichment ratio is low. For example, Chinese patent CN121945282A discloses a mineral processing method for pre-enrichment of copper oxide cobalt ore, which uses crushing to -60mm and screening into three particle sizes, using photoelectric separation for -60+10mm, heavy media separation for -10+0.5mm, and magnetic separation for -0.5mm, and combining the concentrate to achieve pre-enrichment; although this process provides a solution for the treatment of low-grade high-calcium-magnesium copper oxide ore, it still has the following shortcomings: (1) The crushing system is only coarsely crushed to -60mm, with a wide range of feed particle sizes, resulting in poor stability of subsequent sorting operations; (2) The coarse-grained stage uses photoelectric separation, which has high requirements for the ore surface and limited processing capacity, making it unsuitable for large-scale continuous production; (3) it does not have a complete media circulation system, resulting in high operating costs; (4) the fine-grained stage magnetic separation is only described in a general way, without specifying the equipment selection and process parameters, and lacks data support for the recovery effect of fine copper oxide; the process adopts a combination of photoelectric pre-selection + heavy media + conventional magnetic separation, with the core facing the separation of finished ore. It does not design a closed-circuit crushing system for stockpiled waste rock, and does not use vertical ring high gradient magnetic separation equipment, resulting in poor recovery effect of fine copper oxide. In addition, Chinese patent CN122141840A applies the heavy media + strong magnetic process to the separation of iron-containing copper minerals. The processing objects are magnetite and hematite associated copper ore, not high calcium and magnesium copper oxide waste rock. The ore properties and process adaptability are completely different, and it cannot be used by analogy.

[0005] In summary, there is currently no fully physical closed-loop combined sorting process specifically designed for high-calcium and magnesium, low-grade, oxidized copper oxide waste rock stockpiles in the Democratic Republic of Congo. The market urgently needs an industrial pretreatment technology that is low in energy consumption, reagent-free, has recyclable media, and has excellent enrichment effect. Summary of the Invention

[0006] In view of the shortcomings of the above-mentioned technologies, this invention provides a closed-circuit tailings extraction and enrichment process for low-grade copper oxide waste rock using a combined heavy media-strong magnetic field method. This process is particularly suitable for the pretreatment of stockpiled low-grade copper oxide ore resources in the Democratic Republic of Congo, providing high-quality raw materials for subsequent hydrometallurgical copper extraction. The entire process employs physical separation, achieving precise separation of coarse and fine-grained minerals through graded and differentiated separation. It is equipped with a complete heavy media circulation system and a fine-grained strong magnetic tailings extraction process, significantly removing calcium and magnesium gangue impurities, improving copper grade, reducing acid consumption and production costs in subsequent acid leaching processes, and achieving efficient resource utilization of stockpiled waste rock.

[0007] To achieve the above objectives, the present invention adopts the following technical solution.

[0008] A closed-circuit tailings enrichment process for low-grade copper oxide waste rock using heavy medium and strong magnetic field combined, the specific steps of which are as follows: Step 1: The low-grade copper oxide waste rock is subjected to three-stage closed-circuit crushing and screening pretreatment to obtain material with uniform particle size ≤10mm. Step 2: Perform hydraulic classification on the above ≤10mm material to obtain coarse-grained material and fine-grained material; Step 3: The coarse-grained material enters the heavy media separation process to obtain heavy media enriched concentrate; Step 4: Fine-grained materials enter the high-intensity magnetic separation process to obtain magnetic concentrate; Step 5: Combine the heavy media enriched concentrate with the magnetic separation concentrate to obtain the enriched raw material.

[0009] Further, step 1 specifically involves: feeding low-grade copper oxide waste rock into a coarse crushing device, which crushes it to obtain material with a particle size ≤150mm; conveying the material with a particle size ≤150mm to a double-layer vibrating screen, with the upper screen having a mesh size of 40mm×40mm and the lower screen having a mesh size of 10mm×10mm; conveying the material with a particle size ≤10mm under the double-layer vibrating screen to a storage bin, and sending the coarse particles over the two screens to a medium crushing device; feeding the medium crushing product into a single-layer inspection vibrating screen with a mesh size of 10mm×10mm, sending the material with a particle size ≤10mm under the single-layer inspection screen to a storage bin, and sending the coarse particles over the single-layer inspection screen to a fine crushing device; and returning the fine crushing product to the discharge end of the medium crushing device to form a closed-loop crushing and screening cycle, stably producing material with a uniform particle size ≤10mm.

[0010] Further, step 2 specifically involves: ≤10mm material in the ore storage bin is uniformly and quantitatively fed into a high-frequency vibrating screen with a screen aperture of 0.5mm (vibration frequency 47~60Hz (corresponding to a rotation speed of 2800~3600 r / min), amplitude 0.2~2.0mm) for hydraulic classification. After classification, the material is divided into two particle sizes: coarse particles with a particle size of 0.5mm-10mm and fine particles with a particle size of ≤0.5mm. The coarse particles enter the heavy media separation process, and the fine particles enter the strong magnetic separation process.

[0011] Further, step 3 specifically involves using ferrosilicon powder as the heavy medium, with a density of 1.70–2.20 g / cm³. 3 The feed concentration is 15-25%, the feed pressure is 0.08-0.12 MPa, and the underflow diameter is matched with a suitable φ180 mm-φ220 mm. After being separated by a heavy medium hydrocyclone, the material is divided into overflow tailings and underflow concentrate. 1. The overflow tailings are sent to the desliming screen. The material on the screen after desliming is the final tailings, which are transported to the tailings dam for storage or used for backfilling in the mine. The slurry containing medium under the desliming screen is sent to a weak magnetic separator to recover ferrosilicon powder. The recovered ferrosilicon powder is washed and purified and then recycled. The non-magnetic and weakly magnetic minerals produced by the weak magnetic separator are used as the final tailings and are discharged together with the material on the desliming screen. 2. The underflow concentrate is fed into a desliming screen. The material on the screen after desliming is the heavy medium enriched concentrate. The slurry under the desliming screen is fed into a weak magnetic separator to recover ferrosilicon powder. The medium is recycled. The fine-grained weak magnetic concentrate separated by the weak magnetic separator is incorporated into the heavy medium enriched concentrate.

[0012] Further, step 4 specifically involves: a magnetic field strength of 1.3–1.5T, a rotational speed of 2.5–3.5 revolutions / min, and a pulse frequency of 250–350 pulses / min.

[0013] The process adopts vertical ring high gradient magnetic separation, one roughing and one scavenging process. The roughing concentrate and scavenging concentrate are combined to obtain magnetic concentrate. The non-magnetic gangue minerals separated in the vertical ring high gradient magnetic separation process are used as tailings and transported to tailings ponds or underground backfilling.

[0014] Further, step 5 specifically involves merging the heavy media enriched concentrate with the magnetic separation concentrate to obtain the final copper oxide enriched raw material, which is then used for subsequent acid leaching copper extraction operations.

[0015] Compared with the prior art, the beneficial effects of the present invention are as follows.

[0016] (1) The process is highly targeted and fills the technological gap: For the first time, this invention is designed for the high-calcium and magnesium, low-grade, oxidized copper oxide waste rock in the Democratic Republic of Congo. It designs a three-stage closed-circuit crushing + 0.5mm precision hydraulic classification + heavy medium hydrocyclone + vertical ring high gradient strong magnetic coarsening and sweeping integrated process system, which is different from existing similar patents such as photoelectric pre-selection, conventional magnetic separation, and iron ore separation. It specifically solves the separation problem of this type of difficult-to-use waste rock.

[0017] (2) Closed-circuit crushing system with high production stability: It adopts a three-stage closed-circuit crushing structure with double-layer pre-screening + single-layer inspection screening, strictly controls the feed particle size to ≤10mm, and the material mudification degree is low, which effectively ensures the efficiency of subsequent grading and sorting operations and is suitable for continuous large-scale industrial production in mines.

[0018] The three-stage closed-circuit crushing system of this invention strictly controls the feed particle size to ≤10mm, which greatly improves the uniformity of feed and effectively ensures the efficiency of subsequent grading and sorting operations, making it suitable for continuous large-scale industrial production in mines.

[0019] (3) Differentiated sorting and enrichment effect: Hydraulic classification with a critical particle size of 0.5mm is adopted to achieve differentiated treatment of "removing calcium and magnesium gangue by coarse heavy media and recovering copper oxide minerals by fine high gradient magnetic separation", avoiding metal loss and incomplete sorting caused by mixed sorting of coarse and fine minerals, and gangue removal rate ≥60%.

[0020] (4) Closed-loop recycling of heavy media, green and energy-saving, low operating cost: The complete ferrosilicon powder recycling system is equipped with desliming water screen + weak magnetic separator. The media recovery rate is ≥98%, which can be used for a long time and the media loss is extremely low. All production tailings can be backfilled underground to realize the resource utilization of solid waste without secondary pollution.

[0021] (5) Excellent fine particle recovery capability and high metal recovery rate: The vertical ring high gradient magnetic separator adopts a coarse and sweep process, and with optimized magnetic field, speed and pulse parameters, it can efficiently collect -0.5mm fine copper oxide minerals. Compared with conventional magnetic separation, the fine metal recovery rate is significantly improved.

[0022] (6) Significant cost reduction and efficiency improvement, outstanding economic benefits: This process is a fully physical pretreatment process without adding flotation reagents. After pretreatment, the copper grade of the raw material is increased to 2.0%-2.8%, and the acid consumption of the subsequent acid leaching process is reduced by more than 30%, which completely solves the problem that direct acid leaching of raw ore has no economic benefits and has broad prospects for industrial application. Detailed Implementation

[0023] The claims of the present invention will be further described in detail below with reference to specific embodiments, but this does not constitute any limitation on the present invention. Any limited modifications made by any person within the scope of the claims of the present invention shall still be within the scope of protection of the claims of the present invention.

[0024] The vertical ring high gradient magnetic separator of this invention adopts a vertical rotating ring and reverse flushing unloading structure, which fundamentally alleviates the problem of magnetic media blockage. It is equipped with a slurry pulsation mechanism to keep mineral particles in a loose state, reduce gangue mechanical inclusions, and improve the separation effect of fine and weakly magnetic minerals. The equipment is more adaptable to fluctuations in feed particle size and slurry concentration, maintains stable separation indicators during long-term operation, has a high operating rate, and requires less maintenance.

[0025] 1. Principle of Heavy Medium Separation and Necessity of Desliming Heavy media separation relies on the sedimentation differences of particles with different densities in a heavy media suspension to achieve separation. Mineral slime (fine slime) brings several core problems: (1) Deterioration of the stability of heavy medium suspension: Fine mineral mud will enter the suspension, increasing the viscosity of the medium. After the viscosity increases, the settling of low-density gangue particles becomes slower, the sorting accuracy decreases, the sorting density is difficult to control stably, the mismatch between light and heavy products increases, and the tailings rejection index deteriorates.

[0026] (2) Increased load on media recovery system and surge in media loss: Fine mud easily penetrates filter cloth and magnetic separator and enters the media recovery stage with overflow / bottom flow; a large amount of sludge will pollute magnetite media, resulting in large media loss, increased media consumption, and significantly increased operating costs.

[0027] (3) Blocking hydrocyclones and wearing out equipment: Fine mud adheres to the surface of coarse particles, forming a mud coating layer, which changes the apparent density of the particles, causing "false particle density" and interfering with the separation; at the same time, the fine mud + medium mixed slurry aggravates the wear of pumps, hydrocyclones and pipelines, and is also prone to clogging the bottom nozzle.

[0028] (4) Interference with subsequent product dewatering: The concentrate and tailings contain a large amount of sludge, making it difficult to dewater the subsequent screen surface by flushing, resulting in high product moisture content.

[0029] Therefore, the purpose of desliming is to remove fine mineral slime, reduce the viscosity of the suspension, stabilize the separation density, reduce media loss, and ensure the separation accuracy of the heavy media hydrocyclone.

[0030] 2. Desliming particle size design Because the particle size distribution of industrial heavy media is ≥95% at -200 mesh, the screen apertures of the desliming sieves were designed to be 0.3mm, 0.5mm, 0.75mm, 1.0mm, and 1.5mm for comparative testing. The test results show that: (1) Heavy medium gravity separation test: as the screen size of the desliming sieve increases, the consumption of heavy medium decreases accordingly. The copper enrichment ratio and copper recovery rate both increase first and then decrease. The index is optimal at 0.5 mm.

[0031] (2) Magnetic separation test: as the screen size of the desliming screen increases, the copper enrichment ratio does not change much, but the concentrate yield decreases and the copper recovery rate decreases accordingly (because some copper oxide particles are fine and often exist in the form of gangue, which reduces the magnetic induction intensity).

[0032] Therefore, based on the optimal technical indicators of the experiment, the grading particle size point was determined to be 0.5 mm.

[0033] Example 1.

[0034] Experimental materials: copper oxide waste rock stockpiled in a mining area in the Democratic Republic of Congo. The raw ore has a copper grade of 1.16%, contains 1.03% acid-soluble copper, and has a copper oxidation rate of 88.79%.

[0035] (1) Crushing and screening: The raw ore is coarsely crushed to ≤150mm by jaw crusher and then enters a 40mm×40mm / 10mm×10mm double-layer vibrating screen; the material with a particle size of ≤10mm under the screen is transported to the storage bin for storage, the material on the screen enters the cone crusher for medium crushing, the medium crushing product is graded by a 10mm×10mm single-layer inspection screen, the material with a particle size of ≤10mm under the screen is sent to the storage bin for storage, the material on the screen enters the cone crusher for fine crushing, the fine crushing product is returned to the discharge end of the medium crushing to form a closed circuit, and the material with a particle size of ≤10mm is stably produced and sent to the storage bin.

[0036] (2) Hydraulic classification: ≤10mm material in the storage bin is fed into a high-frequency vibrating screen with a screen opening of 0.5mm (vibration frequency 60Hz, amplitude 2.0mm). After classification, the proportion of 0.5-10mm particles is 43.63%, containing 1.50% copper, with a copper distribution rate of 56.44%, containing 1.34% acid-soluble copper, with an acid-soluble copper distribution rate of 56.70%; the proportion of ≤0.5mm particles is 56.37%, containing 0.896% copper, with a copper distribution rate of 43.56%, containing 0.792% acid-soluble copper, with an acid-soluble copper distribution rate of 43.30%.

[0037] (3) Heavy medium separation: Ferrosilicon powder is used as the heavy medium, and the medium density is controlled at 1.74 g / cm³. 3 The feed concentration is 25% and the feed pressure is 0.1 MPa. After separation, the overflow tailings are discharged after demediuming and weak magnetic separation to recover the medium. The underflow concentrate is demediumed to obtain heavy medium concentrate with an operating yield of 30.66% and a tailings rejection rate of 69.34%. The heavy medium concentrate contains 4.148% copper, with a copper enrichment ratio of 2.76 and an operating copper recovery rate of 84.79%. It also contains 3.725% acid-soluble copper, with a copper enrichment ratio of 2.78 and an operating copper recovery rate of 85.23%.

[0038] (4) High-intensity magnetic separation: Parameters of vertical ring high-gradient magnetic separator: magnetic field strength 1.3T, ring speed 3.5r / min, pulse frequency 350 times / min. A roughing and scavenging process is adopted. The roughing concentrate and scavenging concentrate are combined to obtain magnetic concentrate. The output of magnetic concentrate is 41.26%, the tailings rate is 58.74%, the copper content of the concentrate is 1.58%, the copper enrichment ratio is 1.76, the copper recovery rate reaches 72.76%, the acid-soluble copper grade is 1.43%, the copper enrichment ratio is 1.81, and the acid-soluble copper recovery rate is 74.50%. The comprehensive recovery rate of ferrosilicon powder media is 96.5%.

[0039] (5) Concentrate merging: After merging the heavy media enriched concentrate and the magnetic separation concentrate, the concentrate yield is 36.64%, the tailings rate is 63.36%, the copper grade is enriched from 1.16% to 2.518%, the enrichment ratio is 2.17, the copper recovery rate is 79.55%, the acid-soluble copper grade is enriched from 1.03% to 2.268%, the enrichment ratio is 2.20, and the acid-soluble copper recovery rate is 80.59%.

[0040] The enriched raw material in this embodiment was used for acid leaching production. The acid consumption was reduced by 31.52% compared with direct acid leaching of raw ore. The process operated continuously and stably (discard rate 63.36%, media loss 3.5%), as shown in Table 1.

[0041] Table 1 Technical specifications of Example 1.

[0042] Note: All yields in the table are based on 100% of the original ore.

[0043] Example 2.

[0044] Experimental materials: copper oxide waste rock stockpiled in a mining area of ​​Gangbov, with a copper grade of 0.60%, containing 0.54% acid-soluble copper and a copper oxidation rate of 90%.

[0045] (1) Crushing and screening: The raw ore is coarsely crushed to ≤150mm by jaw crusher and then enters a 40mm×40mm / 10mm×10mm double-layer vibrating screen; the material with a particle size of ≤10mm under the screen is transported to the storage bin for storage, the material on the screen enters the cone crusher for intermediate crushing, the intermediate crushing product is graded by a 10mm×10mm inspection screen, the material with a particle size of ≤10mm under the screen is sent to the storage bin for storage, the material on the screen enters the cone crusher for fine crushing, the fine crushing product is returned to the intermediate crushing discharge, forming a closed circuit, and stably producing material with a particle size of ≤10mm is sent to the storage bin.

[0046] (2) Hydraulic classification: ≤10mm material in the storage bin is fed into a high-frequency vibrating screen with a screen opening of 0.5mm (vibration frequency 60Hz, amplitude 2.0mm). After classification, the proportion of 0.5-10mm particles is 43.12%, containing 0.785% copper, with a copper distribution rate of 56.56%, containing 0.712% acid-soluble copper, with an acid-soluble copper distribution rate of 56.95%; the proportion of ≤0.5mm particles is 56.88%, containing 0.457% copper, with a copper distribution rate of 43.44%, containing 0.408% acid-soluble copper, with an acid-soluble copper distribution rate of 43.05%.

[0047] (3) Heavy medium separation: Ferrosilicon powder is used as the heavy medium, and the medium density is controlled at 1.72 g / cm³. 3 The feed concentration was 25% and the feed pressure was 0.1 MPa. After separation, the overflow tailings were demediumed and subjected to weak magnetic separation to recover the media before being discharged. The underflow concentrate, after demediuming, yielded a heavy medium concentrate with an operating yield of 26.70% and a tailings rejection rate of 73.30%. The heavy medium concentrate contained 2.48% copper, with a copper enrichment ratio of 3.16 and a copper recovery rate of 84.35%. It also contained 2.28% acid-soluble copper, with a copper enrichment ratio of 3.20 and an acid-soluble copper recovery rate of 85.50%. The overall recovery rate of ferrosilicon powder was 96.2%.

[0048] (4) High-intensity magnetic separation: Parameters of vertical ring high gradient magnetic separator: magnetic field strength 1.3T, ring speed 3.5r / min, pulse frequency 350 times / min. The process of roughing and scavenging is adopted. The roughing concentrate and scavenging concentrate are combined to obtain magnetic concentrate. The output of magnetic concentrate is 37.47%, the tailings rate is 62.53%, the copper content of the concentrate is 0.938%, the copper enrichment ratio is 2.05, and the copper recovery rate reaches 76.91%; the acid-soluble copper grade is 0.859%, the copper enrichment ratio is 2.11, and the acid-soluble copper recovery rate is 78.89%.

[0049] (5) Concentrate merging: After merging the heavy media enriched concentrate and the magnetic separation concentrate, the concentrate yield is 32.82%, the tailings rate is 67.18%, the copper grade is enriched from 0.6% to 1.479%, the enrichment ratio is 2.47, the copper recovery rate is 81.11%, the acid-soluble copper grade is 1.357%, the copper enrichment ratio is 2.51, and the acid-soluble copper recovery rate is 82.65%.

[0050] In this embodiment, the enriched raw material is used for acid leaching production, and the acid consumption is reduced by 35.32% compared with direct acid leaching of raw ore. The process runs continuously and stably (discard rate 67.18%, media loss 3.8%), as shown in Table 2.

[0051] Table 2 Technical specifications for Example 2.

[0052] Note: All yields in the table are based on 100% of the original ore.

[0053] Comparative Example 1: Comparison of vertical ring high gradient magnetic separation process.

[0054] This comparative example compares the process selection for high-intensity magnetic separation of fine-particle materials. The experimental raw material is ≤0.5mm fine-particle material obtained from hydraulic classification in Example 2. This material contains 0.457% copper and is separated using a vertical ring high-gradient magnetic separator. With a fixed magnetic field strength of 1.3T, a ring rotation speed of 3.5 r / min, and a pulse frequency of 350 times / min, the following three magnetic separation processes are compared: (1) Single coarse selection process; (2) One coarse and one fine scan process; (3) One coarse and two sweep process.

[0055] The test results are shown in Table 3.

[0056] Table 3 Comparative test results of vertical ring high gradient magnetic separation process.

[0057] Note: "Sample" in the table refers to fine-grained material ≤0.5mm that enters the magnetic separation process, i.e., magnetic separation feed.

[0058] As shown in Table 3: (1) If a single roughing process is used, only rough and refined products are obtained, and the copper recovery rate is 67.78%, resulting in significant copper loss. Therefore, although the single roughing process is simple, the recovery rate is low and it is not suitable as the final magnetic separation process for the fine-grained copper oxide material of this invention.

[0059] (2) If a roughing-scavenging process is adopted, that is, the roughing concentrate and the scavenging concentrate are combined as magnetic concentrate, the cumulative copper recovery rate can be increased from 67.78% to 76.91%, an increase of 9.13 percentage points. This process can significantly improve the copper recovery rate with fewer equipment configurations, taking into account both the separation index and production economy.

[0060] (3) If a one-roughing-two-scavenging process is adopted, that is, scavenging 2 is added on the basis of roughing and scavenging 1, the concentrate yield of scavenging 2 is 2.48%, the Cu grade is 0.338%, the Cu operation recovery rate is 1.83%, and the cumulative copper recovery rate increases from 76.91% to 78.74%. Compared with the one-roughing-one-scavenging process, although the one-roughing-two-scavenging process can further increase the copper recovery rate by 1.83 percentage points, the increase is limited, and it requires additional magnetic separation equipment, energy consumption and closed-loop load, and the production operation and maintenance are more complicated.

[0061] In summary, the single roughing process has a low copper recovery rate; although the one-roughing-two-scanning process has a slightly higher recovery rate, it requires more equipment, consumes more energy, has a large closed-loop load, and is complex to operate and maintain; the one-roughing-one-scanning process can achieve a higher copper recovery rate with fewer equipment configurations, taking into account both grade and recovery rate. Therefore, this invention selects the one-roughing-one-scanning process as the preferred process for vertical ring high gradient magnetic separation.

Claims

1. A low-grade copper oxide waste rock heavy medium-strong magnetic combined closed-circuit tailings enrichment process, characterized in that, The specific steps are as follows: Step 1: The low-grade copper oxide waste rock is subjected to three-stage closed-circuit crushing and screening pretreatment to obtain material with uniform particle size ≤10mm. Step 2: Perform hydraulic classification on the above ≤10mm material to obtain coarse-grained material and fine-grained material; Step 3: The coarse-grained material enters the heavy media separation process to obtain heavy media enriched concentrate; Step 4: Fine-grained materials enter the high-intensity magnetic separation process to obtain magnetic concentrate; Step 5: Combine the heavy media enriched concentrate with the magnetic separation concentrate to obtain the enriched raw material.

2. The enrichment process according to claim 1, characterized in that, Step 1 specifically involves: feeding low-grade copper oxide waste rock into a coarse crushing device, which crushes it to obtain material with a particle size ≤150mm; conveying the material with a particle size ≤150mm to a double-layer vibrating screen, with the upper screen having a mesh size of 40mm×40mm and the lower screen having a mesh size of 10mm×10mm; conveying the material with a particle size ≤10mm under the double-layer vibrating screen to a storage bin, and conveying the coarse particles over the two screens to a medium crushing device; conveying the medium crushing product to a single-layer inspection vibrating screen with a mesh size of 10mm×10mm, conveying the material with a particle size ≤10mm under the single-layer inspection screen to a storage bin, and conveying the coarse particles over the single-layer inspection screen to a fine crushing device; and recirculating the fine crushing product back into the discharge end of the medium crushing device to form a closed-loop crushing and screening cycle, stably producing material with a uniform particle size ≤10mm.

3. The enrichment process according to claim 1, characterized in that, Step 2 specifically involves: ≤10mm material in the ore storage bin is fed evenly and quantitatively via a belt conveyor and sent to a high-frequency vibrating screen with a screen aperture of 0.5mm for hydraulic classification. After classification, the material is divided into two particle sizes: coarse material with a particle size of 0.5mm-10mm and fine material with a particle size of ≤0.5mm. The coarse material enters the heavy medium separation process, and the fine material enters the strong magnetic separation process.

4. The enrichment process according to claim 1, characterized in that, Step 3 specifically involves using ferrosilicon powder as a heavy medium, with a density of 1.70–2.20 g / cm³. 3 The feed concentration is 15-25%, the feed pressure is 0.08-0.12 MPa, and the material is separated into overflow tailings and underflow concentrate after being separated by a heavy medium hydrocyclone.

5. The enrichment process according to claim 4, characterized in that, The overflow tailings are sent to a desliming screen. The material on the screen after desliming is the final tailings, which are transported to a tailings dam for storage or used for backfilling in the mine. The slurry containing medium under the desliming screen is sent to a weak magnetic separator to recover ferrosilicon powder. The recovered ferrosilicon powder is washed and purified and then recycled. The non-magnetic and weakly magnetic minerals produced by the weak magnetic separator are used as the final tailings and are discharged together with the material on the desliming screen.

6. The enrichment process according to claim 4, characterized in that, The underflow concentrate is fed into a desliming screen, and the material on the screen after desliming is the heavy medium enriched concentrate. The slurry under the desliming screen is sent to a weak magnetic separator to recover ferrosilicon powder, and the medium is recycled. The fine-grained weak magnetic concentrate separated by the weak magnetic separator is incorporated into the heavy medium enriched concentrate.

7. The enrichment process according to claim 1, characterized in that, Step 4 specifically involves: a magnetic field strength of 1.3–1.5T, a rotating ring speed of 2.5–3.5 rpm, and a pulse frequency of 250–350 pulses / min; a vertical ring high gradient magnetic separation process with one roughing and one scavenging stage is adopted, and the roughing concentrate and scavenging concentrate are combined to obtain the magnetic concentrate; the non-magnetic gangue minerals separated in the vertical ring high gradient magnetic separation process are used as tailings and transported to the tailings dam or underground backfill.

8. The enrichment process according to claim 1, characterized in that, Step 5 specifically involves merging the heavy medium enriched concentrate with the magnetic separation concentrate to obtain the final copper oxide enriched raw material, which is then used for subsequent acid leaching copper extraction operations.

Citation Information

Patent Citations

  • Beneficiation method for preconcentration of copper cobalt oxide ore

    CN121945282A

  • Multi-stage grading enrichment comprehensive recovery method and system for copper-containing magnetite and hematite

    CN122141840A