Methods and systems for the co-mineralization of CO2 and the cascade utilization of waste heat from magnesium slag and calcium carbide slag
By using the synergistic mineralization of magnesium slag and calcium carbide slag and the cascade utilization of waste heat, the problems of high energy consumption, waste heat and low added value of products in the existing CO2 mineralization technology have been solved, and efficient energy utilization and high-value product production have been achieved.
Patent Information
- Application Number
- CN202611412058.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-11
- Publication Date
- 2026-11-17
AI Technical Summary
Existing CO2 mineralization technologies suffer from problems such as high energy consumption for regenerating organic amines and adsorbents, insufficient co-utilization of solid waste, serious waste of waste heat resources, and limited added value of products.
By mixing magnesium slag and calcium carbide slag in a specific ratio, a three-stage waste heat utilization system is constructed, which includes power generation in the high-temperature section, heating in the medium-temperature section, and drying in the low-temperature section. The system integrates the MEA method and the ammonia leaching method in parallel production lines to produce cement admixture-grade calcium carbonate and calcium carbide-grade high-purity calcium carbonate, respectively. The product quality is ensured by multiple ammonia leaching cycles for purification and precise control of carbonation time.
It achieves efficient utilization of sensible heat from magnesium slag and waste heat from calcium carbide furnace tail gas, improves calcium conversion rate, generates approximately 2 million kWh of electricity annually, produces high-value products, realizes system energy self-sufficiency and closed-loop resource management throughout the entire process, and reduces energy consumption and equipment investment.
Smart Images

Figure CN123102723A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the interdisciplinary technical field of industrial solid waste resource utilization and waste heat cascade recovery and utilization, specifically involving a method and system for the co-mineralization of CO2 by magnesium slag and carbide slag and the cascade utilization of waste heat. Background Technology
[0002] The massive emission of carbon dioxide (CO2) is one of the main causes of global warming, and carbon capture, utilization, and storage (CCUS) technology is a key pathway to achieve deep industrial emission reduction. Magnesium slag, a solid waste generated during the silicothermic magnesium smelting process, is rich in calcium oxide (CaO) and calcium silicate, possessing the potential for mineralization with CO2. Calcium carbide slag, a waste residue generated during the acetylene production process using the calcium carbide method, is mainly composed of calcium hydroxide (Ca(OH)2) and can also be used as a mineralization raw material. Furthermore, the slag discharge temperature of magnesium slag reaches as high as 1100℃, while the tail gas temperature of the calcium carbide furnace is approximately 800-1000℃; both contain a large amount of high-grade waste heat. Currently, the main technologies for mineralizing CO2 from industrial solid waste are direct carbonation and indirect carbonation, but these methods suffer from the following problems: traditional mineralization processes require high temperature and high pressure conditions, resulting in high energy consumption; organic amines require high-temperature thermal regeneration after absorbing CO2, with energy consumption accounting for more than 50% of the total process energy consumption; magnesium slag and calcium carbide slag are usually treated separately, lacking synergy; and waste heat is directly emitted, leading to significant energy waste. Traditional mineralization processes (such as direct carbonation in water) have slow reaction rates and low calcium conversion rates, often requiring heating to 100-200℃ or pressurization to 10-20 bar, resulting in large equipment investments and high energy consumption. Existing organic amines absorb CO2 and then undergo thermal desorption regeneration, with regeneration temperatures as high as 100-140℃, consuming enormous amounts of energy (approximately 3.6 GJ / t CO2), leading to persistently high carbon capture costs. Currently, magnesium slag and calcium carbide slag are typically treated separately, without synergistic utilization; the sensible heat from magnesium slag discharge (approximately 1100℃) and the waste heat from calcium carbide furnace tail gas (approximately 900℃) are directly air-cooled or burned, resulting in significant heat waste. In existing processes, the economic added value of mineralization products is low, and a closed loop of "solid waste disposal - carbon sequestration - building material reuse" cannot be formed.
[0003] Chinese patent application CN122141409A discloses a system and method for preparing negative carbon products through carbon dioxide capture and synergistic solid waste mineralization. This system uses a composite amine solution to absorb CO2 and generate a rich amine solution, which is then reacted with a solid waste leachate to achieve non-thermal amine regeneration, producing both nano-calcium carbonate and a cementitious material. However, the solid waste raw materials are only generalized, without targeted synergistic formulation based on the specific component characteristics of wastes such as magnesium slag and carbide slag; waste heat utilization is limited to a single-stage heat exchange, failing to form a tiered utilization system of high-temperature power generation, medium-temperature heating, and low-temperature drying; and the mineralization process is simplistic, unable to flexibly adjust product quality according to downstream demand. Chinese patent application CN114768501B discloses a CO2 capture and industrial solid waste mineralization coupling system based on a calcium cycle method. This system achieves CO2 capture through a CaO carbonation / calcination cycle and sends deactivated oxides to the mineralization system for utilization. However, this technology has prominent problems such as extremely high energy consumption for thermal decomposition (requiring high-temperature calcination at 400-900℃), severe degradation of adsorbents during circulation, and reliance on external heat sources.
[0004] To address the aforementioned issues, there is an urgent need to find a method for the co-mineralization of CO2 from magnesium slag and calcium carbide slag, as well as the cascade utilization of waste heat. This method involves co-mineralizing magnesium slag and calcium carbide slag in a specific ratio to construct a three-stage waste heat cascade utilization system: high-temperature power generation, medium-temperature heating, and low-temperature drying. It integrates parallel production lines using both MEA and ammonia leaching processes to produce cement admixture-grade calcium carbonate and calcium carbide-grade high-purity calcium carbonate, respectively. Product quality is ensured through multiple ammonia leaching cycles for purification and precise control of carbonation time, thereby achieving a closed-loop resource system encompassing solid waste disposal, carbon sequestration, and building material / chemical recycling. Summary of the Invention
[0005] In order to overcome the shortcomings of the prior art, the present invention aims to provide a method and system for the co-mineralization of CO2 by magnesium slag and carbide slag and the cascade utilization of waste heat, so as to solve the technical problems of high energy consumption for regeneration of organic amines and adsorbents, insufficient co-utilization of solid waste, serious waste of waste heat resources and limited added value of products in the existing CO2 mineralization technology.
[0006] To achieve the above objectives, the present invention employs the following technical solution: This invention discloses a method for the co-mineralization of CO2 from magnesium slag and calcium carbide slag and the cascade utilization of waste heat, comprising: Magnesium slag and calcium carbide slag were pretreated separately, and the pretreated magnesium slag was mixed with calcium carbide slag to obtain mixed slag; The sensible heat from magnesium slag discharge and the waste heat from the tail gas of the calcium carbide furnace are recovered and utilized in stages. The high-temperature stage is used to generate steam and generate electricity, the medium-temperature stage is used to supply heat to the mineralization reaction, and the low-temperature stage is used to dry the calcium carbide slag. Collect flue gas from the reduction furnace of the magnesium slag plant and tail gas from the calcium carbide furnace, catalytically combust CO in the tail gas of the calcium carbide furnace to convert it into CO2, and mix it with the flue gas from the reduction furnace of the magnesium slag plant to obtain a CO2 gas source for the mineralization reaction. The mixed slag was divided into two streams. The first stream used the MEA method, where the mixed slag was mixed with an ethanolamine solution, and a CO2 gas source was introduced under the heat provided in the medium-temperature section to carry out a mineralization reaction and then perform solid-liquid separation to obtain calcium carbonate products for cement admixtures. The second stream used the ammonia leaching method, where the mixed slag was mixed with an ammonium chloride solution for ammonia leaching, and solid-liquid separation was performed to obtain a leachate. After purification, the leachate was introduced into a CO2 gas source for a carbonation reaction, and after carbonation, solid-liquid separation was performed. The resulting filter cake was then subjected to ammonia leaching again to obtain high-purity calcium carbonate. The filtrate from the mineralization reaction is replenished with ethanolamine and then reused for MEA mineralization. The filtrate from ammonia leaching is replenished with ammonium chloride and then recycled. The NH3 released during carbonization is also recovered.
[0007] Preferably, the pretreatment of magnesium slag includes: calcining the magnesium slag at 900~950℃ for 1~2 h to activate it, and then ball milling it and passing it through a 150-mesh sieve; The pretreatment of carbide slag includes: using the residual heat of the low-temperature section to dry the carbide slag to a moisture content of less than 10%, and then ball milling and passing it through a 150-mesh sieve; The mass ratio of magnesium slag to calcium carbide slag is 1:(0.5~2).
[0008] Preferably, in the high-temperature section, the sensible heat carried by the magnesium slag at 1000~1100℃ and the waste heat of the calcium carbide furnace tail gas at 900~950℃ are introduced into the waste heat recovery system, and superheated steam is generated through the dual-pressure waste heat boiler to drive the steam turbine generator set to generate electricity. The low-pressure steam generated after power generation or the flue gas discharged from the waste heat boiler are used to generate hot water through heat exchange, which is then used as a heat source in the medium temperature section to supply heat to the MEA method and the ammonia leaching method. The flue gas after being utilized in the medium-temperature section is used as a heat source in the low-temperature section for drying carbide slag or preheating boiler feedwater.
[0009] Preferably, the MEA method mineralization includes: mixing the mixed residue with an ethanolamine solution with a concentration of 1.0~3.0 mol / L at a liquid-to-solid ratio of 20:1 mL / g, and reacting with CO2 gas at a flow rate of 100~300 mL / min at 40~60℃ and 100~300 r / min for 60~90 min; After the reaction is complete, vacuum filtration is performed, and the filter cake is washed with anhydrous ethanol at least three times and then dried.
[0010] Preferably, the ammonia leaching process includes: mixing the mixed residue with an ammonium chloride solution with a concentration of 1.5~2.5 mol / L at a liquid-to-solid ratio of 10:1 mL / g, reacting at 40~60℃ for 40~60 min, and then filtering to obtain the leachate; Add ammonia to the leachate to adjust the pH to 10-11, then add NaOH solution to precipitate Al. 3+ and Fe 3+ The purified liquid was obtained by standing and filtering. CO2 was introduced into the purified liquid to carry out a carbonization reaction for 9-12 minutes. The final pH value of carbonization was 9. After carbonization, the mixture was filtered, and the resulting filter cake was subjected to ammonia leaching again. Then, after solid-liquid separation, water washing and drying, high-purity calcium carbonate was obtained.
[0011] Preferably, the CO2 volume content in the flue gas from the reduction furnace of the magnesium slag plant is 10%~15%, and the CO volume content in the tail gas from the calcium carbide furnace is 60%~80%. The tail gas from the calcium carbide furnace is catalytically combusted at 300-400℃ using a platinum-palladium catalyst to convert CO into CO2, and then mixed with the flue gas from the reduction furnace of the magnesium slag plant. The volume concentration of CO2 in the mixed gas is adjusted to 20%-30%. The filtrate from the MEA mineralization process is recycled after being supplemented with 5% to 10% ethanolamine. The filtrate from the ammonia leaching process is recycled after being supplemented with ammonium chloride. The NH3 released during carbonization is absorbed by water spraying to form ammonia water with a mass concentration of 10% to 15%, which is then reused for pH adjustment.
[0012] This invention also discloses a system for the synergistic mineralization of magnesium slag and calcium carbide slag for CO2 and waste heat utilization, comprising: a waste heat recovery unit, a raw material pretreatment unit, a CO2 gas supply unit, an MEA mineralization unit, and an ammonia leaching mineralization unit; The waste heat cascade recovery unit is connected to the slag outlet of the magnesium slag plant and the tail gas emission outlet of the calcium carbide plant, respectively, to recover the sensible heat of the magnesium slag discharge and the waste heat of the calcium carbide furnace tail gas; the waste heat cascade recovery unit has a high-temperature waste heat utilization end, a medium-temperature waste heat utilization end and a low-temperature waste heat utilization end. The high-temperature waste heat utilization end is used for power generation, the medium-temperature waste heat utilization end is connected to the MEA method mineralization unit and the ammonia leaching method mineralization unit respectively to supply heat to the two, and the low-temperature waste heat utilization end is connected to the raw material pretreatment unit for drying calcium carbide slag. The raw material pretreatment unit is used to pretreat and mix magnesium slag and calcium carbide slag. The mixed material outlet of the raw material pretreatment unit is divided into two paths, one of which is connected to the material inlet of the MEA mineralization unit and the other is connected to the material inlet of the ammonia leaching mineralization unit. The gas inlet of the CO2 gas supply unit is connected to the flue gas source of the magnesium slag plant reduction furnace and the tail gas source of the calcium carbide furnace, respectively. The gas outlet of the CO2 gas supply unit is divided into two paths, one of which is connected to the MEA mineralization unit and the other is connected to the ammonia leaching mineralization unit. The MEA mineralization unit has a MEA filtrate recycling path, and the ammonia leaching mineralization unit has an ammonia leaching filtrate recycling path and an ammonia recovery and recycling path.
[0013] Preferably, the waste heat cascade recovery unit includes a dual-pressure waste heat boiler, a steam turbine generator set, and a heat exchanger; The slag outlet of the magnesium slag plant and the tail gas emission outlet of the calcium carbide plant are respectively connected to the dual-pressure waste heat boiler, and the main steam outlet of the dual-pressure waste heat boiler is connected to the steam turbine generator set. The exhaust port of the steam turbine generator set is connected to the heat exchanger, and the hot water outlet of the heat exchanger is connected to the MEA reactor jacket in the MEA mineralization unit and the ammonia leaching reactor jacket in the ammonia leaching mineralization unit through hot water pipes respectively. The low-temperature flue gas outlet of the waste heat cascade recovery unit is connected to the carbide slag drying section in the raw material pretreatment unit.
[0014] Preferably, the raw material pretreatment unit includes a magnesium slag pretreatment section, a carbide slag pretreatment section, and a mixing mixer. The material outlets of the magnesium slag pretreatment section and the carbide slag pretreatment section are respectively connected to the material inlet of the mixing mixer, and the material outlet of the mixing mixer is respectively connected to the MEA mineralization unit and the ammonia leaching mineralization unit. The CO2 gas supply unit includes magnesium slag flue gas pipeline, calcium carbide furnace tail gas pipeline, catalytic combustion device and gas mixing and blending device; The magnesium slag flue gas pipeline is connected to the gas mixing and blending device, and the calcium carbide furnace tail gas pipeline is connected to the gas mixing and blending device via the catalytic combustion device. The gas outlet of the gas mixing and blending device is connected to the MEA reactor in the MEA mineralization unit and the carbonization reactor in the ammonia leaching mineralization unit, respectively.
[0015] Preferably, the MEA mineralization unit includes an MEA reactor and a solid-liquid separation section connected in sequence. The filtrate outlet of the solid-liquid separation section is connected to the MEA reactor through the MEA filtrate recycling path, so that the MEA filtrate can be returned to the MEA reactor after replenishing MEA. The ammonia leaching mineralization unit includes an ammonia leaching reactor, a purification section, a carbonization reactor, and a solid-liquid separation section connected in sequence. The filtrate outlet of the ammonia leaching mineralization unit is connected to the ammonia leaching reactor via an ammonia leaching filtrate recycling path, so that the ammonia leaching filtrate can be recycled after being supplemented with ammonium chloride. The gas outlet of the carbonization reactor is connected to the ammonia recovery section, which is used to absorb the NH3 released during the carbonization process by water spraying and reuse the resulting ammonia water in the purification section.
[0016] Compared with the prior art, the present invention has the following beneficial effects: This invention discloses a method for the synergistic mineralization of magnesia slag and calcium carbide slag, utilizing CO2 and waste heat in a cascade manner. By mixing magnesia slag and calcium carbide slag in a specific ratio, the rapid reaction characteristics of Ca(OH)2 in the calcium carbide slag compensate for the slow reaction rate of the magnesia slag, thus synergistically improving the overall calcium conversion rate. A three-stage cascade utilization system is constructed by collecting the sensible heat from the magnesia slag discharge and the waste heat from the calcium carbide furnace tail gas: high-temperature power generation, medium-temperature heating, and low-temperature drying. This achieves a thermal energy utilization rate of over 85%, generating approximately 2 million kWh of electricity annually, thus realizing system energy self-sufficiency. The mixed slag is supplied to both the MEA (Medium-Oxygenation) and ammonia leaching mineralization processes for parallel operation, with both processes sharing a CO2 gas source and... The waste heat is used to produce cement admixture-grade calcium carbonate via the MEA method, which increases the 7-day compressive strength by 30%. The ammonia leaching method produces high-purity calcium carbonate with a purity ≥96%, CaO>98%, and MgO<0.03%, achieving high-value production for both products. Simultaneously, by supplementing and reusing the filtrate and recovering the escaping ammonia, a closed-loop material process and zero wastewater discharge are achieved. This method fundamentally solves the technical problems of high energy consumption for organic amine regeneration (reducing from 3.6 GJ / tCO2 to below 0.5 GJ / tCO2), insufficient co-utilization of solid waste, serious waste of waste heat resources, and limited added value of products in existing CO2 mineralization technologies, with annual revenue reaching 70-75 million yuan.
[0017] This invention discloses a magnesia slag and calcium carbide slag co-mineralization CO2 and waste heat cascade utilization system. Through a waste heat cascade recovery system, it recovers and distributes the sensible heat from magnesia slag discharge and the waste heat from calcium carbide furnace tail gas, achieving cascade energy utilization of high-temperature waste heat for power generation and medium-temperature waste heat for heating, with a thermal energy utilization rate exceeding 85%. The MEA (Medium-Oxygenation) mineralization unit and the ammonia leaching mineralization unit are respectively connected to the medium-temperature section of the waste heat cascade recovery system, allowing both processes to share a heat source and avoiding energy waste from independent heating. A CO2 gas supply unit simultaneously supplies gas to both mineralization units, achieving intensive utilization of the gas source. The low-temperature section of the waste heat cascade recovery system is connected to the calcium carbide slag drying device, using the originally emitted low-temperature waste heat for raw material pretreatment, further improving energy utilization efficiency. This deep integration of waste heat recovery, CO2 capture, and solid waste mineralization significantly reduces external energy consumption and equipment investment costs compared to existing technologies where mineralization and capture systems operate independently and heat sources rely on external supplies, demonstrating promising prospects for industrial application. Attached Figure Description
[0018] Figure 1 This is a flowchart illustrating the overall process flow of the present invention. Figure 2This invention relates to the effect of carbonation time on the intensity of characteristic peaks in the XRD pattern of calcium carbonate. Figure 3 This is a SEM image of the MEA method product (mixed morphology of calcite and aragonite) disclosed in Embodiment 1 of the present invention. Figure 4 This is a SEM image of the product obtained by the multiple ammonia leaching method disclosed in Embodiment 3 of the present invention; Figure 5 The Raman spectrum of the ammonia leaching product disclosed in Example 4 of this invention; Figure 6 This is a diagram of the cement compressive strength test for the blank control group; Figure 7 This is a compressive strength test chart of cement with a calcium carbonate content of 15% as disclosed in Example 1 of the present invention. Detailed Implementation
[0019] The technical solution of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0020] Unless otherwise specified, all embodiments and preferred embodiments mentioned herein can be combined to form new technical solutions.
[0021] Unless otherwise specified, all the technical features and preferred features mentioned herein can be combined to form new technical solutions.
[0022] In this invention, unless otherwise specified, percentage (%) or parts refer to weight percentage or parts relative to the composition.
[0023] Unless otherwise specified, the components or preferred components involved in this invention can be combined with each other to form new technical solutions.
[0024] In this invention, unless otherwise specified, the numerical range "a~b" is an abbreviation for any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "6~22" indicates that all real numbers between "6~22" have been listed in this document, and "6~22" is simply an abbreviation for these numerical combinations.
[0025] The "scope" disclosed in this invention can be in the form of a lower limit and an upper limit, and can be one or more lower limits and one or more upper limits, respectively.
[0026] The term “and / or” as used in this invention refers to any combination of one or more of the associated listed items, as well as all possible combinations, and includes such combinations.
[0027] Unless otherwise stated, the technical and scientific terms used herein have the same meanings as those familiar to those skilled in the art. Furthermore, any methods or materials similar to or equivalent to those described herein may also be used in this invention.
[0028] This invention provides a method for the co-mineralization of CO2 from magnesium slag and calcium carbide slag and the cascade utilization of waste heat, comprising the following steps: (a) Waste heat recovery system Stage 1 (High-Temperature Section): High-temperature magnesia slag (1000-1100℃) discharged from the reduction furnace of the magnesia slag plant and tail gas from the calcium carbide furnace of the calcium carbide plant (900-950℃) are introduced into a fully enclosed waste heat recovery system. The high-temperature section employs dual-pressure waste heat boiler technology, generating high-quality superheated steam at 3.82MPa and 450℃ to drive a 1.5MW steam turbine generator set for power generation. These steam parameters match the upper limit of "rated steam temperature less than or equal to 450℃" in the "Energy Saving Design Guidelines for Industrial Boiler Systems" (GB / T 34912-2017). The low-pressure steam (0.5MPa, approximately 160℃) discharged after power generation enters the next stage, achieving efficient cascade utilization of energy.
[0029] Secondary stage (medium temperature section): The 300-400℃ flue gas discharged from the waste heat boiler is processed through a steam turbine extraction system to generate saturated steam at 0.5MPa and approximately 160℃. In addition to being used for power generation, this saturated steam can also be used to generate hot water at 60-90℃ through a heat exchanger to heat the reaction vessels of the two mineralization processes.
[0030] Level 3 (Low Temperature Section): After secondary utilization, the flue gas temperature drops to 100-150℃, which can be directly used to dry carbide slag (moisture content drops from 40% to below 10%) or preheat boiler feedwater.
[0031] (II) Co-treatment of magnesium slag and carbide slag Magnesium slag: activated by calcination in a muffle furnace at 900-950℃ for 1-2 h, and ball-milled through a 150-mesh sieve (≤106 μm).
[0032] Carbide slag: dried to a moisture content of <10% using three-stage waste heat, and ball-milled through a 150-mesh sieve.
[0033] Mixing ratio: Magnesium slag: Carbide slag = 1: (0.5-2) (mass ratio), preferably 1:1.
[0034] (III) Dual-process parallel mineralization system A. MEA process (cement admixture-grade calcium carbonate production line) The mixed residue was mixed with an ethanolamine (MEA) solution at a liquid-solid ratio of 20:1 (mL / g), with a MEA concentration of 1.0-3.0 mol / L (preferably 2.0 mol / L).
[0035] The reaction temperature is 40-60℃ (heated by a secondary waste heat hot water jacket), the stirring speed is 100-300 r / min, and CO2 gas is introduced (flow rate 100-300 mL / min, CO2 source is described later).
[0036] The reaction time is 60-90 min. After the reaction is complete, the mixture is filtered under vacuum, the filter cake is washed three times with anhydrous ethanol, and then dried at 105℃.
[0037] Product specifications: CO2 fixation 16.5%-19.2%, calcium carbonate purity 40%-55%, CaO content approximately 66%. This product can be used directly as a cement admixture. At a dosage of 15%, the 7-day compressive strength is increased by 30% compared to the control (20.88 MPa vs 16.91 MPa).
[0038] B. Ammonia leaching method (multiple ammonia leaching to improve purity, calcium carbide-grade high-purity calcium carbonate production line) The mixed residue is mixed with ammonium chloride (NH4Cl) solution at a liquid-solid ratio of 10:1 (mL / g), and the concentration of NH4Cl is 1.5-2.5 mol / L (preferably 2.0 mol / L).
[0039] The extraction temperature is 40-60℃ (heated by secondary waste heat hot water), and the reaction is stirred for 40-60 min. After filtration, the leachate is obtained (mainly containing CaCl2 and NH3·H2O).
[0040] Leachate purification: Add ammonia to adjust the pH to 10-11, then add NaOH solution to precipitate Al. 3+ Fe 3+ Let it stand and filter.
[0041] Carbonization reaction: After purification, CO2 is introduced into the clear liquid, and the carbonization time is controlled at 9-12 min (optimal 9 min), with a final pH value of ≈9. After carbonization, the solution is filtered, and then leached with ammonia again to improve purity. The filter cake is washed with water three times and dried at 105℃.
[0042] Product specifications: CaO content >98%, MgO <0.03%, purity ≥96%. This product can be returned to calcium carbide plants to replace 30%-50% of limestone.
[0043] (iv) CO2 gas supply The system collects flue gas from the reduction furnace of the magnesia slag plant (CO2 10%-15%) and tail gas from the calcium carbide furnace (CO 60%-80%). The tail gas from the calcium carbide furnace is catalytically combusted (platinum-palladium catalyst, 300-400℃) to convert CO into CO2, which is then mixed with the magnesia slag flue gas. The CO2 concentration is adjusted to 20%-30%, and the mixture is stored in a gas holder. The mixed gas is then supplied to two separate carbonization units.
[0044] (v) Filtrate circulation and ammonia recovery MEA filtrate: After replenishing the lost MEA (approximately 5%-10%), it can be reused directly.
[0045] Ammonia leaching filtrate: after replenishing with NH4Cl, it is recycled; the NH3 released during carbonization is absorbed by water spraying to form 10%-15% ammonia water, which is reused for pH adjustment or sold externally.
[0046] This invention discloses a magnesia slag and calcium carbide slag co-mineralization CO2 and waste heat cascade utilization system. Along the process flow direction, a waste heat cascade recovery zone, a raw material pretreatment zone, a dual-process mineralization zone, and a product post-processing zone are arranged sequentially. In the waste heat cascade recovery system, the slag outlet of the magnesia slag plant and the tail gas emission outlet of the calcium carbide plant are respectively connected to a dual-pressure waste heat boiler via pipelines. The main steam outlet of the boiler is connected to a steam turbine generator set, and the exhaust steam outlet, after passing through a heat exchanger, is connected to the jackets of the MEA reactor and the ammonia leaching reactor via hot water pipelines. In the CO2 gas supply unit, the magnesia slag flue gas pipeline and the calcium carbide furnace tail gas pipeline (via a catalytic combustion device) converge at a gas mixing and blending device, and after mixing, are supplied to the MEA reactor and the carbonization reactor respectively. The raw materials are fed into the two reaction units via a mixing mixer, and the products are output separately after solid-liquid separation, with the filtrate recycled.
[0047] The technical problem to be solved by this invention: 1. A method for co-mineralizing CO2 with magnesium slag and carbide slag is provided, which utilizes the rapid reaction characteristics of Ca(OH)2 in carbide slag to improve the overall calcium conversion rate.
[0048] 2. Provide a waste heat cascade utilization system: the high-temperature section (>800℃) generates electricity, the medium-temperature section (150-300℃) supplies heat to the MEA reactor (40-60℃) and the ammonia leaching reactor (40-60℃), and the low-temperature section (<150℃) dries carbide slag, achieving energy self-sufficiency.
[0049] 3. The integrated MEA process and ammonia leaching process (multiple ammonia leaching) production lines share a CO2 gas source and waste heat, producing medium-purity calcium carbonate (cement admixture) and high-purity calcium carbonate (raw material for calcium carbide plants) respectively, forming a closed-loop resource system.
[0050] 4. Precisely control the carbonization time (9-12 min) to avoid Mg 2+ Co-precipitation ensures high-purity product quality.
[0051] 5. Achieve recycling of amine solution and ammonium salt, reducing reagent consumption.
[0052] Advantages of this invention: 1. Energy self-sufficiency and significant energy savings: Utilizing the sensible heat of magnesia slag and the waste heat from the calcium carbide furnace tail gas to generate electricity and provide cascaded heating, processing 100,000 tons of magnesia slag and 50,000 tons of calcium carbide slag annually can generate approximately 2 million kWh of electricity, saving 1-1.3 million yuan in electricity costs; simultaneously, it provides hot water and low-pressure steam for both processes, replacing electric heating and saving an additional 500,000-800,000 yuan per year. The total thermal energy utilization rate is >85%.
[0053] 2. Dual-process synergy for high-value products: The MEA method rapidly disposes of mixed slag, producing medium-purity calcium carbonate for use as a cement admixture (7-day compressive strength increased by 29%); the ammonia leaching method extracts high-purity calcium carbonate (CaO>98%) for recycling back to the carbide plant. The two production lines share a CO2 gas source and waste heat, achieving a closed loop from solid waste and products to raw materials.
[0054] 3. Multiple ammonia leaching processes improve the purity of calcium carbonate, thereby enhancing product value and performance.
[0055] 4. Mild reaction conditions and low energy consumption: The MEA method fixes carbon at 40℃ and atmospheric pressure, while the ammonia leaching method extracts carbon at 60℃ and atmospheric pressure, neither of which requires high temperature and high pressure. Compared with traditional thermal regeneration (3.6 GJ / t CO2), the energy consumption of chemical regeneration can be reduced to below 0.5 GJ / t CO2.
[0056] 5. Controllable product quality: By controlling the carbonization time to 9-12 minutes, Mg is avoided. 2+ Co-precipitation ensures that the purity of high-purity calcium carbonate is >96%; at the same time, the purity of calcium carbonate in the MEA method product is stable at 40%-55%, which meets the requirements of building material admixtures.
[0057] 6. No secondary pollution: The entire process does not introduce chloride ions (MEA method) or only uses recyclable ammonia salts (ammonia leaching method), the filtrate is recycled, ammonia is recovered, and wastewater is discharged in zero; the mineralized products are stable and there is no risk of heavy metal leaching.
[0058] 7. Excellent economic efficiency. Based on an annual processing capacity of 100,000 tons of magnesium slag and a byproduct of approximately 50,000 cubic meters of calcium carbide furnace tail gas (equivalent to 50,000 tons of calcium carbide slag): Waste heat power generation revenue: Combining sensible heat recovery of magnesium slag with waste heat power generation from calcium carbide furnace tail gas, referencing the Hami project in Xinjiang (which processes 200,000 tons of magnesium slag annually and generates 17.5 million kWh of electricity), approximately 8.75 million kWh of electricity can be generated per year. At an electricity price of 0.5 yuan per kWh, the annual revenue is approximately 4.4 million yuan. At the same time, it provides hot water and low-pressure steam for both processes, saving an additional 500,000 to 800,000 yuan per year by replacing electric heating.
[0059] Product sales revenue: High-purity calcium carbonate (ammonia leaching method) is about 68,100 tons / year, with a market price of 700 yuan / ton, and an annual revenue of about 47.67 million yuan; Medium-purity calcium carbonate (MEA method) is about 26,400 tons / year, with an annual revenue of about 13.2 million yuan, based on the price of 500 yuan / ton for industrial-grade calcium carbonate.
[0060] Savings in solid waste disposal costs: The disposal cost for magnesium slag and calcium carbide slag is 23 yuan / ton, which would save approximately 3.45 million yuan / year for 150,000 tons.
[0061] Carbon emission reduction revenue: Based on a fixed CO2 emission of 20,000 tons / year, the cumulative average transaction price of CCER in 2025 is 70.76 yuan / ton, and the carbon trading revenue is approximately 1.42 million yuan / year.
[0062] Total annual revenue: approximately 70-75 million yuan. After deducting operating costs (ammonia salt and MEA replenishment, electricity consumption, labor, depreciation, etc.), the annual net profit is estimated at 50-55 million yuan, with an investment payback period of 2-3 years.
[0063] Market prospects: Fugu County's magnesium production is expected to reach 557,700 tons in 2025, generating approximately 3 million tons of magnesium slag per year; the national annual production of calcium carbide slag is approximately 50 million tons, indicating abundant solid waste resources and broad prospects for technology promotion.
[0064] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. The components of the embodiments of the present invention described and shown in the accompanying drawings can generally be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the claimed invention, but merely to illustrate selected embodiments of the invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.
[0065] Example 1 Raw materials: magnesium slag (CaO 61.45%) and carbide slag (Ca(OH)2 85%), mixed in a mass ratio of 1:1.
[0066] Waste heat recovery: 1100℃ magnesium slag and 900℃ calcium carbide furnace tail gas enter the waste heat boiler to produce 3.82 MPa, 450℃ steam, which drives a 1.5 MW steam turbine unit to generate electricity. The tail flue gas is then converted into 90℃ hot water through a heat exchanger.
[0067] MEA method: 20 g of mixed residue, 400 mL of 2.0 mol / L MEA, reacted with CO2 at 40℃ and 200 r / min for 90 min to obtain 4.8 g of calcium carbonate of medium purity (CO2 fixation 19.2%).
[0068] Ammonia leaching method: 20 g of mixed residue, 200 mL of 2.0 mol / L NH4Cl, stirred at 60℃ for 40 min, filtered; the filtrate was adjusted to pH=10.5 with ammonia water, and NaOH was added to remove impurities; CO2 was passed through for carbonization for 9 min to obtain 9.6 g of high-purity calcium carbonate (CaO 98.5%).
[0069] Cement admixture test: The MEA method product was added to cement mortar at 15%, and the compressive strength was 20.88 MPa after 7 days.
[0070] Calcium carbide plant recycling: Ammonia leaching process products replace 30% of limestone without reducing calcium carbide yield.
[0071] Example 2 Comparison of different carbonization times in ammonia leaching method Carbonization times were set to 6 min, 9 min, 12 min, and 15 min. The results showed that at 6 min, aragonite was dominant with a Ca content of 30.2%; at 9 min, calcite crystals were fully formed with a Ca content of 59.9%; at 12 min, crystallinity decreased with a Ca content of 35.2%; and at 15 min, an XRD peak of MgCO3 appeared with a Ca content of 22.5%. Therefore, the carbonization time should ideally be controlled between 9 and 12 min.
[0072] Example 3 The effect of repeated ammonia immersion on product performance First ammonia leaching: Take 15.00 g of pretreated magnesium slag, add 200 mL of deionized water, and digest at 50℃ for 40 min. Add 21.40 g of NH4Cl, and stir at 60℃ for 40 min. Filter, and the filtrate is directly carbonized with CO2 for 12 min without purification. Filter, wash, and dry to obtain calcium carbonate product. XRF analysis shows that the CaO content is 96.745% and the MgO content is 0.058%.
[0073] Secondary ammonia leaching: Take 15.00 g of pretreated magnesium slag and perform the same steps as the first ammonia leaching. Filter, wash, and dry to obtain calcium carbonate product. XRF analysis showed that the CaO content was 98.532% and the MgO content was 0.028%. Multiple ammonia leaching significantly improved the product performance.
[0074] Example 4 Effect of carbonization time on purity in ammonia leaching According to the ammonia leaching process, the calcium carbonate purity reaches a maximum of 97.2% at a carbonation time of 9 min, 96.8% at a carbonation time of 12 min, and decreases to 94.5% at 15 min, with EDS showing an increase in Mg content. The optimal carbonation time of 9 min has been confirmed.
[0075] Example 5 Waste heat power generation operation The facility processes 100,000 tons of magnesium slag and 50,000 tons of calcium carbide slag annually, comprehensively recovering and utilizing the sensible heat of the magnesium slag and the waste heat from the calcium carbide furnace tail gas. The waste heat boiler generates hot water to supply two process reactors, replacing electric heating and saving an additional 500,000-800,000 yuan per year. Using a three-stage utilization model (high-temperature power generation, medium-temperature heating, and low-temperature drying), the thermal energy utilization rate is >85%. The total annual power generation is approximately 10.75 million kWh, saving approximately 1,320 tons of standard coal per year and reducing CO2 emissions by approximately 3,500 tons per year.
[0076] Example 6 Raw materials: magnesium slag (CaO content 61.45%) and carbide slag (Ca(OH)2 content 85%), mixed at a mass ratio of 1:0.5.
[0077] Waste heat recovery: 1000℃ magnesium slag and 950℃ calcium carbide furnace exhaust gas enter the waste heat boiler to produce steam, which drives the steam turbine unit to generate electricity. The tail flue gas is then passed through a heat exchanger to produce 60℃ hot water.
[0078] MEA method: 20g of mixed residue, 400mL of 1.0mol / L MEA, CO2 is introduced at 60℃ and 100r / min (flow rate 100mL / min) and reacted for 60min. After filtration, the filter cake is washed and dried to obtain calcium carbonate product.
[0079] Ammonia leaching method: 20g of mixed residue, 200mL of 1.5mol / L NH4Cl, stir at 40℃ for 60min, filter; add ammonia water to adjust the pH value of the filtrate to 10, add NaOH to remove impurities; carbonize with CO2 for 10min, filter, the filter cake is treated with ammonia leaching again, and after filtering, washing and drying, high-purity calcium carbonate product is obtained.
[0080] Example 7 Raw materials: Magnesium slag (CaO content 61.45%) and calcium carbide slag (Ca(OH)2 content 85%) are mixed at a mass ratio of 1:2. The magnesium slag is pre-calcined at 950℃ for 1 hour and then ball-milled through a 150-mesh sieve; the calcium carbide slag is dried using residual heat until the moisture content is <10% and then ball-milled through a 150-mesh sieve.
[0081] Waste heat recovery: 1100℃ magnesium slag and 920℃ calcium carbide furnace tail gas enter the waste heat boiler to produce superheated steam to drive power generation. The tail flue gas is then passed through a heat exchanger to produce 80℃ hot water.
[0082] MEA method: 20g of mixed residue, 400mL of 3.0mol / L MEA, CO2 is introduced at 50℃ and 300r / min (flow rate 300mL / min) and reacted for 75min. After filtration, the filter cake is washed and dried to obtain calcium carbonate product.
[0083] Ammonia leaching method: 20g of mixed residue, 200mL of 2.5mol / L NH4Cl, stir at 50℃ for 50min, filter; add ammonia water to adjust the pH value of the filtrate to 11, add NaOH to remove impurities; carbonize with CO2 for 11min, filter, the filter cake is treated with ammonia leaching again, and after filtering, washing and drying, high-purity calcium carbonate product is obtained.
[0084] CO2 gas source: Collect flue gas from the reduction furnace of the magnesium slag plant (CO2 10-15%) and tail gas from the calcium carbide furnace (CO 60-80%). The tail gas from the calcium carbide furnace is converted from CO to CO2 through catalytic combustion and mixed with the flue gas from the magnesium slag plant to adjust the CO2 volume concentration to 30%.
[0085] Filtrate recycling: The filtrate from the MEA process is reused after being supplemented with ethanolamine; the filtrate from the ammonia leaching process is reused after being supplemented with NH4Cl, and the NH3 released during carbonization is absorbed by water spraying to form 15% ammonia water for reuse.
[0086] Figure 1 This is a flowchart of the overall process of this invention, including waste heat utilization, parallel dual processes, and product destinations. As shown in the diagram, high-temperature magnesium slag and flue gas from the slag plant, and calcium carbide slag and tail gas from the calcium carbide plant are input into the system separately. After mixing and pretreatment, the magnesium slag and calcium carbide slag are divided into two streams: one stream enters the MEA (Medium-Oxide Aging) mineralization unit, where, after reaction, solid-liquid separation, and drying, medium-purity calcium carbonate is produced for use as a cement admixture; the other stream enters the ammonium leaching mineralization unit, where, after leaching, purification, carbonation, solid-liquid separation, and drying, high-purity calcium carbonate is produced and returned to the calcium carbide plant to replace limestone. CO2 for both processes is supplied by catalytic combustion and mixing of magnesium slag flue gas and calcium carbide furnace tail gas. In the waste heat utilization system, the sensible heat of the magnesium slag and the chemical heat of the calcium carbide furnace tail gas are used to generate steam in a waste heat boiler for power generation. The exhaust steam is used to generate hot water via a heat exchanger, which is then supplied to the two reaction units. The tail gas is used to dry the calcium carbide slag. The filtrate from each unit is returned to the corresponding reaction system for recycling, and the ammonia gas generated by the ammonium leaching method is recovered and reused in the purification unit.
[0087] Figure 2 The figure shows the effect of carbonation time on the XRD characteristic peak intensity of calcium carbonate. As can be seen from the figure, the XRD peak is strongest at a carbonation time of 9 minutes, which is the optimal carbonation time.
[0088] Figure 3The image shows a SEM photograph of the MEA product (a mixture of calcite and aragonite) disclosed in Example 1 of this invention. Two typical morphologies can be observed in the image: regular cubic or rhombohedral particles with a particle size of about 1~3 μm, which are calcite crystals; and irregular spherical or flower-shaped particles with a particle size of about 0.5~2 μm, which are aragonite crystals. The coexistence of the two morphologies and good dispersibility indicate that the product is a mixture of calcite and aragonite crystals.
[0089] Figure 4 The image shows a SEM image of the product obtained by the multiple ammonia leaching method disclosed in Example 3 of this invention. As can be seen from the image, aragonite and calcite coexist and are well dispersed.
[0090] Figure 5 The image shows the Raman spectrum of the ammonia leaching product disclosed in Example 4 of this invention. As can be seen from the image, the Raman peak is strongest at a carbonization time of 9 minutes, which is the optimal carbonization time.
[0091] Figure 6 The image shows the cement compressive strength test results for the blank control group (without calcium carbonate). Figure 7 This is a compressive strength test diagram of cement with a calcium carbonate content of 15% as disclosed in Example 1 of this invention. The lightweight calcium carbonate prepared in Example 1 was used as an admixture in cement mortar for application tests. PO 42.5 ordinary Portland cement was used, and the standard sand was Chinese ISO standard sand. The mix ratio was cement:sand:water = 1:3:0.5. Calcium carbonate replaced cement at 15% of its mass, and cylindrical specimens with a diameter of φ50 mm × 50 mm were prepared. After standard curing for 7 days, the compressive strength was tested. The results showed that the compressive strength of the cement column in the blank group was 33.2 kN and 16.91 MPa, while the compressive strength of the mortar specimen with 15% lightweight calcium carbonate was 41 kN and 20.88 MPa, which is about 30% higher than the blank group (without calcium carbonate). This indicates that the calcium carbonate prepared by this invention has a good filling and reinforcing effect and can be used in the building materials field.
[0092] In summary, this invention provides a method and system for the synergistic mineralization of magnesia slag and calcium carbide slag to utilize CO2 and waste heat in a cascade manner. Magnesia slag and calcium carbide slag are mixed to construct a three-stage waste heat utilization system consisting of high-temperature power generation, medium-temperature heating, and low-temperature drying. The mixed slag is supplied to the MEA mineralization process (40℃ atmospheric pressure) and the ammonia leaching mineralization process (60℃ atmospheric pressure) for parallel operation. The two processes share the CO2 gas source and waste heat resources. The ammonia leaching process uses multiple ammonia leaching cycles for purification and precisely controls the carbonization time to 9-12 minutes, while simultaneously achieving full recycling of the filtrate and the released ammonia gas. This invention significantly improves calcium conversion rate through the synergistic effect of magnesium slag and calcium carbide slag. It achieves a thermal energy utilization rate of over 85% and system energy self-sufficiency through three-stage waste heat utilization. The invention utilizes a dual-process approach of MEA and ammonia leaching to produce cement admixture-grade calcium carbonate and calcium carbide-grade high-purity calcium carbonate, respectively. Precise control of multiple ammonia leaching and carbonation times ensures high-purity product quality. Zero wastewater discharge is achieved through the full recycling of filtrate and ammonia. This invention fundamentally solves the technical problems of high energy consumption for organic amine and adsorbent regeneration, insufficient co-utilization of solid waste, serious waste of waste heat resources, and limited added value of products in existing CO2 mineralization technologies, and has broad prospects for industrial application.
[0093] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for the synergistic mineralization of CO2 from magnesium slag and calcium carbide slag and the cascade utilization of waste heat, characterized in that, include: Magnesium slag and calcium carbide slag were pretreated separately, and the pretreated magnesium slag was mixed with calcium carbide slag to obtain mixed slag; The sensible heat from the magnesium slag discharge and the waste heat from the calcium carbide furnace tail gas are recovered and utilized in stages. The high-temperature stage is used to generate steam and generate electricity, the medium-temperature stage is used to supply heat to the mineralization reaction, and the low-temperature stage is used to dry the calcium carbide slag. Collect flue gas from the reduction furnace of the magnesium slag plant and tail gas from the calcium carbide furnace, catalytically combust CO in the tail gas of the calcium carbide furnace to convert it into CO2, and mix it with the flue gas from the reduction furnace of the magnesium slag plant to obtain a CO2 gas source for the mineralization reaction. The mixed slag is divided into two streams. The first stream uses the MEA method, where the mixed slag is mixed with an ethanolamine solution, and under the heat provided in the medium-temperature section, a CO2 gas source is introduced to carry out a mineralization reaction, followed by solid-liquid separation to obtain calcium carbonate products for cement admixtures. The second stream uses the ammonia leaching method, where the mixed slag is mixed with an ammonium chloride solution for ammonia leaching, and solid-liquid separation is performed to obtain a leachate. After purification, the leachate is introduced into the CO2 gas source for a carbonation reaction, followed by solid-liquid separation. The resulting filter cake is then subjected to ammonia leaching again to obtain high-purity calcium carbonate. The filtrate from the mineralization reaction is replenished with ethanolamine and then reused for MEA mineralization. The filtrate from ammonia leaching is replenished with ammonium chloride and then recycled. The NH3 released during carbonization is also recovered.
2. The method for synergistic mineralization of CO2 and cascade utilization of waste heat by magnesium slag and carbide slag according to claim 1, characterized in that, The pretreatment of the magnesium slag includes: calcining the magnesium slag at 900~950℃ for 1~2 h to activate it, and then ball milling it and passing it through a 150-mesh sieve; The pretreatment of the carbide slag includes: using the residual heat of the low-temperature section to dry the carbide slag to a moisture content of less than 10%, and then ball-milling it and passing it through a 150-mesh sieve. The mass ratio of magnesium slag to calcium carbide slag is 1:(0.5~2).
3. The method for synergistic mineralization of CO2 and cascade utilization of waste heat by magnesium slag and carbide slag according to claim 1, characterized in that, The high-temperature section introduces the sensible heat carried by the magnesium slag at 1000~1100℃ and the waste heat of the calcium carbide furnace tail gas at 900~950℃ into the waste heat recovery system, which generates superheated steam through a dual-pressure waste heat boiler and drives the steam turbine generator set to generate electricity. The low-pressure steam generated after power generation or the flue gas discharged from the waste heat boiler are used to generate hot water through heat exchange, which is then used as the heat source for the medium-temperature section to supply heat to the MEA method mineralization and the ammonia leaching method mineralization. The flue gas after being utilized in the medium-temperature section is used as a heat source in the low-temperature section for drying carbide slag or preheating boiler feedwater.
4. The method for synergistic mineralization of CO2 and cascade utilization of waste heat by magnesium slag and carbide slag according to claim 1, characterized in that, The MEA mineralization process includes: mixing the mixed slag with an ethanolamine solution of 1.0-3.0 mol / L at a liquid-to-solid ratio of 20:1 mL / g, and reacting the mixture with CO2 gas at a flow rate of 100-300 mL / min at 40-60℃ and 100-300 r / min for 60-90 min. After the reaction is complete, vacuum filtration is performed, and the filter cake is washed with anhydrous ethanol at least three times and then dried.
5. The method for synergistic mineralization of CO2 and cascade utilization of waste heat by magnesium slag and carbide slag according to claim 1, characterized in that, The ammonia leaching process includes: mixing the mixed residue with an ammonium chloride solution of 1.5-2.5 mol / L at a liquid-to-solid ratio of 10:1 mL / g, reacting at 40-60°C for 40-60 min, and then filtering to obtain a leachate; Ammonia was added to the leachate to adjust the pH to 10-11, and then NaOH solution was added to precipitate Al. 3+ and Fe 3+ The purified liquid was obtained by standing and filtering. CO2 is introduced into the purified liquid to carry out a carbonization reaction for 9-12 minutes. The final pH value of carbonization is 9. After carbonization, the liquid is filtered, and the resulting filter cake is subjected to ammonia leaching again. Then, after solid-liquid separation, water washing and drying, high-purity calcium carbonate is obtained.
6. The method for synergistic mineralization of CO2 and cascade utilization of waste heat by magnesium slag and carbide slag according to claim 1, characterized in that, The CO2 volume content in the flue gas from the reduction furnace of the magnesium slag plant is 10%~15%, and the CO volume content in the tail gas from the calcium carbide furnace is 60%~80%. The tail gas from the calcium carbide furnace is catalytically combusted at 300-400℃ using a platinum-palladium catalyst to convert CO into CO2, and then mixed with the flue gas from the reduction furnace of the magnesium slag plant. The volume concentration of CO2 in the mixed gas is adjusted to 20%-30%. The filtrate from the MEA mineralization process is recycled after being supplemented with 5% to 10% ethanolamine. The filtrate from the ammonia leaching process is recycled after being supplemented with ammonium chloride. The NH3 released during carbonization is absorbed by water spraying to form ammonia water with a mass concentration of 10% to 15%, which is then reused for pH adjustment.
7. A system for the synergistic mineralization of CO2 and waste heat from magnesium slag and calcium carbide slag, characterized in that, include: Waste heat recovery unit, raw material pretreatment unit, CO2 gas supply unit, MEA mineralization unit and ammonia leaching mineralization unit; The waste heat cascade recovery unit is connected to the slag outlet of the magnesium slag plant and the tail gas emission outlet of the calcium carbide plant, respectively, for recovering the sensible heat from the magnesium slag discharge and the waste heat from the tail gas of the calcium carbide furnace; the waste heat cascade recovery unit has a high-temperature waste heat utilization end, a medium-temperature waste heat utilization end and a low-temperature waste heat utilization end, the high-temperature waste heat utilization end is used for power generation, the medium-temperature waste heat utilization end is connected to the MEA method mineralization unit and the ammonia leaching method mineralization unit respectively to supply heat to them, and the low-temperature waste heat utilization end is connected to the raw material pretreatment unit for drying calcium carbide slag. The raw material pretreatment unit is used to pretreat and mix magnesium slag and carbide slag. The mixed material outlet of the raw material pretreatment unit is divided into two paths, one of which is connected to the material inlet of the MEA mineralization unit and the other is connected to the material inlet of the ammonia leaching mineralization unit. The gas inlet of the CO2 gas supply unit is connected to the flue gas source of the magnesium slag plant reduction furnace and the tail gas source of the calcium carbide furnace, respectively. The gas outlet of the CO2 gas supply unit is divided into two paths, one of which is connected to the MEA mineralization unit and the other is connected to the ammonia leaching mineralization unit. The MEA mineralization unit is equipped with a MEA filtrate recycling path, and the ammonia leaching mineralization unit is equipped with an ammonia leaching filtrate recycling path and an ammonia recovery and recycling path.
8. The magnesia slag and carbide slag co-mineralization CO2 and waste heat cascade utilization system according to claim 7, characterized in that, The waste heat cascade recovery unit includes a dual-pressure waste heat boiler, a steam turbine generator set, and a heat exchanger. The slag outlet of the magnesium slag plant and the tail gas outlet of the calcium carbide plant are respectively connected to the dual-pressure waste heat boiler, and the main steam outlet of the dual-pressure waste heat boiler is connected to the steam turbine generator set. The exhaust port of the steam turbine generator set is connected to the heat exchanger, and the hot water outlet of the heat exchanger is connected to the MEA reactor jacket in the MEA mineralization unit and the ammonia leaching reactor jacket in the ammonia leaching mineralization unit through hot water pipes respectively. The low-temperature flue gas outlet of the waste heat cascade recovery unit is connected to the carbide slag drying section in the raw material pretreatment unit.
9. The magnesia slag and carbide slag co-mineralization CO2 and waste heat cascade utilization system according to claim 7, characterized in that, The raw material pretreatment unit includes a magnesium slag pretreatment section, a carbide slag pretreatment section, and a mixing mixer. The material outlets of the magnesium slag pretreatment section and the carbide slag pretreatment section are respectively connected to the material inlet of the mixing mixer. The material outlet of the mixing mixer is respectively connected to the MEA mineralization unit and the ammonia leaching mineralization unit. The CO2 gas supply unit includes a magnesium slag flue gas pipeline, a calcium carbide furnace tail gas pipeline, a catalytic combustion device, and a gas mixing and blending device. The magnesium slag flue gas pipeline is connected to the gas mixing and blending device, and the calcium carbide furnace tail gas pipeline is connected to the gas mixing and blending device via the catalytic combustion device. The gas outlet of the gas mixing and blending device is connected to the MEA reactor in the MEA mineralization unit and the carbonization reactor in the ammonia leaching mineralization unit, respectively.
10. The magnesia slag and carbide slag co-mineralization CO2 and waste heat cascade utilization system according to claim 7, characterized in that, The MEA mineralization unit includes an MEA reactor and a solid-liquid separation section connected in sequence. The filtrate outlet of the solid-liquid separation section is connected to the MEA reactor through the MEA filtrate recycling path, so that the MEA filtrate can be returned to the MEA reactor after replenishing MEA. The ammonia leaching mineralization unit includes an ammonia leaching reactor, a purification section, a carbonization reactor, and a solid-liquid separation section connected in sequence. The filtrate outlet of the ammonia leaching mineralization unit is connected to the ammonia leaching reactor through the ammonia leaching filtrate recycling path, so that the ammonia leaching filtrate can be recycled after being supplemented with ammonium chloride. The gas outlet of the carbonization reactor is connected to the ammonia recovery section, which is used to absorb the NH3 released during the carbonization process by water spraying and to reuse the resulting ammonia water in the purification section.
Citation Information
Patent Citations
CO2 capture from flue gas and coupled system for CO2 mineralization based on industrial solid waste
CN114768501B
System and method for preparing negative carbon product through cooperation of carbon dioxide capture and solid waste mineralization
CN122141409A