A method for reducing the incidence of surface cracking in thin-strip cast-rolled hot-rolled strip steel

By precisely matching process parameters and actively intervening in the non-equilibrium solidification process, and synergistically controlling the stress and temperature fields, the cracking problem of thin strip casting and hot rolling steel was solved, achieving high-quality and stable production.

CN123102755APending Publication Date: 2026-11-17ZHANGJIAGANG ZHONGMEI UCS TECH CO LTD +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611377143.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-07
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Thin-strip cast-rolled hot-rolled strip steel is prone to cracking during solidification and deformation, which affects product quality and production stability, and existing technologies are unable to effectively solve this problem.

Method used

By precisely matching process parameters and actively intervening in the non-equilibrium solidification process, the stress and temperature fields are synergistically controlled, including controlling the tundish temperature, casting strip thickness, roller brush process parameters, and chemical composition, especially the P content, to suppress crack initiation and propagation.

Benefits of technology

Under existing production conditions, no additional equipment is required, which significantly reduces the cracking rate of thin strip cast-rolled hot-rolled strip steel and improves product qualification rate and production stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102755A_ABST
    Figure CN123102755A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of steel production technology and relates to a method for reducing the surface cracking rate of hot-rolled strip steel produced by thin-strip casting and rolling. The method mainly includes: controlling the tundish temperature; for low-carbon steel production, the tundish temperature is controlled at 1610~1630℃; for medium- and high-carbon steel production, the tundish temperature is controlled at 1580~1615℃; controlling the roller brush vibration amplitude to ≤30 lbin, the roller brush rotation speed amplitude to ±20 r / min, and the roller brush torque amplitude to ±20 ibf; controlling the strip thickness to 1.85~2.5 mm; and controlling the hot-rolling reduction rate to ≥22%. By controlling the tundish temperature, roller brush vibration, roller brush rotation speed and torque, strip thickness, and hot-rolling reduction rate, this invention reduces the surface cracking rate of hot-rolled thin strip steel produced using the thin-strip casting and rolling process, thereby improving the product qualification rate and efficiency of thin-strip cast hot-rolled strip steel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of steel production technology and relates to a method for reducing the incidence of surface cracking in thin-strip cast-rolled hot-rolled strip steel. Background Technology

[0002] Thin strip casting and rolling technology is a new technology that uses molten steel as raw material and two casting rolls rotating in opposite directions as crystallizers to directly produce strip steel from molten steel. The key feature of this technology is that molten steel is directly injected into the gap between the rotating casting rolls, allowing it to undergo pressure processing and plastic deformation while simultaneously crystallizing and solidifying, thus completing the forming process from molten steel to ultra-thin cast strip. After passing through a hot rolling mill and completing the plastic processing of the cast strip, the produced ultra-thin cast strip is formed into a hot-rolled strip steel product that meets the user's dimensional specifications.

[0003] Thin strip casting and rolling technology, as an important development direction in the field of near-net-shape processing, faces a critical bottleneck in product cracking, hindering its technological maturity and industrial application. Because this technology allows the molten metal to complete the solidification and deformation coupling process within milliseconds to seconds, the evolution of the cast strip's microstructure and stress field distribution are highly unbalanced. This results in the strip steel being subjected to multiple superimposed effects of solidification shrinkage stress, thermal stress, and rolling mechanical stress during the final stage of solidification and the rolling stage, potentially leading to cracking. Strip cracking not only significantly degrades the initial quality of the cast strip but also forms stress concentration sources during subsequent cold rolling and deep processing, inducing strip breakage or finished product failure, severely impacting product yield and production line stability.

[0004] Therefore, solving the cracking problem of hot-rolled strip steel in thin strip casting is a prerequisite for achieving high-quality and stable manufacturing in thin strip casting technology. Summary of the Invention

[0005] This invention provides a method for reducing the surface cracking rate of thin-strip cast-rolled hot-rolled strip steel. The method of this invention adopts a completely different approach from existing technologies, requiring no additional equipment. Its core lies in achieving coordinated control of the stress and temperature fields through precise matching of process parameters and active intervention in the non-equilibrium solidification process, thereby effectively suppressing crack initiation and propagation.

[0006] Specifically, the inventors discovered that surface cracking in thin-strip cast-rolled hot-rolled steel products involves the following mechanism: When molten steel cools on the surface of a copper casting roll to form a billet shell, a high-temperature ferrite δ phase is initially formed. As cooling continues, the high-temperature ferrite δ phase subsequently transforms into austenite γ phase. This phase transformation process is accompanied by approximately 0.3% volume shrinkage. If the thickness or strength of the solid billet shell formed at the start of the solid-state phase transformation is too low, the strip steel is prone to cracking under stress. The inventors recognize that the formation of surface cracks in strip steel is easily affected by multiple factors, including the thermal conductivity of the molten steel itself, the thermal conduction rate at the interface between the molten steel and the casting roll, and the uniformity of heat transfer on the surface of the casting roll during the cooling process.

[0007] Through the inventor's research, the problem of strip cracking can be effectively reduced by adjusting the following process parameters without the need to add additional equipment.

[0008] (1) Tundish temperature: The inventors found that excessively high tundish temperature can lead to a thin billet shell and segregation, while excessively low tundish temperature can worsen the uniformity of billet shell growth and thus affect the strength of the billet shell. Furthermore, the inventors proposed different tundish temperature ranges for different steel grades to adapt to the thermal stress sensitivity coefficient of different steel grades.

[0009] (2) Cast strip thickness: The inventors found that by appropriately increasing the thickness of the cast strip, the interfacial heat transfer rate can be reduced, thermal stress can be reduced, heat transfer uniformity can be improved, and the ability of the billet shell to resist cracking can be improved.

[0010] (3) Roller brush process parameters: The inventors found that the thickness of the oxide film on the surface of the casting roll significantly affects the interfacial heat transfer between the molten steel and the casting roll. In particular, both excessively thin and excessively thick oxide films will inhibit interfacial heat transfer. If the roller brush operates abnormally, it will also cause local oxide films to be too thick, resulting in uneven solidification and thus causing cracks. Therefore, the working condition of the roller brush can be monitored and adjusted during production. For example, the vibration amplitude of the roller brush can be controlled to ≤30 lb. The rotational speed amplitude of the roller brush is controlled at ±20 r / min, and the torque amplitude of the roller brush is controlled at ±20 ibf.

[0011] (4) Chemical composition: Chemical element P is a strong grain boundary embrittlement element. The inventors found that, for thin strip cast hot-rolled strip steel, the segregation and aggregation behavior of chemical element P will greatly weaken the strength of the billet shell, thus having a significant impact on the cracking of the strip steel.

[0012] (5) Strip reduction rate: There are often solidification defects such as pores and looseness inside the cast strip. The inventors have found that, for thin strip cast hot-rolled steel, by setting a large hot rolling reduction rate, these pores can be pressed together through plastic deformation, so as to avoid these micro defects being left in the finished product and becoming possible crack sources that lead to cracking.

[0013] To achieve the aforementioned technical objectives, the present invention adopts the following technical solutions and methods.

[0014] According to a first aspect of the present invention, a method for reducing the incidence of surface cracking in thin-strip cast-rolled hot-rolled strip steel is provided, the method comprising the following steps: (1) Steel is obtained through smelting; (2) The molten steel obtained in step (1) is transferred to the tundish through the long nozzle. When producing low carbon steel, the tundish temperature is controlled at 1610~1630℃, and when producing high carbon steel, the tundish temperature is controlled at 1580~1615℃. (3) The molten steel obtained in step (2) is continuously cast into a thin strip through two counter-rotating casting rolls to obtain a casting strip, wherein the thickness of the casting strip is controlled to be 1.85~2.5 mm, and the surface of the casting rolls is cleaned using a roller brush, wherein the vibration amplitude of the roller brush is controlled to be ≤30 lb. The rotational speed amplitude of the roller brush is controlled at ±20 r / min, and the torque amplitude of the roller brush is controlled at ±20 lbf. (4) The cast strip obtained in step (3) is hot rolled to obtain hot rolled thin strip.

[0015] According to the method for reducing the surface cracking rate of thin strip cast hot-rolled strip steel of the present invention, preferably, in step (1), the P content of molten steel is controlled to be ≤0.02%.

[0016] According to the method for reducing the surface cracking rate of hot-rolled strip steel according to the present invention, preferably, in step (4), the total reduction rate of hot rolling is controlled to be ≥22%.

[0017] According to the method for reducing the surface cracking rate of thin strip cast-rolled hot-rolled strip steel of the present invention, preferably, in step (4), the hot rolling is a single hot rolling.

[0018] According to the method for reducing the surface cracking rate of hot-rolled strip steel according to the present invention, preferably, in step (4), the total reduction rate of hot rolling is controlled to be ≥30%.

[0019] According to the method of reducing the surface cracking rate of hot-rolled strip steel according to the present invention, preferably, in step (4), the total reduction rate of hot rolling is controlled to be ≥35%.

[0020] According to the method for reducing the surface cracking rate of hot-rolled strip steel according to the present invention, preferably, the method further includes the following steps: (5) cooling the hot-rolled strip with air mist and then winding it to obtain a hot-rolled strip coil.

[0021] According to the method of reducing the surface cracking rate of thin strip cast hot-rolled strip steel of the present invention, preferably, in step (1), steelmaking is carried out by EAF electric furnace or converter, VD vacuum decarburization and deoxidation, and LF refining to obtain molten steel with qualified composition.

[0022] According to the method for reducing the surface cracking rate of hot-rolled strip steel according to the present invention, preferably, in step (3), the vibration amplitude of the roller brush is controlled to be ≤20 lb. The rotational speed amplitude of the roller brush is controlled at ±15 r / min, and the torque amplitude of the roller brush is controlled at ±15 lbf.

[0023] According to a second aspect of the present invention, a hot-rolled thin strip steel is provided, wherein the production process of the hot-rolled thin strip steel is controlled by the aforementioned method, wherein the cracking rate of the hot-rolled thin strip steel is not higher than 0.5%.

[0024] Beneficial technical effects

[0025] Compared with the prior art, the technical concept and corresponding technical solution of the present invention can achieve at least the following beneficial technical effects: The technical solution of this invention is applicable to thin strip casting and rolling production lines. Under existing production conditions, no additional equipment is required. By optimizing casting and rolling process parameters and molten steel chemical composition, and through precise matching of process parameters and active intervention in the non-equilibrium solidification process, the stress field and temperature field are synergistically controlled, effectively suppressing crack initiation and propagation. This effectively reduces the cracking rate on the surface of thin strip casting and rolling hot-rolled strip steel, and significantly improves the product qualification rate and production stability of thin strip casting and rolling hot-rolled strip steel. Attached Figure Description

[0026] To more clearly illustrate the technical concept and solution of the present invention, the accompanying drawings will be briefly described below.

[0027] Figure 1 This is a schematic diagram of the process and equipment for producing thin strip cast-rolled hot-rolled strip steel according to an embodiment of the present invention.

[0028] Figure 2 A metallographic cross-section of surface cracks in medium carbon steel is shown.

[0029] Figure 3 A metallographic cross-section of surface cracks in high-carbon steel is shown. Detailed Implementation

[0030] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of the embodiments of this invention will be clearly and completely described below. Obviously, the described embodiments are only some, not all, of the embodiments of this invention. All other embodiments obtained by those skilled in the art based on the described embodiments of this invention without creative effort are within the scope of protection of this invention.

[0031] Unless otherwise defined, the technical or scientific terms used in this invention shall have the ordinary meaning as understood by one of ordinary skill in the art to which this invention pertains.

[0032] The following are embodiments of the present invention. The described embodiments are only a part of the embodiments of the present invention. All other embodiments that can be obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.

[0033] Figure 1 A schematic diagram of a thin strip casting and rolling process according to an embodiment of the present invention is shown. According to an embodiment of the present invention, molten steel is obtained through smelting, for example, by using an EAF electric furnace or converter for steelmaking, VD vacuum decarburization and deoxidation, and LF refining to obtain molten steel with qualified composition. According to an embodiment of the present invention, the P content of the molten steel can be controlled to ≤0.02%.

[0034] like Figure 1 As shown, molten steel obtained from smelting is transferred to tundish 2 through a long nozzle. For example, molten steel is transferred from ladle 1 to tundish 2 through a long nozzle. When producing low-carbon steel, the tundish temperature is controlled at 1610~1630℃; when producing high-carbon steel, the tundish temperature is controlled at 1580~1615℃. According to an embodiment of the invention, molten steel from tundish 2 can be continuously cast into a thin strip using two counter-rotating casting rolls (e.g., first casting roll 41 and second casting roll 42). For example, molten steel from tundish 2 flows through transition ladle 3 to the molten pool formed between the two counter-rotating casting rolls. According to an embodiment of the invention, the thickness of the cast strip is controlled at 1.85~2.5 mm.

[0035] like Figure 1 Further illustrating, according to an embodiment of the invention, roller brushes are used to clean the surface of the casting rolls. For example, a first roller brush 51 is configured to clean the first casting roll 41, and a second roller brush 52 is configured to clean the second casting roll 42. According to an embodiment of the invention, the vibration amplitude of the roller brushes is controlled to ≤30 lb. In this embodiment, the rotational speed amplitude of the roller brush is controlled to be ±20 r / min, and the torque amplitude of the roller brush is controlled to be ±20 lbf. According to another embodiment of the invention, the vibration amplitude of the roller brush is controlled to be ≤20 lbf. In this configuration, the rotational speed amplitude of the roller brush is controlled at ±15 r / min, and the torque amplitude of the roller brush is controlled at ±15 lbf. For example... Figure 1 As shown, the obtained cast strip will undergo hot rolling, and a hot box can be installed between the casting rolls and the hot rolling mill, for example... Figure 1 The first hot box 61, the second hot box 62, and the third hot box 63 are shown.

[0036] Continue to refer to Figure 1 The obtained cast strip is hot-rolled at hot rolling mill 7 to obtain hot-rolled thin strip. According to an embodiment of this disclosure, the hot rolling is a single-pass hot rolling, for example, hot rolling mill 7 is a single-stand hot rolling mill. According to an embodiment of this disclosure, the total reduction rate of hot rolling is ≥22%, for example, the reduction rate of a single-pass hot rolling is ≥22%. According to another embodiment of this disclosure, the total reduction rate of hot rolling is ≥30%. According to yet another embodiment of this disclosure, the total reduction rate of hot rolling is ≥35%.

[0037] like Figure 1 As shown, the hot-rolled thin strip can be cooled by air mist at the air mist cooling device 8, and then wound at the coiler 9 to obtain a hot-rolled thin strip coil. This results in a hot-rolled thin strip coil with a reduced cracking rate. According to embodiments of this disclosure, the cracking rate of the obtained hot-rolled thin strip steel is no higher than 0.5%, in other words, the cracking rate of the product is no higher than 0.5%. Figure 2 The image shows a metallographic cross-section of surface cracks in medium carbon steel. Figure 3 A metallographic cross-section of surface cracking in high-carbon steel is shown, illustrating that cracks in strip steel are prone to initiation on the strip surface. According to embodiments of the present invention, the cracking rate of the product can be reduced by effectively treating the interfacial interaction between molten steel and the casting roll.

[0038] The technical solution of the present invention will be further described in detail below with reference to specific embodiments.

[0039] Example 1

[0040] Low-carbon steel, with a chemical composition of 0.025% C and 0.017% P, is produced by electric furnace smelting. The molten steel, meeting the required composition, is transferred to the tundish through a long nozzle at a temperature of 1630℃. Thin strip is continuously cast using two counter-rotating casting rolls, while a roller brush cleans the roll surface with a vibration amplitude of 20 lb. The roller brush rotation speed amplitude is 10 r / min, the roller brush torque amplitude is 10 ibf, the cast strip thickness is 1.85 mm, the cast strip is hot rolled in one pass with a reduction rate of 40%, cooled by air mist, and then coiled to obtain a low-carbon hot-rolled thin strip coil. Under the control of these process parameters, the product crack incidence rate is 0%.

[0041] Example 2

[0042] Medium carbon steel, with a chemical composition of 0.25% C and 0.013% P, is produced by converter smelting. The molten steel, meeting the required composition, is transferred to the tundish through a long nozzle at a temperature of 1610℃. Thin strip is continuously cast using two counter-rotating casting rolls, while a roller brush cleans the roll surface with a vibration amplitude of 15 lb. The roller brush rotation speed amplitude was 15 r / min, the roller brush torque amplitude was 15 ibf, the cast strip thickness was 1.95 mm, the cast strip was hot rolled in one pass with a reduction rate of 35%, cooled by air mist, and then coiled to obtain a medium carbon hot-rolled thin strip coil. Under the control of these process parameters, the product crack incidence rate was 0.1%.

[0043] Example 3

[0044] High-carbon steel, with a chemical composition of 0.5% C and 0.01% P, is produced by converter smelting. The molten steel, meeting the required composition, is transferred to the tundish through a long nozzle at a temperature of 1585℃. Thin strip is continuously cast using two counter-rotating casting rolls, while a roller brush cleans the roll surface with a vibration amplitude of 10 lb. The roller brush rotation speed amplitude was 20 r / min, the roller brush torque amplitude was 20 ibf, the cast strip thickness was 2.1 mm, the cast strip was hot rolled in one pass with a reduction rate of 30%, cooled by air mist, and then coiled to obtain a high-carbon hot-rolled thin strip coil. Under the control of these process parameters, the product crack incidence rate was 0.3%.

[0045] The above description is only a specific embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A method for reducing the incidence of surface cracking in thin-strip cast-rolled hot-rolled strip steel, characterized in that, The method includes the following steps: (1) Steel is obtained through smelting; (2) The molten steel obtained in step (1) is transferred to the tundish through the long nozzle. When producing low carbon steel, the tundish temperature is controlled at 1610~1630℃, and when producing high carbon steel, the tundish temperature is controlled at 1580~1615℃. (3) The molten steel obtained in step (2) is continuously cast into a thin strip through two counter-rotating casting rolls to obtain a casting strip, wherein the thickness of the casting strip is controlled to be 1.85~2.5 mm, and the surface of the casting rolls is cleaned using a roller brush, wherein the vibration amplitude of the roller brush is controlled to be ≤30 lb. The rotational speed amplitude of the roller brush is controlled at ±20 r / min, and the torque amplitude of the roller brush is controlled at ±20 lbf. (4) The cast strip obtained in step (3) is hot rolled to obtain hot rolled thin strip.

2. The method for reducing the surface cracking rate of thin-strip cast-rolled hot-rolled strip steel according to claim 1, characterized in that: In step (1), the P content of the molten steel is controlled to be ≤0.02%.

3. The method for reducing the surface cracking rate of thin-strip cast-rolled hot-rolled strip steel according to claim 1, characterized in that: In step (4), the total reduction rate of the hot rolling is controlled to be ≥22%.

4. The method for reducing the surface cracking rate of thin-strip cast-rolled hot-rolled strip steel according to claim 3, characterized in that: In step (4), the hot rolling is a single hot rolling process.

5. The method for reducing the surface cracking rate of thin-strip cast-rolled hot-rolled strip steel according to claim 4, characterized in that: In step (4), the total reduction rate of the hot rolling is controlled to be ≥30%.

6. The method for reducing the surface cracking rate of thin-strip cast-rolled hot-rolled strip steel according to claim 5, characterized in that: In step (4), the total reduction rate of the hot rolling is controlled to be ≥35%.

7. The method for reducing the surface cracking rate of thin-strip cast-rolled hot-rolled strip steel according to claim 1, characterized in that, The method further includes the following steps: (5) The hot-rolled strip is cooled by air mist and then wound up to obtain a hot-rolled strip coil.

8. The method for reducing the surface cracking rate of thin-strip cast-rolled hot-rolled strip steel according to claim 1, characterized in that: In step (1), steelmaking is carried out using an EAF electric furnace or converter, VD vacuum decarburization and deoxidation, and LF refining to obtain molten steel with qualified composition.

9. The method for reducing the surface cracking rate of thin-strip cast-rolled hot-rolled strip steel according to claim 1, characterized in that: In step (3), the vibration amplitude of the roller brush is controlled to be ≤20 lb. The rotational speed amplitude of the roller brush is controlled at ±15 r / min, and the torque amplitude of the roller brush is controlled at ±15 lbf.

10. A hot-rolled thin strip steel, characterized in that, The production process of the hot-rolled thin strip steel is controlled by the method according to any one of claims 1 to 9, wherein the cracking rate of the hot-rolled thin strip steel is not higher than 0.5%.