A method for preparing bimetallic material spray-rolled composite plates and coils.

By using the spray rolling method, molten metal is sprayed onto the surface of the substrate, solving the problem of high surface flatness requirements between the substrate and the cladding. This enables efficient and low-cost preparation of bimetallic composite plates and rolls, improving the shear strength and application range of the composite interface.

CN123102968APending Publication Date: 2026-11-17刘厚新
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611073982.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing methods for preparing bimetallic sprayed composite plates and rolls, the surface flatness requirements of the substrate and the coating are high, which leads to long pretreatment time and reduces the preparation efficiency.

Method used

The spray-rolling method is adopted, which involves sandblasting the substrate and atomizing the molten metal coating onto the substrate surface, eliminating the need for precision milling and directly forming a composite billet, thus simplifying the preparation process.

Benefits of technology

It improves preparation efficiency, reduces production costs, achieves a metallurgical bonding state at the composite interface, has a shear strength greater than 300 MPa, expands the application range, and is suitable for various composite materials and layer thickness requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102968A_ABST
    Figure CN123102968A_ABST
Patent Text Reader

Abstract

This invention relates to the field of metal composite materials technology, specifically to a method for preparing bimetallic material spray-coated composite plates and coils, comprising: Step 1, substrate selection: selecting a steel plate of suitable size as the substrate; Step 2, substrate pretreatment: sandblasting the surface of the substrate; Step 3, cladding smelting: melting the cladding material to obtain molten cladding metal; Step 4, spray-coating: conveying the substrate to a spray chamber for preheating, then spraying the molten cladding metal onto the surface of the substrate to obtain a single-sided composite billet; Step 5, cooling: cooling the single-sided composite billet to room temperature; Step 6, double-sided composite billet fabrication: flipping the single-sided composite billet and repeating steps 2 to 5 to obtain a double-sided composite billet; Step 7, rolling: rolling the single-sided and double-sided composite billets. This invention directly atomizes and sprays the molten cladding metal onto the surface of the substrate to form a composite billet, requiring only sandblasting, eliminating the need for precision milling and shortening the preparation cycle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metal composite materials technology, specifically to a method for preparing composite plates and coils by spraying and rolling bimetallic materials. Background Technology

[0002] Bimetallic composite plates and coils include composites of different metal materials such as stainless steel and carbon steel, titanium and carbon steel, and copper and carbon steel. The following explanation uses stainless steel and carbon steel composite plates as an example.

[0003] The base material of stainless steel composite plates can use various ordinary carbon steels and special steels such as Q235B, Q345R, and 20R. The cladding material can use various grades of stainless steel such as 304, 316L, and 1Cr13. Materials and thicknesses can be freely combined to meet the needs of different users. Stainless steel composite plates not only possess the corrosion resistance of stainless steel but also the good mechanical strength and processing performance of carbon steel, making them a new type of industrial product. Stainless steel composite plates have been widely used in urban pipe networks, petroleum, marine, coal chemical, salt industry, water conservancy and hydropower, hydrogen energy, and other industries. As a resource-saving product, stainless steel composite plates reduce the consumption of precious metals, significantly lower project costs, and achieve a perfect combination of low cost and high performance, resulting in significant social benefits.

[0004] The existing methods for preparing bimetallic sprayed composite plates and rolls mainly include vacuum welding and rolling. This method involves surface-treating a carbon steel substrate and a stainless steel cladding plate, then performing assembly welding in a vacuum environment of 10⁻²Pa, followed by hot rolling to form a metallurgical bonding interface between the substrate and the cladding.

[0005] When using vacuum welding to prepare composite plates and rolls, this method requires high surface flatness of the substrate and cladding material, necessitating milling and surface treatment of both materials. This increases the pretreatment time for the substrate and cladding material, thereby reducing the preparation efficiency of composite plates and rolls.

[0006] Therefore, this invention proposes a method for preparing composite plates and coils of bimetallic material spray-rolled billets to solve the above problems. Summary of the Invention

[0007] To address the aforementioned issues, this invention provides a method for preparing composite plates and coils of bimetallic material spray-blown composite plates and coils. The molten metal coating is directly atomized and sprayed onto the surface of the substrate to form a composite billet, requiring only sandblasting, thus eliminating the need for precision milling and shortening the preparation cycle.

[0008] To achieve the above objectives, the technical solution of the present invention is as follows: A method for preparing a bimetallic material spray-rolled composite plate or coil, comprising the following steps:

[0009] Step 1, Substrate Selection: Select a steel plate of appropriate size as the substrate based on the product performance and thickness requirements;

[0010] Step 2, Substrate pretreatment: The substrate is fed into a sandblasting device via a conveyor roller to perform sandblasting treatment on the substrate surface;

[0011] Step 3, Coating Material Smelting: The coating material is placed in a ladle and smelted to obtain molten coating metal, which is then transferred to an intermediate ladle.

[0012] Step 4, Spraying the blank: The substrate after substrate pretreatment is transported to the spraying chamber protected by inert gas. The substrate is preheated in the spraying chamber. The substrate enters the spraying area at a constant speed of 1~1.2m / min. At the same time, spraying preparation is carried out in the spraying area. Then, the molten metal coating is sprayed onto the surface of the substrate to obtain a single-sided composite blank. The sprayed single-sided composite blank is sent out through the conveyor roller.

[0013] Step 5, Cooling: Cool the single-sided composite blank to room temperature;

[0014] Step 6, Double-sided composite billet production: When producing the double-sided composite billet, flip the single-sided composite billet over and repeat steps 2 to 5 to obtain the double-sided composite billet.

[0015] Step 7, Rolling: Roll the single-sided composite billet and the double-sided composite billet that have been cooled to room temperature. After rolling, cool the single-sided composite billet and the double-sided composite billet to 800~820℃ to obtain the corresponding single-sided composite plate and double-sided composite plate.

[0016] Furthermore, the base material in step one is set as carbon structural steel, low alloy structural steel, shipbuilding steel, wind power steel, and pipeline steel.

[0017] Furthermore, in step three, the cladding material is smelted using an intermediate frequency furnace, an LF refining furnace, and a VOD furnace to obtain molten cladding metal, while maintaining the temperature of the molten cladding metal 60-80°C above its liquidus line. After smelting the cladding material, the ladle containing the molten cladding metal is hoisted onto the spraying area platform, the ladle outlet is opened, and the molten cladding metal is injected into the tundish through a long nozzle. The long nozzle contains inert gas, which is used to cover and protect the tundish, while maintaining the temperature of the molten cladding metal in the tundish 20-30°C above its liquidus line.

[0018] Furthermore, in step four, before the substrate enters the spray chamber, inert gas is introduced into the spray chamber to maintain a positive pressure inside the spray chamber.

[0019] Furthermore, in step four, after the substrate enters the spray chamber, the surface of the substrate is preheated by medium-frequency induction until the surface of the substrate is heated to 200~300℃.

[0020] Furthermore, in step four, the injection preparation includes opening the inert gas pipeline connected to the injection chamber, making the gas pressure in the pipeline 0.6~0.8MPa, and the inert gas enters the injection chamber and is ejected through the nozzle.

[0021] Further, in step four, the spraying assembly is carried out. First, the tundish nozzle is opened, and the molten metal coating enters the spraying chamber through the short nozzle. The molten metal coating is atomized by high-pressure gas and then sprayed out through the nozzle, so that the molten metal coating covers the surface of the substrate moving at a uniform speed. After the spraying is completed, the tundish nozzle and the inert gas pipeline are closed.

[0022] Furthermore, in step four, the intermediate tundish is equipped with four outlets whose flow rate is controlled by plunger rods. Each outlet is connected to a spray chamber via a short outlet. The short outlet is protected by inert gas. The nozzle diameter of the spray chamber is set to 20mm, and the spray speed of each nozzle is set to 200Kg / min. The spray thickness of the molten metal coating is controlled according to the running speed of the substrate, and the spray thickness of the molten metal coating is controlled between 5 and 30mm.

[0023] Furthermore, in step seven, the rolling heating temperature is set to 1250~1280℃, and the rolling heating time is set according to the thickness of the composite billet. The corresponding rolling heating time is set at 0.8 minutes / mm according to the thickness of the composite billet, and the initial rolling temperature is controlled at 1000~1150℃ by controlling the rolling temperature.

[0024] Furthermore, in step seven, different heat treatments are applied to the rolled composite plates and coils according to the product's application field and performance requirements.

[0025] The above approach has the following beneficial effects:

[0026] 1. This solution produces composite plates using the spray rolling method, achieving a metallurgical bond at the composite interface with a shear strength greater than 300 MPa. This improves the product quality of composite materials and expands their application range.

[0027] 2. This solution adopts spraying and hot rolling processes, which have low requirements for the flatness of the substrate surface and short surface treatment time. It can form a semi-continuous mechanized production process, improve product production capacity, and meet the needs of large-scale engineering construction materials such as oil and gas pipelines, urban pipe networks, shipbuilding, offshore platforms and hydrogen energy transportation.

[0028] 3. This solution adopts a spray composite process, which is applicable to various steel grades of composite materials and can adapt to the requirements of various composite layer thicknesses.

[0029] 4. Compared with the vacuum welding and rolling method, this solution uses a spraying composite method to produce composite billets, which eliminates the need for secondary billet assembly and rolling, thereby reducing production and manufacturing costs and simplifying the composite process. Attached Figure Description

[0030] Figure 1 This is a schematic diagram illustrating the steps of an embodiment of the method for preparing bimetallic material spray-rolled composite plates and coils according to the present invention. Detailed Implementation

[0031] The technical solution of the present invention will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0032] In the description of this invention, it should be noted that the terms "center," "upper," "lower," "left," "right," "vertical," "horizontal," "inner," and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing the invention and for simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the invention. Furthermore, the terms "first," "second," and "third" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.

[0033] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection of two components. Those skilled in the art can understand the specific meaning of the above terms in this invention based on the specific circumstances.

[0034] The following detailed description illustrates the specific implementation method:

[0035] Example 1:

[0036] As attached Figure 1 The following is a method for preparing a bimetallic material spray-rolled composite plate or coil, comprising the following steps:

[0037] Step 1, Base Material Selection: Based on product performance and thickness requirements, select steel plates of appropriate size as the base material; the base material is set as carbon structural steel, low alloy structural steel, shipbuilding steel, wind power steel, and pipeline steel, and the preferred base material dimensions are thickness of 150~350mm, width of 1500~2000mm, and length of 2000~4000mm;

[0038] Step 2, Substrate pretreatment: After preheating the substrate to 600°C, the substrate is fed into a sandblasting device through a conveyor roller to sandblast the surface of the substrate until the substrate body is exposed, thus obtaining the pretreated substrate.

[0039] Step 3, Coating Material Smelting: The preferred coating materials are stainless steel, titanium, copper, and aluminum. The coating material is placed in a ladle and smelted using a medium-frequency furnace, an LF refining furnace, and a VOD furnace to obtain molten coating metal. At the same time, the temperature of the molten coating metal is kept 60-80°C above its liquidus line. After smelting, the ladle of molten coating metal is hoisted onto the spraying area platform, the ladle outlet is opened, and the molten coating metal is injected into the tundish through a long nozzle. The long nozzle is filled with inert gas and the tundish is covered for protection. At the same time, the temperature of the molten coating metal in the tundish is kept 20-30°C above its liquidus line.

[0040] Step 4, Spraying and Assembly: Before the substrate enters the spraying chamber, inert gas is introduced into the spraying chamber to maintain positive pressure. The substrate, after pretreatment, is transported to the inert gas-protected spraying chamber. In the spraying chamber, the substrate is preheated by medium-frequency induction until the surface of the substrate is heated to 200~300℃. After heating, the substrate is uniformly introduced into the spraying zone at a speed of 1~1.2m / min. At the same time, spraying preparation is carried out in the spraying zone. Spraying preparation includes opening the inert gas pipeline connected to the spraying chamber, making the gas pressure in the pipeline 0.6~0.8MPa, and the inert gas enters the spraying chamber and is sprayed out through the nozzle. Then, the tundish nozzle is opened, and the molten metal coating enters the spraying chamber through the short nozzle. The molten metal coating is atomized by the high-pressure gas in the spraying chamber and sprayed out through the nozzle. The molten metal coating is then sprayed onto the surface of the substrate to obtain a single-sided composite billet. The sprayed single-sided composite billet is then sent out through the conveyor roller conveyor. After spraying is completed, the tundish nozzle and the inert gas pipeline are closed.

[0041] The intermediate tundish is equipped with four outlets whose flow rate is controlled by plunger rods. Each outlet is connected to a spray chamber via a short outlet. The short outlet is protected by inert gas. The nozzle diameter of the spray chamber is set to 20 mm, and the spray speed of each nozzle is set to 200 kg / min. The spray thickness of the molten metal coating is controlled according to the running speed of the substrate, and the spray thickness of the molten metal coating is controlled between 5 and 30 mm.

[0042] Step 5, Cooling: Cool the single-sided composite blank to room temperature;

[0043] Step 6, Double-sided composite billet production: When producing the double-sided composite billet, flip the single-sided composite billet over and repeat steps 2 to 5 to obtain the double-sided composite billet.

[0044] Step 7, Rolling: Roll the single-sided composite billet and the double-sided composite billet cooled to room temperature. After rolling, cool the single-sided composite billet and the double-sided composite billet to 800~820℃ to obtain the corresponding single-sided composite plate and double-sided composite plate.

[0045] The rolling heating temperature is set to 1250~1280℃, and the rolling heating time is set according to the thickness of the composite billet. The corresponding rolling heating time is set at 0.8 minutes / mm according to the thickness of the composite billet. The initial rolling temperature is controlled at 1000~1150℃ by controlling the rolling temperature.

[0046] After rolling, the rolled composite plates and coils undergo different heat treatments depending on the product's application and performance requirements.

[0047] The specific implementation process is as follows:

[0048] For composite board manufacturing:

[0049] Prepare a 25mm double-sided stainless steel composite plate for offshore wind turbine towers according to steps one to seven. The composite plate has a structure of 304L stainless steel + Q355E + 304L stainless steel, with each layer having a thickness of 1.5mm + 22mm + 1.5mm.

[0050] Substrate selection: Based on product performance and thickness requirements, continuously cast slabs made of Q355E material with dimensions of 250mm*1800mm*3500mm are selected as the substrate.

[0051] Substrate pretreatment: The Q355E slab is hoisted to the conveyor roller conveyor and preheated to 600°C in a continuous heating furnace. After preheating, the Q355E slab is conveyed to the sandblasting device via the conveyor roller conveyor to sandblast the surface of the Q355E slab to remove iron oxide scale and oil stains, thus exposing the Q355E slab body.

[0052] Coating smelting: 304L stainless steel is placed in a ladle and smelted in a medium frequency furnace until the temperature of the molten 304L stainless steel reaches 1650℃. The ladle is then hoisted onto the platform in the spraying area. The ladle outlet is connected to the tundish through a long nozzle. Molten 304L stainless steel is injected into the tundish through the ladle outlet and the long nozzle. Inert gas is provided in the long nozzle.

[0053] Spraying billet assembly: Inert gas is introduced into the spraying chamber, and the gas pressure in the spraying chamber is controlled at 0.8MPa. Then, the tundish nozzle is opened, allowing molten 304L stainless steel to enter the spraying chamber for atomization. The spraying speed of the molten 304L stainless steel is set to 200Kg / min. At the same time as spraying, the Q355E slab is conveyed to the spraying chamber and enters the spraying zone at a uniform speed of 1.1m / min to complete the spraying and compositing of the Q355E slab surface, resulting in a 304L stainless steel composite billet. The composite billet is then conveyed out via a conveyor roller conveyor, while the molten 304L stainless steel is continuously sprayed and the preheated Q355E slab is continuously fed in, forming a continuous compositing mode.

[0054] Cooling: The composite billet is hoisted onto a cooling platform and air-cooled to room temperature;

[0055] Double-sided composite billet preparation: After flipping the composite billet, repeat the operations of substrate pretreatment, cladding smelting, spraying billet assembly and cooling to obtain a double-sided composite billet; then the double-sided composite billet is sent into a heating furnace and heated to 1250℃-1280℃, with a soaking temperature of 1200~1230℃; the heating time is ≥1 minute / mm to ensure that the double-sided composite billet is thoroughly fired;

[0056] Rolling: The initial rolling temperature is controlled at 1100~1150℃. After rolling, the steel is cooled to 800℃-820℃ according to the product performance requirements. It is then rapidly cooled to 550℃ in ACC, leveled, and air-cooled. The edges are then trimmed to obtain a composite plate.

[0057] Finally, the prepared composite plate was sampled and tested, and its various properties were evaluated. The test results are as follows:

[0058] Mechanical properties of composite board I:

[0059]

[0060] Samples were taken 2 mm subcutaneously from the coated skin. Charpy V-shaped sample, 10 mm × 100 × 55 mm:

[0061]

[0062] Composite interface shear strength:

[0063]

[0064] Flaw detection: Meets the Class I standard of GB / T2970-2004 "Ultrasonic Testing Method for Thick Steel Plates";

[0065] Conclusion: The product meets the requirements of product symbol T / SSEA 0042-2019 "Hot-rolled Stainless Steel Composite Plate";

[0066] Finally, the surface of the composite flat plate is inspected and cleaned, cut according to size requirements, and labeled as qualified before being put into storage.

[0067] For the fabrication of composite rolls:

[0068] Prepare 3mm double-sided composite stainless steel hot-rolled coils according to steps one to seven, and make a composite coil with a structure of 304L stainless steel + Q235B + 304L stainless steel, and each layer thickness of 0.25mm + 2.5mm + 0.25mm.

[0069] Substrate selection: Based on product performance and thickness requirements, continuously cast slabs made of Q235B with dimensions of 150mm*1800mm*3500mm are selected as the substrate.

[0070] Substrate pretreatment: The Q235B slab is hoisted to the conveyor roller conveyor and preheated to 600°C in a continuous heating furnace. After preheating, the Q235B slab is conveyed to the sandblasting device via the conveyor roller conveyor to sandblast the surface of the Q235B slab to remove iron oxide scale and oil stains, thus exposing the Q235B slab body.

[0071] Coating smelting: 304L stainless steel is placed in a ladle and smelted in a medium frequency furnace until the temperature of the molten 304L stainless steel reaches 1650℃. The ladle is then hoisted onto the platform in the spraying area. The ladle outlet is connected to the tundish through a long nozzle. Molten 304L stainless steel is injected into the tundish through the ladle outlet and the long nozzle. Inert gas is provided in the long nozzle.

[0072] Spraying billet assembly: Inert gas is introduced into the spraying chamber, and the gas pressure in the spraying chamber is controlled at 0.8MPa. Then, the tundish nozzle is opened, allowing molten 304L stainless steel to enter the spraying chamber for atomization. The spraying speed of the molten 304L stainless steel is set to 200Kg / min. At the same time as spraying, Q235B slabs are conveyed to the spraying chamber and enter the spraying zone at a uniform speed of 1.1m / min to complete the spraying and compositing of the Q235B slab surface, resulting in 304L stainless steel composite billets. The composite billets are then conveyed out via a conveyor roller conveyor, while molten 304L stainless steel is continuously sprayed and preheated Q235B slabs are continuously fed in, forming a continuous compositing mode.

[0073] Cooling: The composite billet is hoisted onto a cooling platform and air-cooled to room temperature;

[0074] Double-sided composite billet preparation: After flipping the composite billet, repeat the operations of substrate pretreatment, cladding smelting, spraying billet assembly and cooling to obtain a double-sided composite billet; then the double-sided composite billet is sent into a heating furnace and heated to 1250℃-1280℃, with a soaking temperature of 1200~1230℃; the heating time is ≥1 minute / mm to ensure that the double-sided composite billet is thoroughly fired;

[0075] Rolling: The initial rolling temperature is controlled at 1100~1150℃. After rolling, the steel is cooled to 800℃-820℃ according to the product performance requirements. It is then subjected to ACC rapid cooling to 550℃ and coiled to obtain composite coil.

[0076] Finally, the prepared composite steel coil was sampled and inspected, and its various properties were tested. The test results are as follows:

[0077]

[0078] Flaw detection: Meets the Class I standard of GB / T2970-2004 "Ultrasonic Testing Method for Thick Steel Plates";

[0079] Conclusion: The product meets the requirements of product symbol T / SSEA 0042-2019 "Hot-rolled Stainless Steel Composite Plate";

[0080] Finally, the surface of the composite sheet is inspected and cleaned, cut according to size requirements, and labeled as qualified before being put into storage.

[0081] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.

Claims

1. A method for preparing a composite plate or coil of bimetallic material by spray-rolling, characterized in that, Includes the following steps: Step 1, Substrate Selection: Select a steel plate of appropriate size as the substrate based on the product performance and thickness requirements; Step 2, Substrate pretreatment: The substrate is fed into a sandblasting device via a conveyor roller to perform sandblasting treatment on the substrate surface; Step 3, Coating Material Smelting: The coating material is placed in a ladle and smelted to obtain molten coating metal, which is then transferred to an intermediate ladle. Step 4, Spraying the blank: The substrate after substrate pretreatment is transported to the spraying chamber protected by inert gas. The substrate is preheated in the spraying chamber. The substrate enters the spraying area at a constant speed of 1~1.2m / min. At the same time, spraying preparation is carried out in the spraying area. Then, the molten metal coating is sprayed onto the surface of the substrate to obtain a single-sided composite blank. The sprayed single-sided composite blank is sent out through the conveyor roller. Step 5, Cooling: Cool the single-sided composite blank to room temperature; Step 6, Double-sided composite billet production: When producing the double-sided composite billet, flip the single-sided composite billet over and repeat steps 2 to 5 to obtain the double-sided composite billet. Step 7, Rolling: Roll the single-sided composite billet and the double-sided composite billet that have been cooled to room temperature. After rolling, cool the single-sided composite billet and the double-sided composite billet to 800~820℃ to obtain the corresponding single-sided composite plate and double-sided composite plate.

2. The method for preparing bimetallic material spray-rolled composite plates and coils according to claim 1, characterized in that: The base material in step one is set as carbon structural steel, low alloy structural steel, shipbuilding steel, wind power steel, and pipeline steel.

3. The method for preparing bimetallic material spray-rolled composite plates and coils according to claim 2, characterized in that: In step three, the cladding material is smelted using an intermediate frequency furnace, an LF refining furnace, and a VOD furnace to obtain molten cladding metal. At the same time, the temperature of the molten cladding metal is kept 60-80°C above its liquidus line. After smelting the cladding material, the ladle containing the molten cladding metal is hoisted onto the spraying area platform. The ladle outlet is opened, and the molten cladding metal is injected into the tundish through a long nozzle. The long nozzle contains inert gas, and the tundish is covered for protection. At the same time, the temperature of the molten cladding metal in the tundish is kept 20-30°C above its liquidus line.

4. The method for preparing bimetallic material spray-rolled composite plates and coils according to claim 3, characterized in that: In step four, before the substrate enters the spray chamber, inert gas is introduced into the spray chamber to maintain a positive pressure inside the spray chamber.

5. The method for preparing bimetallic material spray-rolled composite plates and coils according to claim 4, characterized in that: In step four, after the substrate enters the spray chamber, the surface of the substrate is preheated by medium-frequency induction until the surface of the substrate is heated to 200~300℃.

6. The method for preparing bimetallic material spray-rolled composite plates and coils according to claim 5, characterized in that: In step four, the injection preparation includes opening the inert gas pipeline connected to the injection chamber, making the gas pressure in the pipeline 0.6~0.8MPa, and the inert gas enters the injection chamber and is ejected through the nozzle.

7. The method for preparing bimetallic material spray-rolled composite plates and coils according to claim 6, characterized in that: In step four, the spraying assembly is carried out. First, the tundish nozzle is opened, and the molten metal coating enters the spraying chamber through the short nozzle. The molten metal coating is atomized by high-pressure gas and then sprayed out through the nozzle, so that the molten metal coating covers the surface of the substrate moving at a uniform speed. After the spraying is completed, the tundish nozzle and the inert gas pipeline are closed.

8. The method for preparing bimetallic material spray-rolled composite plates and coils according to claim 7, characterized in that: In step four, the intermediate tundish is equipped with four water outlets whose flow rate is controlled by plunger rods. Each water outlet is connected to a spray chamber via a short water outlet. The short water outlet is protected by inert gas. The nozzle diameter of the spray chamber is set to 20mm, and the spray speed of each nozzle is set to 200Kg / min. The spraying thickness of the molten metal coating is controlled according to the running speed of the substrate, and the spraying thickness of the molten metal coating is controlled between 5 and 30 mm.

9. The method for preparing bimetallic material spray-rolled composite plates and coils according to claim 8, characterized in that: In step seven, the rolling heating temperature is set to 1250~1280℃, and the rolling heating time is set according to the thickness of the composite billet. The corresponding rolling heating time is set at 0.8 minutes / mm according to the thickness of the composite billet. The initial rolling temperature is controlled at 1000~1150℃ by controlling the rolling temperature.

10. The method for preparing bimetallic material spray-rolled composite plates and coils according to claim 9, characterized in that: In step seven, different heat treatments are applied to the rolled composite plates and coils according to the product's application field and performance requirements.