A method for the industrialized, continuous, and stable production of atomized nickel powder

By combining standardized furnace construction and gradient furnace drying processes with closed-loop medium-frequency melting, staged deoxidation and slag removal, continuous and stable production of atomized nickel powder has been achieved. This has solved problems such as short furnace lining life, incomplete deoxidation, and large fluctuations in atomized particle size in existing technologies, thereby improving product quality and safety.

CN123103003APending Publication Date: 2026-11-17JINCHUAN GROUP NICKEL COBALT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611277282.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing atomized nickel powder production suffers from problems such as short furnace lining life, incomplete deoxidation, large fluctuations in atomized particle size, discontinuous drying and reduction, poor batch consistency, and high safety risks, resulting in unstable product quality.

Method used

By adopting standardized furnace construction and gradient furnace drying processes, combined with closed-loop medium-frequency melting, staged deoxidation and slag removal, precise high-pressure water-gas atomization, constant temperature drying, continuous atmosphere reduction and multi-stage screening, the entire process system is integrated and parameters are precisely controlled, forming continuous and stable production.

Benefits of technology

It significantly extends the service life of the furnace body, reduces production risks, ensures low oxygen content, concentrated particle size distribution, and excellent batch stability of products, thereby improving production efficiency and economic benefits and meeting the requirements of high-end applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123103003A_ABST
    Figure CN123103003A_ABST
Patent Text Reader

Abstract

This invention discloses a method for the industrialized, continuous, and stable production of atomized nickel powder, belonging to the field of metal powder preparation technology. The method uses nickel as raw material and sequentially involves furnace construction and drying, medium-frequency melting, deoxidation and slag removal, water-air combined atomization, drying and dehydration, reduction protection, sieving and batching, and vacuum packaging, achieving continuous production throughout the entire process. Standardized furnace construction and gradient furnace drying extend furnace life; graded deoxidation and slag removal reduce impurities; precise control of atomization water pressure and reducing atmosphere; and multi-stage sieving and batching ensure batch consistency. The resulting product has low oxygen content, hydrogen loss ≤0.10%, concentrated particle size distribution, good flowability, and a bulk density of 2.4–3.2 g / cm³ for ordinary nickel powder. 3 The loose packing density of the fine nickel powder is 2.1–2.7 g / cm³. 3 It can meet the requirements of high-end fields such as powder metallurgy, battery materials, and cemented carbide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of industrial preparation technology of non-ferrous metal powder, specifically to a method for large-scale production of atomized nickel powder using water-air combined atomization and continuous reduction, which is suitable for the industrial continuous manufacturing of high-purity, low-oxygen, and uniformly sized atomized nickel powder. Background Technology

[0002] Atomized nickel powder, due to its high purity, good flowability, stable bulk density, and excellent electrical and thermal conductivity, is widely used in powder metallurgy, diamond tools, battery anode materials, cemented carbide, electronic pastes, and other fields. With the increasing demands for nickel powder quality in high-end manufacturing, the industry urgently needs continuous, safe, and stable industrial production technologies.

[0003] The existing atomized nickel powder production has the following problems: (1) There is no standardized gradient process for furnace lining and furnace drying, resulting in short furnace life and easy furnace leakage; (2) The deoxidation and slag removal operation is rough, and there are many impurities in the nickel liquid, resulting in high hydrogen loss and high oxygen content in the product; (3) The atomized water pressure and flow control are unstable, resulting in wide particle size distribution and low fine powder yield; (4) Drying, reduction and screening are independent, the process is not continuous, and the batch consistency is poor; (5) The safety management and emergency mechanism is not perfect, and there are safety risks in the high temperature, high pressure and ammonia links.

[0004] Therefore, developing a fully integrated, precisely controllable, safe, stable, and large-scale continuous production method for preparing atomized nickel powder has significant engineering value and market implications. Summary of the Invention

[0005] The purpose of this invention is to overcome the shortcomings of existing technologies and provide an industrially sustainable and stable method for producing atomized nickel powder. This invention addresses the problems in existing atomized nickel powder production, such as short furnace lining life, incomplete deoxidation, large fluctuations in atomized particle size, discontinuous drying and reduction, poor batch consistency, and high safety risks. Through standardized furnace construction and baking, closed-loop medium-frequency melting, staged deoxidation and slag removal, precise high-pressure water-air atomization, constant-temperature drying, continuous atmosphere reduction, multi-stage sieving and batching, and vacuum sealing packaging, the entire process is integrated with precise parameter control, achieving large-scale, continuous, and stable production of both ordinary and micro-fine atomized nickel powder.

[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows: A method for the industrial-scale, continuous, and stable production of atomized nickel powder includes the following steps: (1) Furnace construction and drying: The furnace lining is prepared by mixing fused magnesia, boric acid and water glass. After the furnace is constructed by layering and compacting, it is dried according to the gradient power to complete the sintering of the furnace lining. (2) Medium frequency melting: Add dry nickel material to a medium frequency furnace, control the melting power to 90-150kW, and heat until completely melted to form nickel molten liquid; (3) Deoxidation and slag removal: Add silicon-calcium alloy deoxidizer and slag remover to the nickel melt, stir, let stand, and then remove the surface slag to obtain clear nickel melt; (4) Water-air combined atomization: the deoxidized nickel liquid is poured into the preheated intermediate tundish and atomized into powder by high pressure water; (5) Drying and dehydration: Dry the atomized wet nickel powder at 90-170℃ for 7-12 hours, cool it and then sieve it to remove large particles; (6) Reduction protection: After drying, the nickel powder is continuously reduced in a steel strip furnace under an ammonia decomposition atmosphere; (7) Screening and batching: The reduced nickel powder is screened in multiple stages and then mixed in batches. (8) Packaging and warehousing: qualified products are weighed and vacuum-sealed.

[0007] Further, the furnace charge in step (1) is a mixture of fused magnesia, water glass, boric acid and water. The fused magnesia contains three bags of each of four particle sizes: 0-1mm, 1-3mm, 3-5mm and 250 mesh. The water glass is 25kg and the boric acid content is 0.5-1%. 3-6kg of water is added and mixed until it can be formed into a ball by hand and can be easily dispersed by light pressure. The furnace bottom is compacted to a thickness of 15-21cm, the furnace collar is 10-15cm wide and 10-20cm high, and a V-shaped guide groove is reserved.

[0008] Further, the gradient power oven described in step (1) is as follows: starting from 5kW, increasing by 5kW every 5h, and baking for 20h to 25kW; then increasing by 5kW every 3h, and baking for 15h to 45kW, with a total oven baking time of 35h.

[0009] Furthermore, in step (2), the nickel material must be dry and free of moisture. When feeding, first add lumpy nickel, and after the molten pool is formed, add nickel slag and sieve powder to prevent the material from being suspended or splashed. Stop feeding when the molten pool reaches the lower edge of the furnace.

[0010] Further, in step (3), when the nickel material is melted to half the furnace, add 2 to 4 pieces of silicon-calcium alloy deoxidizer, each piece weighing about 50g; after the material is completely melted, reduce the power to 25kW, add 2 to 4 pieces of deoxidizer, stir for 1 minute, let stand for 5 minutes, then add 2 to 4 spoons of slag remover, each spoon weighing about 100g, and remove the slag until the nickel liquid is clear.

[0011] Further, in step (4), the preheating temperature of the tundish is: 350±70℃ for furnace #1 and 890±50℃ for furnace #2; the atomizing water pressure is controlled at 5~15MPa for the production of ordinary nickel powder, or 80~120kg for the production of fine nickel powder; the atomization system is started in the following order: first start the high-pressure blower, then start the high-pressure pump. When producing fine nickel powder, the pre-pump must be started first and then the load added; the casting is slow and stable, and the molten liquid at the bottom of the furnace is not drained to protect the furnace lining.

[0012] Further, in step (5), after drying, the product is cooled to room temperature and then passed through a 3-mesh sieve to remove large particles and clumps.

[0013] Further, in step (6), the reduction temperature is: 480±50℃ for ordinary atomized nickel powder and 360±50℃ for micro-atomized nickel powder; the temperature of the ammonia decomposition furnace is 950±50℃, the flow rate of ammonia decomposition gas is 20±5m³ / h, the frequency of the steel strip furnace is 8±2Hz, and the feed thickness is 30~50mm and the width is 300~500mm.

[0014] Furthermore, in step (7), the powder on the sieve is returned to the medium-frequency melting process for recycling, and the qualified powder under the sieve is fed into the batching machine for thorough mixing to control the loose packing density.

[0015] Furthermore, in step (8), the products are weighed at 25±0.04kg, vacuum-sealed, capped, and labeled before being stored in batches.

[0016] Compared with the prior art, the present invention has the following beneficial effects: (1) The present invention adopts standardized furnace construction and gradient furnace drying process, which makes the furnace lining structure dense and uniform, without cracks and voids, significantly improving the service life of the furnace body, reducing the production risks such as furnace leakage and furnace penetration from the source, and with the perfect emergency response mechanism for water outage, power outage and ammonia leakage, the production safety is greatly improved.

[0017] (2) The present invention can fully remove oxides and impurities in nickel liquid through graded deoxidation and deep slag removal process. Combined with precise and controllable water vapor atomization parameters and ammonia decomposition reduction atmosphere, the final product has low oxygen content, qualified hydrogen loss, concentrated particle size distribution, and excellent batch-to-batch stability, which fully meets the requirements of high-end applications.

[0018] (3) This invention integrates multiple processes such as furnace construction, smelting, deoxidation and slag removal, atomization, drying, reduction, screening and packaging, realizing the continuous, automated and stable production process, resulting in high production efficiency and consistent product quality.

[0019] (4) This invention realizes the closed-loop return of powder on the sieve to smelting and the optimized utilization of reducing atmosphere. The comprehensive utilization rate of materials is high, and the energy consumption and auxiliary material consumption are significantly reduced. While ensuring product quality, it effectively improves production economic benefits and has stronger industrial competitiveness. Attached Figure Description

[0020] Figure 1 This is a process flow diagram for the industrial-scale continuous and stable production of atomized nickel powder according to the present invention. Detailed Implementation

[0021] The present invention will be further described in detail below with reference to embodiments, but the implementation of the present invention is not limited thereto.

[0022] Example 1 Three bags each of fused magnesia (0-1mm, 1-3mm, 3-5mm, and 250 mesh), 25kg of water glass, 0.8% boric acid, and 4.5kg of water were mixed until the mixture could be formed into a ball by hand and crumbled easily under light pressure. The furnace lining was prepared by compacting the bottom to a thickness of 18cm, and the furnace collar was 12cm wide and 15cm high, with a V-shaped guide groove reserved. The furnace was dried using a gradient heating process, starting from 5kW, increasing by 5kW every 5 hours to 25kW and holding for 20 hours, then increasing by 5kW every 3 hours to 45kW and holding for 15 hours, for a total of 35 hours to complete the sintering of the furnace lining. Use dry, moisture-free nickel material; do not add water. Start feeding when the induction furnace power reaches 80kW or higher. First, add lumps of nickel to form a molten pool, then add returned material and sieved powder. Observe the molten state in real time to prevent bridging. Stop feeding when the molten pool reaches the lower edge of the furnace leader. Control the smelting power at 120kW and heat until completely melted to form molten nickel. When the nickel material is half-melted, add 3 pieces of silicon-calcium alloy deoxidizer (approximately 50g each). After the material is completely melted, reduce the power to 25kW, add 3 more pieces of deoxidizer, stir for 1 minute, let stand for 5 minutes, then add 3 spoonfuls of slag remover (approximately 100g each) to form flakes of slag. Remove surface slag until the nickel liquid is clear and free of impurities. Preheat the tundish in advance, controlling the temperature of furnace #1 at 350℃ and furnace #2 at 900℃. After checking that the nozzles, water tank, and high-pressure pump are all normal, start the atomization system in sequence, slowly tilt the furnace and pour the deoxidized nickel liquid into the preheated tundish. Atomize the nickel into powder using high-pressure water, controlling the atomization water pressure at 10MPa (ordinary nickel powder) or 100kg (fine nickel powder). When tapping out of the furnace, leave a portion of the molten liquid at the bottom of the furnace to protect the furnace lining. Evenly pack the collected atomized wet nickel powder into a material box, place it in an oven and dry it at 120℃ for 10 hours. After cooling to room temperature, pass it through a 3-mesh sieve to remove large particles and agglomerates, obtaining dry and loose atomized nickel powder. The dried nickel powder is evenly fed into a steel strip furnace for continuous reduction under an ammonia decomposition atmosphere. The reduction temperature for ordinary atomized nickel powder is controlled at 480℃, and for micro-atomized nickel powder at 370℃. The ammonia decomposition furnace temperature is 950℃, the ammonia decomposition gas flow rate is 20 m³ / h, the steel strip frequency is 8 Hz, and the feed thickness is 40 mm and the width is 400 mm for even distribution. The reduced nickel powder is then graded according to specifications by multi-stage vibration and ultrasonic sieving. The powder that passes through the sieve is returned to the medium-frequency smelting process for recycling, while the qualified powder that passes through the sieve is sent to a batching machine for thorough mixing to stabilize the loose packing density and particle size. The finished product is then precisely weighed at 25 ± 0.04 kg, vacuum-sealed, capped, and labeled with batch markings, and stored according to batch specifications. Testing showed that the particle size of the product obtained in this embodiment was qualified. For ordinary nickel powder, the hydrogen loss was ≤0.10% and the loose packing density was 2.6~3.2g / cm³. For fine nickel powder, the hydrogen loss was ≤0.09% and the loose packing density was 2.3~2.7g / cm³. The product had excellent flowability and batch stability met the requirements of high-end applications.

[0023] Example 2 Three bags each of fused magnesia (0-1mm, 1-3mm, 3-5mm, and 250 mesh), 25kg of water glass, 0.9% boric acid, and 4kg of water were mixed until the mixture could be formed into a ball by hand and crumbled easily under light pressure. The furnace lining was prepared by compacting the bottom to a thickness of 18cm, and the furnace collar was 12cm wide and 15cm high, with a V-shaped guide groove reserved. The furnace was dried using a gradient heating process, starting from 5kW, increasing by 5kW every 5 hours to 25kW and holding for 20 hours, then increasing by 5kW every 3 hours to 45kW and holding for 15 hours, for a total of 35 hours to complete the sintering of the furnace lining. Use dry, moisture-free nickel material; do not add water. Start feeding when the induction furnace power reaches 80kW or higher. First, add lumps of nickel to form a molten pool, then add returned material and sieved powder. Observe the molten state in real time to prevent bridging. Stop feeding when the molten pool reaches the lower edge of the furnace collar. Control the smelting power to 90-150kW and heat until completely melted to form molten nickel. When the nickel material is half-melted, add 3 pieces of silicon-calcium alloy deoxidizer (approximately 50g each). After the material is completely melted, reduce the power to 25kW, add 3 more pieces of deoxidizer, stir for 1 minute, let stand for 5 minutes, then add 2 spoonfuls of slag remover (approximately 100g each) to form flakes of slag. Remove surface slag until the nickel liquid is clear and free of impurities. Preheat the tundish in advance, controlling the temperature of furnace #1 at 380℃ and furnace #2 at 920℃. After checking that the nozzles, water tank, and high-pressure pump are all normal, start the atomization system in sequence, slowly tilt the furnace and pour the deoxidized nickel liquid into the preheated tundish. Atomize the nickel powder using high-pressure water, controlling the atomization water pressure at 12MPa (ordinary nickel powder) or 120kg (fine nickel powder). When tapping out of the furnace, leave a portion of the molten liquid at the bottom of the furnace to protect the furnace lining. Evenly pack the collected atomized wet nickel powder into a material box, place it in an oven and dry it at 140℃ for 11 hours. After cooling to room temperature, pass it through a 3-mesh sieve to remove large particles and agglomerates, obtaining dry and loose atomized nickel powder. The dried nickel powder is evenly fed into a steel strip furnace for continuous reduction under an ammonia decomposition atmosphere. The reduction temperature for ordinary atomized nickel powder is controlled at 480℃, and for micro-atomized nickel powder at 370℃. The ammonia decomposition furnace temperature is 970℃, the ammonia decomposition gas flow rate is 24 m³ / h, the steel strip frequency is 8 Hz, and the feed thickness is 35 mm and the width is 350 mm for even distribution. The reduced nickel powder is then graded according to specifications by multi-stage vibration and ultrasonic sieving. The powder that passes through the sieve is returned to the medium-frequency smelting process for recycling, while the qualified powder that passes through the sieve is sent to a batching machine for thorough mixing to stabilize the loose packing density and particle size. The finished product is then precisely weighed at 25 ± 0.04 kg, vacuum-sealed, capped, and labeled with batch markings, and stored according to batch specifications. Testing showed that the particle size of the product obtained in this embodiment was qualified. For ordinary nickel powder, the hydrogen loss was ≤0.095% and the loose packing density was 2.5~3.2g / cm³. For fine nickel powder, the hydrogen loss was ≤0.08% and the loose packing density was 2.2~2.5g / cm³. The product had excellent flowability and batch stability met the requirements of high-end applications.

[0024] Example 3 Three bags each of fused magnesia (0-1mm, 1-3mm, 3-5mm, and 250 mesh), 25kg of water glass, 0.9% boric acid, and 4.5kg of water were mixed until the mixture could be formed into a ball by hand and crumbled easily under light pressure. The furnace lining was prepared by compacting the bottom to a thickness of 18cm, and the furnace collar was 12cm wide and 15cm high, with a V-shaped guide groove reserved. The furnace was dried using a gradient heating process, starting from 5kW, increasing by 5kW every 5 hours to 25kW and holding for 20 hours, then increasing by 5kW every 3 hours to 45kW and holding for 15 hours, for a total of 35 hours to complete the sintering of the furnace lining. Use dry, moisture-free nickel material; do not add water. Start feeding when the induction furnace power reaches 80kW or higher. First, add lumps of nickel to form a molten pool, then add returned material and sieved powder. Observe the molten state in real time to prevent bridging. Stop feeding when the molten pool reaches the lower edge of the furnace collar. Control the smelting power at 150kW and heat until completely melted to form molten nickel. When the nickel material is half-melted, add 3 pieces of silicon-calcium alloy deoxidizer (approximately 50g each). After the material is completely melted, reduce the power to 25kW, add 3 more pieces of deoxidizer, stir for 1 minute, let stand for 5 minutes, then add 3 spoonfuls of slag remover (approximately 100g each) to form flakes of slag. Remove surface slag until the nickel liquid is clear and free of impurities. Preheat the tundish in advance, controlling the temperature of furnace #1 at 400℃ and furnace #2 at 950℃. After checking that the nozzles, water tank, and high-pressure pump are all normal, start the atomization system in sequence, slowly tilt the furnace and pour the deoxidized nickel liquid into the preheated tundish. Atomize the nickel into powder using high-pressure water, controlling the atomization water pressure at 15MPa (ordinary nickel powder) or 110kg (fine nickel powder). When tapping out of the furnace, leave a portion of the molten liquid at the bottom of the furnace to protect the furnace lining. Evenly pack the collected atomized wet nickel powder into a material box, place it in an oven and dry it at 150℃ for 10 hours. After cooling to room temperature, pass it through a 3-mesh sieve to remove large particles and agglomerates, obtaining dry and loose atomized nickel powder. The dried nickel powder is evenly fed into a steel strip furnace for continuous reduction under an ammonia decomposition atmosphere. The reduction temperature for ordinary atomized nickel powder is controlled at 480℃, and for micro-atomized nickel powder at 370℃. The ammonia decomposition furnace temperature is 970℃, the ammonia decomposition gas flow rate is 22 m³ / h, the steel strip frequency is 8 Hz, and the feed thickness is 35 mm and the width is 350 mm for even distribution. The reduced nickel powder is then graded according to specifications through multi-stage vibration and ultrasonic sieving. The powder that passes through the sieve is returned to the medium-frequency smelting process for recycling, while the qualified powder that passes through the sieve is sent to a batching machine for thorough mixing to stabilize the loose packing density and particle size. The mixed finished product is precisely weighed at 25 ± 0.04 kg, vacuum-sealed, capped, and labeled with batch markings, and then stored according to batch specifications. Testing showed that the particle size of the product obtained in this embodiment was qualified. For ordinary nickel powder, the hydrogen loss was ≤0.09% and the loose packing density was 2.4~3.1g / cm³. For fine nickel powder, the hydrogen loss was ≤0.08% and the loose packing density was 2.3~2.5g / cm³. The product had excellent flowability and batch stability met the requirements of high-end applications.

[0025] Example 4 Three bags each of fused magnesia (0-1mm, 1-3mm, 3-5mm, 250 mesh), 25kg of water glass, 0.9% boric acid, and 4kg of water were mixed until the mixture could be formed into a ball by hand and crumble easily under light pressure to prepare the furnace charge. The furnace bottom was compacted to a thickness of 18cm, and the furnace collar was 12cm wide and 15cm high, with a pre-reserved V-shaped guide groove. The furnace drying process adopted a gradient heating process, starting from 5kW, increasing by 5kW every 5 hours to 25kW and holding for 20 hours, then increasing by 5kW every 3 hours to 45kW and holding for 15 hours, for a total of 35 hours to complete the furnace lining sintering. Dry, moisture-free nickel material was selected, and feeding with water was prohibited. The charging began when the power of the medium-frequency furnace reached 80kW or above. First, lumpy nickel was added to form a molten pool, and then return material and sieved powder were added. The molten state was observed in real time to prevent bridging. The charging was stopped when the molten pool reached the lower edge of the furnace collar, and the smelting power was controlled at 120kW. The furnace was heated until it was completely melted to form a nickel molten liquid. When the nickel material is half-melted, add two pieces of silicon-calcium alloy deoxidizer (approximately 50g each). After the material is completely melted, reduce the power to 25kW, add two more pieces of deoxidizer, stir for 1 minute, let stand for 5 minutes, then add four spoonfuls of slag remover (approximately 100g each) to form slag flakes. Remove surface slag until the nickel liquid is clear and free of impurities. Preheat the tundish in advance, controlling the temperature of furnace #1 at 320℃ and furnace #2 at 860℃. After checking that the nozzles, water tank, and high-pressure pump are all normal, start the atomization system in sequence, slowly tilt the furnace and pour the deoxidized nickel liquid into the preheated tundish. Atomize it into powder using high-pressure water, controlling the atomization water pressure at 13MPa (ordinary nickel powder) or 100kg (fine nickel powder). When tapping out of the furnace, leave a portion of the molten liquid at the bottom of the furnace to protect the furnace lining. The collected atomized wet nickel powder was evenly packed into a material box and dried in an oven at 130℃ for 10 hours. After cooling to room temperature, it was passed through a 3-mesh sieve to remove large particles and agglomerates, resulting in dry and loose atomized nickel powder. The dried nickel powder was evenly fed into a steel strip furnace for continuous reduction treatment under an ammonia decomposition atmosphere. The reduction temperature for ordinary atomized nickel powder was controlled at 480℃, and for fine atomized nickel powder at 340℃. The ammonia decomposition furnace temperature was 880℃, the ammonia decomposition gas flow rate was 25 m³ / h, the steel strip frequency was 10 Hz, and the feed thickness was 30 mm and the width was 350 mm for even distribution. The reduced nickel powder was graded according to specifications by multi-stage vibration and ultrasonic sieving. The powder on the sieve was returned to the medium-frequency smelting process for recycling, while the qualified powder under the sieve was sent to a batching machine for thorough mixing to stabilize the loose packing density and particle size. The mixed finished product was accurately weighed at 25 ± 0.04 kg, vacuum-sealed, capped, and labeled with batch markings, and stored according to batch specifications. Testing showed that the particle size of the product obtained in this embodiment was qualified. For ordinary nickel powder, the hydrogen loss was ≤0.1% and the loose packing density was 2.6~3.2g / cm³. For fine nickel powder, the hydrogen loss was ≤0.09% and the loose packing density was 2.1~2.5g / cm³. The product had excellent flowability and batch stability met the requirements of high-end applications.

[0026] Example 5 Three bags each of fused magnesia (0-1mm, 1-3mm, 3-5mm, 250 mesh), 25kg of water glass, 0.9% boric acid, and 5kg of water were mixed until the mixture could be formed into a ball by hand and crumble easily under light pressure to prepare the furnace charge. The furnace bottom was compacted to a thickness of 18cm, and the furnace collar was 12cm wide and 15cm high, with a pre-reserved V-shaped guide groove. The furnace drying process adopted a gradient heating process, starting from 5kW, increasing by 5kW every 5 hours to 25kW and holding for 20 hours, then increasing by 5kW every 3 hours to 45kW and holding for 15 hours, for a total of 35 hours to complete the furnace lining sintering. Dry nickel material without moisture was selected, and feeding with water was prohibited. The charging began when the power of the medium-frequency furnace reached 80kW or more. First, lumpy nickel was added to form a molten pool, and then return material and sieved powder were added. The molten state was observed in real time to prevent bridging. The charging was stopped when the molten pool reached the lower edge of the furnace collar, and the smelting power was controlled at 130kW. The furnace was heated until it was completely melted to form a nickel molten liquid. When the nickel material is half-melted, add 3 pieces of silicon-calcium alloy deoxidizer (approximately 50g each). After the material is completely melted, reduce the power to 25kW, add 3 more pieces of deoxidizer, stir for 1 minute, let stand for 5 minutes, then add 2 spoonfuls of slag remover (approximately 100g each) to form slag flakes. Remove surface slag until the nickel liquid is clear and free of impurities. Preheat the tundish in advance, controlling the temperature of furnace #1 at 360℃ and furnace #2 at 920℃. After checking that the nozzles, water tank, and high-pressure pump are all normal, start the atomization system in sequence, slowly tilt the furnace and pour the deoxidized nickel liquid into the preheated tundish. Atomize it into powder using high-pressure water, controlling the atomization water pressure at 12MPa (ordinary nickel powder) or 120kg (fine nickel powder). When tapping out of the furnace, leave a portion of the molten liquid at the bottom of the furnace to protect the furnace lining. The collected atomized wet nickel powder was evenly packed into a material box and dried in an oven at 160℃ for 12 hours. After cooling to room temperature, it was passed through a 3-mesh sieve to remove large particles and agglomerates, resulting in dry and loose atomized nickel powder. The dried nickel powder was evenly fed into a steel strip furnace for continuous reduction treatment under an ammonia decomposition atmosphere. The reduction temperature for ordinary atomized nickel powder was controlled at 450℃, and for fine atomized nickel powder at 360℃. The ammonia decomposition furnace temperature was 920℃, the ammonia decomposition gas flow rate was 25 m³ / h, the steel strip frequency was 10 Hz, and the feed thickness was 30 mm and the width was 350 mm for even distribution. The reduced nickel powder was graded according to specifications by multi-stage vibration and ultrasonic sieving. The powder on the sieve was returned to the medium-frequency smelting process for recycling, while the qualified powder under the sieve was sent to a batching machine for thorough mixing to stabilize the loose packing density and particle size. The mixed finished product was accurately weighed at 25 ± 0.04 kg, vacuum-sealed, capped, and labeled with batch markings, and stored according to batch specifications. Testing showed that the particle size of the product obtained in this embodiment was qualified. For ordinary nickel powder, the hydrogen loss was ≤0.1% and the loose packing density was 2.7~3.2g / cm³. For fine nickel powder, the hydrogen loss was ≤0.09% and the loose packing density was 2.1~2.6g / cm³. The product had excellent flowability and batch stability met the requirements of high-end applications.

[0027] As can be seen from the above five embodiments, the method of the present invention can stably produce high-quality atomized nickel powder with qualified particle size, acceptable hydrogen loss, stable bulk density, and excellent flowability under different combinations of process parameters, demonstrating the wide applicability and stability of the method of the present invention. The particle size distribution, bulk density, flowability, and other physical properties of the nickel powder obtained in each embodiment all meet the requirements of high-end applications, and the consistency between product batches is good.

Claims

1. A method for producing atomized nickel powder in an industrial continuous stable production, characterized in that, Includes the following steps: (1) Furnace construction and drying: The furnace lining is prepared by mixing fused magnesia, boric acid and water glass. After the furnace is constructed by layering and compacting, it is dried according to the gradient power to complete the sintering of the furnace lining. (2) Medium frequency melting: Add dry nickel material to a medium frequency furnace, control the melting power to 90-150kW, and heat until completely melted to form molten nickel; (3) Deoxidation and slag removal: Add silicon-calcium alloy deoxidizer and slag remover to the nickel melt, stir, let stand, and then remove the surface slag to obtain clear nickel melt; (4) Water-air combined atomization: the deoxidized nickel liquid is poured into the preheated intermediate tundish and atomized into powder by high pressure water; (5) Drying and dehydration: Dry the atomized wet nickel powder at 90-170℃ for 7-12 hours, cool it and then sieve it to remove large particles; (6) Reduction protection: After drying, the nickel powder is continuously reduced in a steel strip furnace under an ammonia decomposition atmosphere; (7) Screening and batching: The reduced nickel powder is screened in multiple stages and then mixed in batches. (8) Packaging and warehousing: qualified products are weighed and vacuum-sealed.

2. The method of claim 1, wherein, The furnace charge in step (1) is a mixture of fused magnesia, water glass, boric acid and water. The fused magnesia contains three bags of each of four particle sizes: 0-1mm, 1-3mm, 3-5mm and 250 mesh. The water glass is 25kg and the boric acid content is 0.5-1%. 3-6kg of water is added and mixed until it can be formed into a ball by hand and can be easily dispersed by light pressure. The furnace bottom is compacted to a thickness of 15-21cm, the furnace collar is 10-15cm wide and 10-20cm high, and a V-shaped guide groove is reserved.

3. The method of claim 1, wherein, The gradient power oven described in step (1) is as follows: starting from 5kW, increasing by 5kW every 5 hours, and baking for 20 hours to 25kW; then increasing by 5kW every 3 hours, and baking for 15 hours to 45kW, with a total oven baking time of 35 hours.

4. The method of claim 1, wherein, In step (2), the nickel material must be dry and free of moisture. When feeding, first add lumpy nickel, and after the molten pool is formed, add nickel slag and sieve powder to prevent the material from being suspended or splashed. Stop feeding when the molten pool reaches the lower edge of the furnace.

5. The method of claim 1, wherein, In step (3), when the nickel material is melted to half the furnace, add 2 to 4 pieces of silicon-calcium alloy deoxidizer, each piece weighing about 50g; after the material is completely melted, reduce the power to 25kW, add 2 to 4 pieces of deoxidizer, stir for 1 minute, let stand for 5 minutes, then add 2 to 4 spoons of slag remover, each spoon weighing about 100g, and remove the slag until the nickel liquid is clear.

6. The method of claim 1, wherein, In step (4), the preheating temperature of the tundish is: 350±70℃ for furnace #1 and 890±50℃ for furnace #2; the atomizing water pressure is controlled at 5~15MPa for producing ordinary nickel powder, or 80~120kg for producing fine nickel powder; the atomization system is started in the following order: first start the high-pressure blower, then start the high-pressure pump. When producing fine nickel powder, the pre-pump must be started first and then the load added; the casting is slow and stable, and the molten liquid at the bottom of the furnace is not drained to protect the furnace lining.

7. The method of claim 1, wherein, In step (5), after drying, the product is cooled to room temperature and then passed through a 3-mesh sieve to remove large particles and clumps.

8. The method of claim 1, wherein, The reduction temperature in step (6) is: 480±50℃ for ordinary atomized nickel powder and 360±50℃ for micro-atomized nickel powder; the temperature of the ammonia decomposition furnace is 950±50℃, the flow rate of ammonia decomposition gas is 20±5m³ / h, the frequency of the steel strip furnace is 8±2Hz, and the feed thickness is 30~50mm and the width is 300~500mm.

9. The method of claim 1, wherein, In step (7), the powder on the sieve is returned to the medium-frequency melting process for recycling, and the qualified powder under the sieve is fed into the batching machine for thorough mixing to control the loose packing density.

10. The method according to claim 1, characterized in that, In step (8), the products are weighed at 25±0.04kg, vacuum sealed, capped, and labeled before being stored in batches.