A method and system for preparing blades

By using laser selective melting of nickel-based superalloy powder followed by stress-relief annealing, hot isostatic pressing densification, and two-stage aging heat treatment, the problems of precision forming, stress relief, defect closure, and microstructure homogenization in the blade forming process were solved, and the preparation of high-performance diffuser blades was realized.

CN123103019APending Publication Date: 2026-11-17AECC HUNAN AVIATION POWERPLANT RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611635711.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-22
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing blade forming processes cannot simultaneously achieve precision forming, stress relief, defect closure, microstructure homogenization, and performance enhancement, thus hindering the large-scale engineering application of laser selective melting technology in high-performance diffuser blades.

Method used

Nickel-based high-temperature alloy powder is deposited layer by layer through selective laser melting, combined with a process flow of stress-relief annealing, hot isostatic pressing densification, solution treatment, and two-stage aging heat treatment, including stress-relief annealing, hot isostatic pressing densification, solution treatment, and two-stage aging heat treatment, to optimize the microstructure and properties.

Benefits of technology

Significant improvements in the high-temperature strength and fatigue resistance of the blades were achieved. By synergistically regulating the microstructure, internal defects were eliminated, the microstructure was homogenized, and the performance was enhanced, thus meeting the service requirements of aero-engines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123103019A_ABST
    Figure CN123103019A_ABST
Patent Text Reader

Abstract

This invention, in the field of additive manufacturing and precision heat treatment of metallic materials, discloses a method and system for blade preparation. The method includes: depositing nickel-based high-temperature alloy powder layer by layer under a protective atmosphere using laser selective melting to obtain a blade blank; performing stress-relief annealing on the blade blank to eliminate residual stress generated during forming; performing hot isostatic pressing densification on the stress-controlled blade blank to eliminate internal porosity and incomplete fusion defects; performing solution treatment on the densified blade blank to fully dissolve the alloying elements and obtain a uniform austenitic matrix; and performing a two-stage aging heat treatment on the homogenized blade blank to precipitate strengthening phases to obtain a blade that meets service requirements. This invention achieves synergistic control of the densification, homogenization, and strengthening of the blade's microstructure, ultimately enabling the blade to obtain excellent high-temperature strength and fatigue resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of additive manufacturing and precision heat treatment technology of metal materials, and specifically relates to a method and system for preparing blades. Background Technology

[0002] Diffuser blades are core components of aero-engines and gas turbines, and their service performance directly affects the efficiency and reliability of the entire power plant. These components operate under extreme conditions of high-speed rotation, high temperature and pressure, and complex alternating loads, placing stringent requirements on material microstructure, internal defect control, mechanical properties, and dimensional accuracy. Traditional manufacturing methods for diffuser blades primarily rely on precision forging and precision casting. However, as aero-engines evolve towards higher efficiency, blades increasingly adopt integrated configurations with complex three-dimensional twisted surfaces and built-in fine cooling channels. Traditional forging and casting processes have gradually revealed their shortcomings: long manufacturing cycles, low material utilization, and difficulty in achieving complex internal cavity structures.

[0003] Selective laser melting (SLM), a typical process in metal additive manufacturing, relies on the layer-by-layer melting and deposition of metal powder to form components. It can process complex geometric structures that are difficult to achieve with traditional equal-material and subtractive processes, greatly improving the design freedom of parts and providing a new technical approach for the rapid manufacturing of complex metal components.

[0004] However, there are still many technical challenges in directly using selective laser melting (SLM) to manufacture high-performance diffuser blades: the rapid solidification characteristic of SLM makes it easy to generate metallurgical defects such as porosity and lack of fusion inside the parts, which can easily evolve into fatigue crack initiation points, endangering the service safety of the blades; the huge temperature gradient during the forming process will generate high residual stress, and thin-walled blades are prone to warping and cracking, resulting in low product yield; due to the influence of epitaxial growth and directional heat dissipation, coarse columnar crystal structures are easily formed inside the components, resulting in anisotropic mechanical properties, with particularly weak mechanical properties perpendicular to the construction direction; at the same time, the original non-equilibrium structure of additive manufacturing is difficult to meet the requirements of blades for high-temperature strength, creep resistance and long-term structural stability.

[0005] To address these issues, the industry typically employs post-processing techniques, but existing post-processing methods generally suffer from poor process coordination. Stress-relief annealing alone cannot close internal defects; direct hot isostatic pressing densification of components with high residual stress can easily induce part deformation and has limited effect on microstructure optimization; conventional heat treatment processes also struggle to eliminate material anisotropy and cannot precisely control the precipitation and distribution of strengthening phases.

[0006] In summary, existing blade forming processes cannot simultaneously achieve precision forming, stress relief, defect closure, microstructure homogenization, and performance enhancement, thus hindering the large-scale engineering application of laser selective melting technology in high-performance diffuser blades. Summary of the Invention

[0007] To address the above problems, the present invention provides a method for preparing blades, comprising the following steps: Nickel-based superalloy powder is deposited layer by layer by laser selective melting under a protective atmosphere to obtain a blade blank; The blade blank is subjected to stress-relief annealing to eliminate residual stress generated during the forming process; The stress-controlled blade blank is subjected to hot isostatic pressing densification treatment to eliminate internal porosity and incomplete fusion defects. The blade blank after densification is subjected to solution treatment to fully dissolve the alloying elements and obtain a uniform austenitic matrix structure. The blade blank, after being homogenized, is subjected to a two-stage aging heat treatment to precipitate strengthening phases and obtain blades that meet service requirements.

[0008] Furthermore, nickel-based superalloy powder is deposited layer by layer under a protective atmosphere by selective laser melting to obtain a blade blank, including the following steps: The substrate is subjected to rust removal, cleaning and drying treatment, and the nickel-based high-temperature alloy powder is subjected to vacuum drying treatment; A three-dimensional model of the blade is established based on the blade structural parameters, and a support structure is designed for the tenon and overhang areas in the three-dimensional model of the blade to obtain the blade printing model. Based on the blade printing model, a printing task file including the scanning path and process parameters is generated; The processed substrate and powder are loaded into a laser selective melting device, and after vacuuming, argon gas is introduced to create a protective atmosphere. The laser selective melting equipment prints out a supported blade blank according to the printing task file; after cooling, the supported blade blank is cut and separated from the substrate, and the support structure is removed to obtain the blade blank.

[0009] Furthermore, the blade blank undergoes stress-relief annealing, including the following steps: The blade blank is placed in the cold furnace of a vacuum heat treatment furnace; Heat to 900-1150℃ at a heating rate of 5-10℃ / min, and hold for a set time. After the heat preservation is completed, high-purity argon gas is introduced for forced cooling to room temperature, with a cooling pressure of 120 kPa ± 20 kPa.

[0010] Furthermore, the stress-controlled blade blank undergoes hot isostatic pressing densification treatment, including the following steps: The stress-controlled blade blank is placed into the furnace of a hot isostatic pressing equipment. The furnace of the hot isostatic pressing equipment is heated to 1170~1190℃ and pressurized to 150~180MPa, and held at the temperature and pressure for 2.5~3.5h. After the heat preservation and pressure holding are completed, the furnace is cooled to room temperature.

[0011] Furthermore, the blade blank after densification is subjected to solution treatment, including the following steps: The densified blade blanks are placed in a protective atmosphere heat treatment furnace. The temperature is increased to 980℃±10℃ at a rate of 5~10℃ / min, and the temperature is held for a set time. After the holding time is completed, argon gas is used for forced cooling at a cooling pressure of 120kPa±20kPa to rapidly cool the temperature to room temperature.

[0012] Furthermore, the blade blank after tissue homogenization treatment undergoes a two-stage aging heat treatment, including the following steps: The blade blank after the tissue homogenization treatment is subjected to the first stage of aging heat treatment, which includes: holding at 720℃±10℃ for a set time, and furnace cooling to 620℃±10℃ at a controlled rate of 50±10℃ / h. After the tissue homogenization treatment, the blade blanks undergo a second-stage aging heat treatment, which includes holding at 620℃±10℃ for a set time and then cooling to room temperature with argon gas.

[0013] Furthermore, the process parameters include: laser power of 300~500W, scanning speed of 1000~1100m / s, channel spacing of 0.08~0.12mm, tolerance controlled within ±0.03mm, powder layer thickness of 0.03~0.06mm, tolerance controlled within ±0.0005mm, and the scanning strategy is a Zigzag scanning strategy.

[0014] Furthermore, the particle size of the nickel-based superalloy powder is 15-53 μm.

[0015] The present invention also provides a diffuser blade, which is prepared by the blade preparation method described above.

[0016] The present invention also provides a blade preparation system, comprising: Laser selective melting equipment is used to deposit nickel-based superalloy powder layer by layer under a protective atmosphere through laser selective melting to obtain blade blanks; Vacuum heat treatment furnace is used to perform stress-relieving annealing on blade blanks to eliminate residual stress generated during the forming process. Hot isostatic pressing equipment is used to perform hot isostatic pressing densification treatment on stress-controlled blade blanks to eliminate internal porosity and incomplete fusion defects. A protective atmosphere heat treatment furnace is used to perform solution treatment on the densified blade blanks to fully dissolve the alloying elements and obtain a uniform austenitic matrix structure. A temperature-controlled, sealed heat treatment furnace is used to perform two-stage aging heat treatment on blade blanks after microstructure homogenization to precipitate strengthening phases and obtain blades that meet service requirements.

[0017] The beneficial effects of this invention are: This invention places stress-relief annealing before hot isostatic pressing (HIP), releasing most of the printing stress and avoiding the risk of deformation due to residual stress during HIP. Through a combined post-processing flow of HIP, solution treatment, and two-stage aging, the synergistic control of the microstructure densification, homogenization, and strengthening of the blade is achieved. HIP closes internal defects, solution treatment optimizes the matrix, and two-stage aging precipitates nanoscale strengthening phases, ultimately giving the blade excellent high-temperature strength and fatigue resistance.

[0018] Other features and advantages of the invention will be set forth in the following description, and will be apparent in part from the description, or may be learned by practicing the invention. The objects and other advantages of the invention may be realized and obtained by means of the structures pointed out in the description and the drawings. Attached Figure Description

[0019] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0020] Figure 1 A schematic diagram of the main process of a blade preparation method according to an embodiment of the present invention is shown; Figure 2 A schematic diagram of diffuser blade partitioning according to an embodiment of the present invention is shown; Figure 3 A schematic diagram of a laser selective melting and forming scanning strategy according to an embodiment of the present invention is shown; Figure 4 A schematic diagram of the process curve for a two-stage aging heat treatment according to an embodiment of the present invention is shown; Figure 5 A schematic diagram of the blade microstructure obtained by a conventional single additive manufacturing process is shown. Figure 6 A schematic diagram of the leaf microstructure obtained by the preparation method according to an embodiment of the present invention is shown; Figure 7A schematic diagram of a blade manufacturing system according to an embodiment of the present invention is shown. Detailed Implementation

[0021] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0022] It should be noted that the terms "first," "second," etc., used in this application are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate for the embodiments of this application described herein.

[0023] This invention provides a blade manufacturing method and system for manufacturing high-performance diffuser blades for high-end equipment such as aero engines and gas turbines. By constructing a collaboratively controlled laser selective melting forming and post-processing integrated process, the overall performance of diffuser blades is systematically improved.

[0024] like Figure 1 As shown, a method for preparing a blade includes the following steps: S1. Selective Laser Melting (SLM) step: Nickel-based superalloy powder is deposited layer by layer in a protective atmosphere by selective laser melting to obtain a blade blank.

[0025] The goal of this step is to obtain a blade blank with accurate geometric dimensions, as few internal defects as possible, and preliminary control of residual stress.

[0026] For example, step S1 specifically includes: removing rust, cleaning and drying the substrate, and vacuum drying the nickel-based high-temperature alloy powder; establishing a three-dimensional model of the blade based on the blade structure parameters, and designing support structures for the tenon and overhang areas in the three-dimensional model of the blade to obtain a blade printing model; generating a printing task file including scanning path and process parameters based on the blade printing model; loading the processed substrate and powder into a laser selective melting device, evacuating and filling with argon to establish a protective atmosphere; printing a supported blade blank based on the printing task file using the laser selective melting device; cutting and separating the cooled supported blade blank from the substrate, removing the support structure to obtain the blade blank.

[0027] Table 1

[0028] For example, as shown in Table 1, the process parameters include: laser power of 300~500W, scanning speed of 1000~1100m / s, channel spacing of 0.08~0.12mm, tolerance controlled within ±0.03mm, powder layer thickness of 0.03~0.06mm, tolerance controlled within ±0.0005mm, and the scanning strategy is to adopt a zigzag scanning strategy.

[0029] This invention ensures high dimensional accuracy and low defect rate of the formed blank by precisely controlling the process parameters of laser selective melting forming.

[0030] The present invention will be described in detail using the manufacture of diffuser blades of a certain type of nickel-based high-temperature alloy (such as GH4169 alloy) as an example.

[0031] Select laser selective melting equipment with a highly stable beam, a precision powder spreading system, and high-precision oxygen content control (usually required to be <100ppm).

[0032] The substrate is made of the same material as the blade or has similar thermophysical properties, typically GH4169 alloy forged plate. Before being mounted on the machine, the substrate must be sandblasted, cleaned, and dried to ensure that its surface is free of oil and oxide scale, thus guaranteeing a good bond with the formed part.

[0033] The powder material is spherical IN718 alloy powder prepared by the plasma rotating electrode method, with a preferred particle size distribution of 15-53 μm. Before use, the powder needs to be dried in a vacuum drying oven at 80℃~100℃ for at least 2 hours to remove adsorbed moisture and prevent the formation of pores during the forming process.

[0034] Import the blade's CAD model into the equipment slicing software to generate a printing task file that includes the scanning path and process parameters, such as... Figure 2 As shown, the CAD model of the blade is imported into the equipment slicing software, and the CAD model of the blade is divided into an annular gasket area and multiple fan-shaped blade units.

[0035] The annular gasket area is located at the bottom of the blade in contact with the substrate. It is used to establish a stable molten pool transition zone in the early stage of forming, buffer the difference in thermal properties between the substrate and the blade body, and avoid interlayer cracking caused by abrupt changes in heat conduction rate. Multiple fan-shaped blade units are evenly distributed circumferentially, and each fan-shaped unit corresponds to an independent scanning zone. Each zone has its own planned scanning path and process parameters.

[0036] Through the above-mentioned partitioning design, the following beneficial effects can be achieved in the laser selective melting forming process: First, dividing the large-area continuous scanning area into several smaller fan-shaped units effectively avoids excessive local heat accumulation caused by long-line scanning, making the temperature field distribution within the layer more uniform, thereby significantly reducing the thermal stress and residual stress generated during the forming process; Second, the independent scanning path planning of each partition allows the melting channel directions between adjacent partitions to be staggered. Combined with the strategy of rotating the scanning direction by 67° after each layer is completed, the continuous epitaxial growth of columnar crystals can be effectively interrupted, weakening the mechanical anisotropy of the component; Third, the annular gasket area acts as a stress buffer zone, concentrating the thermal stress between the blade body and the substrate in the gasket area, reducing the risk of warping deformation of the blade body, especially the thin-walled blade section; Fourth, the partitioned scanning strategy facilitates the differential adjustment of process parameters such as laser power and scanning speed according to the structural characteristics of different regions in subsequent printing tasks, achieving the matching and control of the microstructure properties of different regions of the component.

[0037] To reduce deformation, necessary support structures need to be designed and constructed at the contact area between the blade tenon and the substrate, as well as below any potential overhangs on the blade. These support structures are typically point- or line-shaped, designed to distribute thermal stress and provide sufficient support while facilitating subsequent removal.

[0038] The prepared substrate and powder are loaded into the equipment, vacuumed, and filled with high-purity argon gas (purity ≥99.999%) until a protective atmosphere is established.

[0039] Set the following key process parameters and start construction: The laser power is set to 400W (selected within the range of 300~500W). This power value ensures that the powder is completely melted, forming a good molten pool, while avoiding excessive evaporation and splashing due to excessive power.

[0040] The scanning speed was set to 1050 mm / s (selected within the range of 1000~1100 m / s). This speed, combined with the laser power, forms a suitable volumetric energy density, ensuring a stable molten pool and good overlap.

[0041] The run spacing is set to 0.10 mm (selected within the range of 0.08~0.12 mm), with tolerances strictly controlled within ±0.03 mm. Appropriate run spacing ensures sufficient overlap between adjacent runners, avoiding incomplete fusion defects.

[0042] The powder coating thickness is set to 0.04 mm (selected within the range of 0.03~0.06 mm), with tolerance strictly controlled within ±0.0005 mm. This extremely narrow coating thickness tolerance is crucial for ensuring dimensional accuracy and surface finish at the thin-walled sections of the blade.

[0043] A zigzag scanning strategy is employed, with the scanning direction rotating by 67° after each layer is completed. This rotation angle, which is not an integer multiple of 90°, effectively interrupts the continuous epitaxial growth of columnar crystals and is one of the core methods to reduce the anisotropy of the formed part.

[0044] like Figure 3 As shown, Figure 3 The diagram illustrates a zigzag scanning strategy, where Layer n, Layer n+1, and Layer n+2 are continuously formed layers. The arrows in the diagram represent the laser scanning direction. After each layer is printed, the laser scanning direction for the next layer rotates by a set angle, resulting in an alternating arrangement of melt paths. This scanning strategy is used to interrupt the continuous epitaxial growth of columnar crystals, weaken the mechanical anisotropy of the component, disperse the accumulated printing heat, reduce residual stress, and improve the interlayer fusion quality.

[0045] During the forming process, the galvanometer system of the laser selective melting equipment performs closed-loop control on the scanning speed and track spacing; the grating ruler monitors and provides feedback on the powder layer thickness in real time at a frequency of up to 5kHz, ensuring the laying accuracy of each layer.

[0046] After construction, the blade blank is cooled to below 80°C in the furnace. The formed substrate is removed, and the supported blade blank is separated from the substrate by wire cutting. The support structure is carefully removed by mechanical grinding or electrochemical methods, and the contact area of ​​the support is preliminarily ground to obtain the blade blank.

[0047] S2. Stress control steps: Perform stress-relief annealing on the blade blank to eliminate residual stress generated during the forming process.

[0048] For example, stress-relief annealing of blade blanks includes: placing the blade blank in the cold furnace of a vacuum heat treatment furnace, heating it to 900~1150℃ at a heating rate of 5~10℃ / min, holding it for a set time, for example, the holding time can be 1 hour; after the holding time is completed, high-purity argon gas is introduced for forced cooling to room temperature, wherein the cooling pressure is 120kPa±20kPa.

[0049] This step aims to release most of the macroscopic residual stress generated during the laser selective melting process, in order to prepare for the subsequent hot isostatic pressing densification process and avoid uncontrollable deformation of the parts caused by direct hot isostatic pressing under high stress.

[0050] For example, the blade blank obtained in step S1 is placed in the cold furnace of a vacuum heat treatment furnace. It is heated to 1050°C (selected within the range of 900~1150°C) at a heating rate of 5~10°C / min.

[0051] After reaching the temperature, hold for 1 hour. The holding time is sufficient to allow atoms to diffuse fully, complete the recovery and recrystallization process, and thus effectively relax the internal stress.

[0052] After the heat preservation is completed, high-purity argon gas is introduced into the furnace, and the gas pressure is rapidly increased to 120 kPa (for VGQ240 and smaller equipment, the pressure is controlled at 120 ± 20 kPa) to force-cool the blades until they reach room temperature. Rapid cooling can prevent the precipitation of certain brittle phases.

[0053] During the stress-relief annealing process, the temperature curve is recorded throughout the process by temperature control thermocouples and instruments in the furnace to ensure that the actual temperature is within ±10℃ of the set value; the cooling pressure is monitored by a pressure transmitter.

[0054] S3. Densification process: The stress-controlled blade blank is subjected to hot isostatic pressing densification to eliminate internal pores and incomplete fusion defects.

[0055] For example, hot isostatic pressing densification treatment is performed on the stress-controlled blade blank, including: placing the stress-controlled blade blank into the furnace of a hot isostatic pressing equipment; heating the furnace to 1170~1190℃ and pressurizing it to 150~180MPa, and holding it at the temperature and pressure for 2.5~3.5h; and cooling it to room temperature with the furnace after the holding and pressure treatment is completed.

[0056] This step is crucial for closing internal defects and achieving material densification. After stress relief in step S2, the risk of part deformation is reduced, making hot isostatic pressing (HIP) the optimal treatment at this stage.

[0057] For example, the blades processed in step S2 are placed in the furnace of a hot isostatic pressing equipment, and high temperature and high pressure are applied simultaneously. The temperature is raised to 1180°C (selected in the range of 1170~1190°C), and an isostatic pressure of 165MPa (selected in the range of 150~180MPa) is applied.

[0058] Under the target temperature and pressure, the material is held at the same temperature and pressure for 3 hours (selected within the range of 2.5~3.5h). Under the combined action of high temperature and hydrostatic pressure, the micropores and defects such as incomplete fusion remaining inside the blade undergo plastic flow and diffusion connection and are effectively welded together. After the process is completed, the material is cooled to room temperature in the furnace.

[0059] During the hot isostatic pressing densification process, the temperature is monitored (tolerance ±10℃) by the equipment's PLC and temperature control instrument, and the pressure is monitored (tolerance ±2MPa) by the pressure transmitter.

[0060] S4. Homogenization treatment step: The blade blank after densification treatment is subjected to solution treatment to fully dissolve the alloying elements and obtain a uniform austenitic matrix structure.

[0061] For example, solution treatment of the densified blade blank includes: placing the densified blade blank in a protective atmosphere heat treatment furnace; heating to 980℃±10℃ at a rate of 5~10℃ / min, holding for a set time, and after the holding is completed, using argon gas for forced cooling at a cooling pressure of 120kPa±20kPa to rapidly cool to room temperature.

[0062] The purpose of this step is to dissolve the unfavorable carbides or δ phases that may precipitate during laser selective melting and hot isostatic pressing densification, to obtain a supersaturated single austenitic solid solution, in preparation for subsequent aging precipitation, and to further homogenize the microstructure.

[0063] For example, a protective atmosphere heat treatment furnace can be used, such as a vacuum heat treatment furnace or a controlled atmosphere heat treatment furnace, to heat the blades to 980°C at a rate of 5~10°C / min. The temperature is then held for 1 hour to allow the alloying elements to fully dissolve into the matrix.

[0064] After the heat preservation is completed, the material is rapidly cooled to room temperature using the same argon forced cooling method (pressure 120±20Kpa) as S2 to obtain a supersaturated solid solution.

[0065] During the solution treatment process, the temperature controller monitors the temperature (±10℃), and the pressure transmitter monitors the cooling pressure.

[0066] S5. Performance enhancement treatment steps: The blade blank after the microstructure homogenization treatment is subjected to two-stage aging heat treatment to precipitate the strengthening phase and obtain a blade that meets the service requirements.

[0067] like Figure 4 As shown, the blade blank after microstructure homogenization treatment undergoes a two-stage aging heat treatment, including: The blade blank after the tissue homogenization treatment is subjected to the first stage of aging heat treatment, which includes: holding at 720℃±10℃ for a set time (e.g., 8 hours), and furnace cooling to 620℃±10℃ at a controlled rate of 50±10℃ / h. After the tissue homogenization treatment, the blade blank undergoes a second-stage aging heat treatment, which includes holding at 620℃±10℃ for a set time (e.g., 8 hours), and finally cooling to room temperature with argon gas.

[0068] This step is crucial for achieving precipitation strengthening and obtaining the final mechanical properties. By precisely controlling the precipitation process, the γ' and γ" strengthening phases are uniformly dispersed at the nanoscale with high density.

[0069] For example, the two-stage aging heat treatment uses a temperature-controlled closed heat treatment furnace, which can be a box furnace or a vacuum furnace with high program temperature control accuracy.

[0070] The first stage of aging heat treatment involves placing the blades in a furnace preheated to 720°C and holding them there for 8 hours. This stage primarily promotes the formation and initial growth of metastable γ" phase (Ni3Nb) nuclei.

[0071] After the heat treatment was completed, the furnace was slowly cooled to 620°C at a precisely controlled rate of 50°C / h. This slow cooling process was crucial for the continued precipitation of the γ" phase and its transition to a stable state.

[0072] The second-stage aging heat treatment process includes holding at 620℃ for another 8 hours. This stage aims to further grow and stabilize the strengthening phase, and may be accompanied by the supplementary precipitation of the γ' phase (Ni3(Al,Ti)) to achieve the best strengthening effect.

[0073] After the second stage of aging heat treatment is completed, argon gas (pressure 120±20Kpa) is introduced to cool to room temperature.

[0074] During the two-stage aging heat treatment process, the temperature is monitored by a temperature control instrument to ensure that the first-stage aging temperature tolerance is ±10℃, the second-stage aging temperature tolerance is ±5℃, and the holding time tolerance is ±15min.

[0075] The preparation method of this invention has clear tolerance ranges and monitoring methods for each key process, which ensures the stability of the process and the consistency of the product, making it particularly suitable for mass production quality control of aerospace products.

[0076] like Figure 5 The diagram shows the microstructure of a blade obtained by a single additive manufacturing process without the post-processing described in this invention. Figure 5 As can be seen, its matrix structure is mainly composed of coarse columnar or cellular crystals that grow epitaxially along the construction direction. The interior of the grains is a supersaturated solid solution, and there is obvious microsegregation.

[0077] like Figure 6 The image shown is a schematic diagram of the leaf microstructure obtained by the preparation method of this invention. Figure 6 As can be seen, after post-processing using the technology of this invention, the matrix structure transforms into uniform and fine austenitic γ-equiaxed grains with clear grain boundary outlines. A suitable amount of lath-like δ-phase is distributed within the grains and at the grain boundaries, which can pin the grain boundaries and improve creep resistance. Furthermore, no metallurgical defects such as porosity or lack of fusion are observed in the metallographic field of view, indicating high component density. This embodiment of the invention effectively weakens the inherent mechanical anisotropy of SLM components through the optimization of laser selective melting process parameters and the synergistic control of subsequent heat treatment, and rationally controls the distribution of strengthening phases and δ-phase, thereby meeting the high-temperature strength and microstructure stability requirements of aerospace diffuser blades.

[0078] The preparation method of this invention, through its process sequence, places stress-relief annealing before hot isostatic pressing (HIP) to preferentially release printing stress, fundamentally avoiding the risk of deformation of high residual stress components during HIP. Secondly, through a specific post-treatment combination of HIP, solution treatment, and two-stage aging, it systematically achieves synergistic control over the densification, homogenization, and strengthening of the blade's structure and properties, with an overall effect far exceeding the simple summation of individual steps. Finally, at the forming source, extremely precise process control (such as a powder layer thickness tolerance of ±0.0005 mm and a scanning strategy that is not an integer multiple of 90°) ensures low defects, low anisotropy, and high precision of the preform, laying a solid foundation for subsequent processing.

[0079] This invention also provides a diffuser blade, which is prepared by the above-described blade preparation method. The prepared diffuser blade exhibits excellent high-temperature strength and fatigue resistance.

[0080] Based on the above blade preparation method, such as Figure 7 As shown, this embodiment of the invention also provides a blade preparation system, including a laser selective melting device, a vacuum heat treatment furnace, a hot isostatic pressing device, a protective atmosphere heat treatment furnace, and a temperature-controlled sealed heat treatment furnace.

[0081] Among them, the laser selective melting equipment is used to deposit nickel-based high-temperature alloy powder layer by layer under a protective atmosphere through laser selective melting to obtain a blade blank.

[0082] Vacuum heat treatment furnaces are used to perform stress-relief annealing on blade blanks to eliminate residual stress generated during the forming process.

[0083] Hot isostatic pressing equipment is used to perform hot isostatic pressing densification treatment on stress-controlled blade blanks to eliminate internal porosity and incomplete fusion defects.

[0084] A protective atmosphere heat treatment furnace is used to perform solution treatment on the densified blade blanks to fully dissolve the alloying elements and obtain a uniform austenitic matrix structure.

[0085] A temperature-controlled, sealed heat treatment furnace is used to perform two-stage aging heat treatment on blade blanks after microstructure homogenization to precipitate strengthening phases and obtain blades that meet service requirements.

[0086] The preparation system of this invention consists of a laser selective melting device, a vacuum heat treatment furnace, a hot isostatic pressing device, a protective atmosphere heat treatment furnace, and a temperature-controlled closed heat treatment furnace, forming a complete preparation system. The synergistic technical effect achieved by each device in the preparation system is to systematically solve the problems from precision forming, stress relief, defect closure to microstructure homogenization and performance enhancement.

[0087] Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a blade, characterized in that, Includes the following steps: Nickel-based superalloy powder is deposited layer by layer by laser selective melting under a protective atmosphere to obtain a blade blank; The blade blank is subjected to stress-relief annealing to eliminate residual stress generated during the forming process; The stress-controlled blade blank is subjected to hot isostatic pressing densification treatment to eliminate internal porosity and incomplete fusion defects. The blade blank after densification is subjected to solution treatment to fully dissolve the alloying elements and obtain a uniform austenitic matrix structure. The blade blank, after being homogenized, is subjected to a two-stage aging heat treatment to precipitate strengthening phases and obtain blades that meet service requirements.

2. The blade preparation method according to claim 1, characterized in that, Nickel-based superalloy powder is deposited layer by layer under a protective atmosphere by selective laser melting to obtain a blade blank, including the following steps: The substrate is subjected to rust removal, cleaning and drying treatment, and the nickel-based high-temperature alloy powder is subjected to vacuum drying treatment; A three-dimensional model of the blade is established based on the blade structural parameters, and a support structure is designed for the tenon and overhang areas in the three-dimensional model of the blade to obtain the blade printing model. Based on the blade printing model, a printing task file including the scanning path and process parameters is generated; The processed substrate and powder are loaded into a laser selective melting device, and after vacuuming, argon gas is introduced to create a protective atmosphere. The laser selective melting equipment prints out a supported blade blank according to the printing task file; after cooling, the supported blade blank is cut and separated from the substrate, and the support structure is removed to obtain the blade blank.

3. The blade preparation method according to claim 1, characterized in that, The stress-relief annealing process for the blade blank includes the following steps: The blade blank is placed in the cold furnace of a vacuum heat treatment furnace; Heat to 900-1150℃ at a heating rate of 5-10℃ / min, and hold for a set time. After the heat preservation is completed, high-purity argon gas is introduced for forced cooling to room temperature, with a cooling pressure of 120 kPa ± 20 kPa.

4. The blade preparation method according to claim 1, characterized in that, The stress-controlled blade blank undergoes hot isostatic pressing densification treatment, including the following steps: The stress-controlled blade blank is placed into the furnace of a hot isostatic pressing equipment. The furnace of the hot isostatic pressing equipment is heated to 1170~1190℃ and pressurized to 150~180MPa, and held at the temperature and pressure for 2.5~3.5h. After the heat preservation and pressure holding are completed, the furnace is cooled to room temperature.

5. The blade preparation method according to claim 1, characterized in that, Solution treatment is performed on the densified blade blank, including the following steps: The densified blade blanks are placed in a protective atmosphere heat treatment furnace. The temperature is increased to 980℃±10℃ at a rate of 5~10℃ / min, and the temperature is held for a set time. After the holding time is completed, argon gas is used for forced cooling at a cooling pressure of 120kPa±20kPa to rapidly cool the temperature to room temperature.

6. The blade preparation method according to claim 1, characterized in that, The blade blank, after undergoing tissue homogenization treatment, is subjected to a two-stage aging heat treatment, including the following steps: The blade blank after the tissue homogenization treatment is subjected to the first stage of aging heat treatment, which includes: holding at 720℃±10℃ for a set time, and furnace cooling to 620℃±10℃ at a controlled rate of 50±10℃ / h. After the tissue homogenization treatment, the blade blanks undergo a second-stage aging heat treatment, which includes holding at 620℃±10℃ for a set time and then cooling to room temperature with argon gas.

7. The method for preparing blades according to any one of claims 1-6, characterized in that, The process parameters include: laser power of 300~500W, scanning speed of 1000~1100m / s, channel spacing of 0.08~0.12mm, tolerance controlled within ±0.03mm, powder layer thickness of 0.03~0.06mm, tolerance controlled within ±0.0005mm, and the scanning strategy is to adopt the Zigzag scanning strategy.

8. The blade preparation method according to claim 1, characterized in that, The particle size of nickel-based superalloy powder is 15-53 μm.

9. A diffuser blade, characterized in that, The blade is prepared using the blade preparation method described in any one of claims 1-8.

10. A blade preparation system, characterized in that, include: Laser selective melting equipment is used to deposit nickel-based superalloy powder layer by layer under a protective atmosphere through laser selective melting to obtain blade blanks; Vacuum heat treatment furnace is used to perform stress-relieving annealing on blade blanks to eliminate residual stress generated during the forming process. Hot isostatic pressing equipment is used to perform hot isostatic pressing densification treatment on stress-controlled blade blanks to eliminate internal porosity and incomplete fusion defects. A protective atmosphere heat treatment furnace is used to perform solution treatment on the densified blade blanks to fully dissolve the alloying elements and obtain a uniform austenitic matrix structure. A temperature-controlled, sealed heat treatment furnace is used to perform two-stage aging heat treatment on blade blanks after microstructure homogenization to precipitate strengthening phases and obtain blades that meet service requirements.