A method for welding and forming high permeability soft magnetic alloys

By controlling the heat input and annealing process of electron beam welding, the problems of grain coarsening and element segregation during the welding of high permeability soft magnetic alloys have been solved, thereby improving the welding quality and magnetic properties, and making it suitable for the manufacture of complex structural parts.

CN123103148APending Publication Date: 2026-11-17XIAN GANGYAN SPECIAL ALLOY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611188989.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-06
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In traditional welding processes, abnormal grain growth and element segregation occur in the weld and heat-affected zone of high-permeability soft magnetic alloys, leading to a decrease in magnetic properties and making it difficult to meet the requirements of complex components.

Method used

By controlling the heat input of electron beam welding and combining it with annealing, grain coarsening and elemental segregation are suppressed, and appropriate annealing conditions are used to restore the microstructure uniformity and magnetic properties of the welded area.

Benefits of technology

It effectively suppresses grain coarsening and element segregation in the weld and heat-affected zone, improves welding quality and dimensional accuracy, restores post-weld magnetic properties, and achieves synergistic optimization of weld formation, dimensional accuracy, and magnetic properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123103148A_ABST
    Figure CN123103148A_ABST
Patent Text Reader

Abstract

This invention relates to the field of soft magnetic alloy technology, specifically to a method for welding and forming a high-permeability soft magnetic alloy. The method includes: clamping and fixing the soft magnetic alloy in a welding chamber; performing electron beam welding under preset first conditions, wherein the heat input of the electron beam welding is within a preset heat input threshold range, to obtain a first welding alloy; annealing the first welding alloy according to a target magnetic property to obtain a second welding alloy; and heat-treating the second welding alloy to obtain a finished soft magnetic alloy. This invention effectively suppresses grain coarsening and elemental segregation in the weld and heat-affected zone by controlling the heat input of electron beam welding; it promotes uniform microstructure at the weld by employing corresponding annealing processes according to different magnetic property requirements; and it restores the post-weld magnetic properties through heat treatment. This achieves synergistic optimization of welding formation, dimensional accuracy, and magnetic property recovery, and is suitable for manufacturing complex structural parts made of high-permeability soft magnetic alloys.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of soft magnetic alloy technology, and more specifically to a method for welding and forming a high-permeability soft magnetic alloy. Background Technology

[0002] High-permeability soft magnetic alloys possess excellent magnetic properties such as high permeability, low coercivity, and low hysteresis loss, and are widely used in aerospace, electronics, precision instruments, medical equipment, and power equipment. They are often used as important materials for magnetic shielding structures, magnetic circuit components, and electromagnetic conversion devices. As equipment develops towards larger, more complex, and lighter designs, the difficulty and cost of integrally forging or machining complex soft magnetic alloy components are constantly increasing. Therefore, using welding to form complex components is gradually becoming an important manufacturing method.

[0003] However, high permeability soft magnetic alloys are extremely sensitive to microstructure and residual stress. In traditional welding processes, high heat input can easily lead to abnormal grain growth, element segregation, and concentration of residual stress in the weld and heat-affected zone, which can damage the magnetic domain structure, significantly reduce the initial and maximum permeability of the material, increase coercivity, and make it difficult to meet the application requirements after welding.

[0004] Therefore, how to balance magnetic properties while welding is a current research direction. Summary of the Invention

[0005] (a) Purpose of the invention The purpose of this invention is to provide a method for welding and forming high-permeability soft magnetic alloys. By controlling the heat input of electron beam welding, the method effectively suppresses grain coarsening and element segregation in the weld and heat-affected zone. According to different magnetic performance requirements, corresponding annealing processes are adopted to promote the homogenization of the microstructure at the weld and restore the post-weld magnetic properties through heat treatment.

[0006] (II) Technical Solution To address the above problems, this invention provides a method for welding and forming high-permeability soft magnetic alloys, comprising: The soft magnetic alloy is clamped and fixed in the welding chamber, and electron beam welding is performed under preset first conditions and then cooled to obtain the first welding alloy. According to the target magnetic properties, the first welding alloy is annealed to obtain a second welding alloy, comprising: If the target magnetic properties are the first magnetic property requirements, the first welding alloy is annealed according to the preset second conditions to obtain the second welding alloy. If the target magnetic properties are the second magnetic property requirements, the first welding alloy is annealed according to the preset third conditions to obtain the second welding alloy. The second welding alloy is heat-treated to obtain a soft magnetic alloy product.

[0007] In another aspect of the present invention, preferably, the soft magnetic alloy comprises: C, Mn, Si, P, S, Cr, Mo, Cu, Co, Ni, Ce, Fe and unavoidable impurities, wherein by mass percentage, C≤0.05%, Mn≤0.80%, Si≤0.05%, P≤0.030%, S≤0.010%, Cr≤0.30%, Mo≤0.30%, Cu≤0.30%, Co≤0.50%, Ni is 43.5%~46.5%, Ce is 0.1%~0.2%, and the balance is Fe and unavoidable impurities.

[0008] In another aspect of the invention, preferably, the preset first condition includes: vacuum to 3 × 10⁻⁶. -3 Pa ~ 7×10 - 3 Pa, accelerating voltage of 80KV~90KV, electron beam current of 20mA~30mA, welding speed of 150cm / min~200cm / min.

[0009] In another aspect, preferably, the invention further includes: pre-treating the soft magnetic alloy before welding to obtain a pre-treated soft magnetic alloy.

[0010] In another aspect of the present invention, preferably, the first magnetic properties require: μi ≥ 3.1 mH / m; maximum permeability μm ≥ 31.3 mH / m; coercivity Hc ≤ 14.4 A / m; and magnetic flux density B (8000~40000) ≥ 1.5 T at room temperature. The preset second condition includes: heating the furnace to the first temperature and holding it at that temperature for a first time, then cooling the furnace.

[0011] In another aspect of the present invention, preferably, the first temperature is 400℃~500℃, and the temperature is maintained for 4h~6h.

[0012] In another aspect of the present invention, preferably, the second magnetic performance requirement is higher than the first magnetic performance requirement; The preset third condition includes: After being held at a first vacuum level and a second temperature for a second time, the furnace is cooled to a third temperature and then cooled to room temperature at a preset cooling rate.

[0013] In another aspect of the present invention, preferably, the first vacuum degree is less than or equal to 10. -3 Pa, the second temperature is 800℃~1000℃, the second time is 4h~6h, the third temperature is 500℃~600℃, and the preset cooling rate is 180℃ / h~220℃ / h.

[0014] In another aspect of the present invention, preferably, the heat treatment includes: placing the second welding alloy in a hydrogen furnace with an ambient dew point of less than -60°C or a vacuum furnace with a vacuum degree of less than or equal to a second vacuum degree; The temperature is raised to the fourth temperature within the third time period, and then maintained at that temperature for the fourth time. The temperature is raised to the fifth temperature within the fifth time period, and then maintained at that temperature for the sixth time. The furnace temperature is lowered to the sixth temperature, and then held for the seventh time. The furnace is cooled to the seventh temperature, and nitrogen is used for cooling at a rate of ≥200℃ / h.

[0015] In another aspect of the invention, preferably, the second vacuum degree is less than or equal to 10. -3 Pa, the third time is 2h, the fourth temperature is 1000±20℃, the fourth time is 40~60min; the fifth time is 30min, the fifth temperature is 1160±20℃, the sixth time is 40~60min; the sixth temperature is 800~900℃, the seventh time is 60~90min, the seventh temperature is 600℃.

[0016] (III) Beneficial Effects The above-described technical solution of the present invention has the following beneficial technical effects: This invention effectively suppresses grain coarsening and elemental segregation in the weld and heat-affected zone by controlling the heat input of electron beam welding, thereby reducing residual welding stress and welding deformation of thin-walled parts, and improving welding quality and dimensional accuracy. It also employs corresponding annealing processes based on different magnetic performance requirements to promote uniform microstructure of the weld joint, and restores post-weld magnetic properties through heat treatment, increasing initial and maximum permeability while reducing coercivity. This achieves synergistic optimization of welding formation, dimensional accuracy, and magnetic performance recovery, making it suitable for manufacturing complex structural parts made of high-permeability soft magnetic alloys. Attached Figure Description

[0017] Figure 1 This is an overall flowchart of one embodiment of the present invention. Detailed Implementation

[0018] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to specific embodiments and the accompanying drawings. It should be understood that these descriptions are merely exemplary and not intended to limit the scope of the invention. Furthermore, descriptions of well-known structures and techniques are omitted in the following description to avoid unnecessarily obscuring the concept of the invention.

[0019] Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.

[0020] In the description of this invention, it should be noted that the terms "first," "second," and "third" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.

[0021] Furthermore, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0022] Example A method for welding and forming a high-permeability soft magnetic alloy. Figure 1 An overall flowchart of one embodiment of the present invention is shown, as follows: Figure 1 As shown, it includes: The soft magnetic alloy can be an iron-nickel based high-permeability soft magnetic alloy, an iron-cobalt based soft magnetic alloy, an iron-silicon based soft magnetic alloy, or other soft magnetic alloys with high permeability. In this embodiment, the soft magnetic alloy is an iron-nickel based high-permeability soft magnetic alloy. The soft magnetic alloy includes: C, Mn, Si, P, S, Cr, Mo, Cu, Co, Ni, Ce, Fe, and unavoidable impurities. By mass percentage, C≤0.05%, Mn≤0.80%, Si≤0.05%, P≤0.030%, S≤0.010%, Cr≤0.30%, Mo≤0.30%, Cu≤0.30%, Co≤0.50%, Ni is 43.5%~46.5%, Ce is 0.1%~0.2%, and the balance is Fe and unavoidable impurities. Metallic cerium can combine with O and S during smelting to preferentially form high-melting-point Ce₂O₃, CeS, and Ce₂O₂S, removing free oxygen and low-melting-point sulfide impurities at grain boundaries from the alloy. It also eliminates harmful phases such as FeS and NiS, which easily cause hot brittleness and welding hot cracking, improving the hot working plasticity and weldability of thin strips. Furthermore, rare earth elements can effectively refine grains, mitigating the obstacles to grain growth during hot and cold forming, thus improving the cast / cold rolled microstructure of the alloy. Metallic cerium can purify and refine the alloy microstructure, thereby increasing the alloy's magnetic permeability and reducing its coercivity.

[0023] Soft magnetic alloys can be plates, strips, bars, rings, or other structural components to be welded. Pretreatment of the soft magnetic alloy removes contaminants and oxide layers from the surface of the areas to be welded, improving the weld joint's quality and stability. Specifically, the soft magnetic alloy can be subjected to machining, degreasing, cleaning, pickling, rinsing, and drying in sequence. Machining forms bevels or butt joints that meet welding requirements; degreasing removes oil and machining residues from the workpiece surface; cleaning can be performed using alcohol, acetone, or other organic solvents via ultrasonic cleaning; pickling removes the surface oxide film; rinsing uses deionized water; and drying can be done using hot air or vacuum drying to prevent residual moisture on the workpiece surface from affecting weld quality. After pretreatment, the areas to be welded are inspected to ensure that the welding area is free of obvious oxidation, oil, rust, and other impurities.

[0024] The pretreated soft magnetic alloy is clamped and fixed in the welding chamber, and electron beam welding is performed under preset first conditions to obtain a first welding alloy. The welding chamber can be a high-vacuum electron beam welding chamber. Before welding, the welding chamber is first evacuated to achieve a preset vacuum level, thereby reducing the adverse effects of gases such as oxygen and nitrogen on the weld structure and magnetic properties during welding. During welding, the electron beam welding parameters are coordinated and adjusted according to the workpiece thickness, material type, and weld structure to achieve a stable weld penetration and continuous forming. In this embodiment, the preset first conditions include: vacuum to 3×10 -3 Pa ~ 7×10 -3 Pa, 3×10 -3 Pa, 4×10 -3 Pa, 5×10 -3 Pa, 6×10 -3 Pa, 7×10 -3 Pa, etc., can also be any value between the above values. 5 × 10⁻⁶ can be used. -3A vacuum environment of approximately Pa effectively reduces contamination of the molten pool by residual gases such as oxygen, water vapor, and nitrogen, inhibiting weld oxidation and inclusion formation, reducing the probability of porosity, and minimizing oxidation loss of active elements in high-permeability soft magnetic alloys. This ensures high purity and good magnetic properties in the welded joint. The accelerating voltage is 80kV~90kV, specifically 80kV, 82kV, 84kV, 85kV, 86kV, 88kV, 90kV, or any value within this range. A higher accelerating voltage increases the kinetic energy of the electron beam, giving it stronger penetration capabilities, resulting in a weld with a large depth-to-width ratio and achieving full penetration in a single pass. When the accelerating voltage is below 80kV, the electron beam penetration is insufficient, easily leading to incomplete penetration or insufficient weld penetration. When the accelerating voltage is above 90kV, the electron beam energy is too concentrated, easily causing weld collapse, burn-through, or increased spatter. The electron beam current is 20mA~30mA, specifically 20mA, 22mA, 24mA, 25mA, 26mA, 28mA, 30mA, etc., or any value within the above range. The electron beam current determines the electron beam output power per unit time. When the electron beam current is too small, the weld penetration is insufficient, easily leading to defects such as incomplete fusion. When the electron beam current is too large, the molten pool size increases, the heat-affected zone of the weld expands significantly, and crystal... Grain coarsening is prone to occur, which is detrimental to the recovery of the magnetic properties of the weld joint. The welding speed is 150cm / min~200cm / min, specifically 150cm / min, 160cm / min, 170cm / min, 175cm / min, 180cm / min, 190cm / min, 200cm / min, etc., or any value within the above range. When the welding speed is too low, the heat received per unit length of weld increases, the heat-affected zone expands, and the grains in the weld and heat-affected zone tend to grow, increasing the residual stress in the weld. When the welding speed is too high, the heat input per unit length is insufficient, which easily leads to welding defects such as incomplete penetration and lack of fusion. In this embodiment, low heat input can be achieved by reducing the accelerating voltage, electron beam current, or increasing the welding speed. Low heat input can reduce the growth of grain size at the weld, avoid local grain coarsening due to local overheating, and prevent local segregation of Si and P elements. It can also prevent deformation of the alloy due to excessive local heat input, which would lead to deviations in precision. Annealing is performed after welding cooling.

[0025] According to the target magnetic properties, the first welding alloy is annealed to obtain the second welding alloy. Due to the rigid clamping of the welding machine fixture and the thermal stress introduced during welding, the grain size difference between the weld, the surrounding area, and the matrix is ​​large, and the stress level difference is huge, resulting in the deterioration of the magnetic properties of the welded iron-nickel parts, which cannot meet the magnetic property requirements of industrial applications. Annealing is used to eliminate the welding residual stress formed during electron beam welding and promote the homogenization of the microstructure of the weld and heat-affected zone. In this embodiment, according to the target magnetic properties, the first welding alloy is annealed to obtain the second welding alloy, including: If the target magnetic properties meet the first magnetic property requirement, the first welding alloy is annealed according to the preset second conditions to obtain the second welding alloy. If the target magnetic properties meet the first magnetic property requirement, the weldment shall have sufficient finishing allowance on one side before welding, which can be 2mm. The first magnetic property requirement includes: μi≥3.1mH / m; maximum permeability μm≥31.3mH / m; coercivity Hc≤14.4A / m; magnetic induction intensity B (8000~40000)≥1.5T at room temperature. The preset second conditions include: heating to the first temperature in the furnace and holding for a first time, then cooling in the furnace to avoid excessively rapid cooling and secondary introduction of thermal stress. The initial temperature is 400℃~500℃, specifically 400℃, 410℃, 420℃, 430℃, 440℃, 450℃, 460℃, 470℃, 480℃, 490℃, 500℃, etc., or any value within the above range. The holding time is 4h~6h, specifically 4h, 4.5h, 5h, 5.5h, 6h, etc., or any value within the above range. Because machining allowance is left during welding, annealing can be performed under normal atmospheric conditions. The machining allowance is used for subsequent grinding. This ensures the stability of the weld joint structure while fully eliminating residual welding stress.

[0026] If the target magnetic properties meet the second magnetic property requirement, the first welding alloy is annealed according to a preset third condition to obtain the second welding alloy. The second magnetic property requirement is higher than the first magnetic property requirement; that is, the weld joint must have higher initial permeability, maximum permeability, lower coercivity, and lower iron loss. This second magnetic property requirement is applicable to applications requiring high-precision magnetic shielding devices, aerospace magnetic sensitive elements, precision current transformers, fluxgate sensors, and high-sensitivity electromagnetic detection devices, where a high degree of magnetic property recovery is required.

[0027] The preset third condition includes: holding at a first vacuum level and a second temperature for a second time, then cooling with the furnace to a third temperature and subsequently cooling to room temperature at a preset cooling rate. The first vacuum level is less than or equal to 10. -3 Pa, specifically 1×10 -3 Pa, 8×10-4 Pa, 5×10 -4 Pa, 3×10 -4 Pa, 1×10 -4 Pa, etc., or any value within the above range, a higher vacuum degree can effectively reduce the contamination of the material surface by oxygen, water vapor and other impurity gases during the annealing process, avoid weld oxidation and impurity segregation, and improve the purity of the weld joint. The second temperature is 800℃~1000℃, specifically 800℃, 820℃, 850℃, 880℃, 900℃, 920℃, 950℃, 980℃, 1000℃, etc., or any value within the above range. During the heating process, a continuous heating method or a staged heating method can be used to reduce the temperature difference between the inside and outside of the workpiece and avoid generating new thermal stress. The second time is 4h~6h, specifically 4h, 4.5h, 5h, 5.5h, 6h, etc., or any value within the above range. During the heat preservation process, sufficient recrystallization, grain homogenization and stress release occur in the weld zone and heat-affected zone, the internal dislocation density of the material is significantly reduced, and the structural defects formed during the welding process are effectively eliminated. The third temperature is 500℃~600℃, specifically 500℃, 520℃, 540℃, 550℃, 560℃, 580℃, 600℃, etc., or any value within the above range. The preset cooling rate is 180℃ / h~220℃ / h, specifically 180℃ / h, 190℃ / h, 200℃ / h, 210℃ / h, or 220℃ / h, etc., or any value within the above range. Since the cooling process involves passing through the disordered-ordered phase transformation region of the iron-nickel alloy, it is necessary to rapidly pass through the 500-600℃ region during the cooling process. Therefore, after heating and holding, this annealing process is cooled at a preset cooling rate of 180℃ / h~220℃ / h to shorten the residence time of the material within the disordered-ordered phase transformation temperature range and suppress the formation of long-range ordered phases.

[0028] The second welding alloy is heat-treated to obtain a soft magnetic alloy product. The heat treatment aims to eliminate residual stress generated during electron beam welding, restore the microstructure and magnetic properties of the welded area, and obtain the soft magnetic alloy product. The heat treatment includes placing the second welding alloy in a hydrogen furnace with an ambient dew point less than -60°C (where the ambient dew point represents the water vapor content in the hydrogen gas). A lower dew point effectively reduces the oxygen partial pressure inside the furnace, preventing oxidation of the alloy under high-temperature conditions, and also facilitates the reduction of residual oxides on the surface, improving the cleanliness of the weld area. Alternatively, the alloy can be placed in a vacuum furnace with a vacuum level less than or equal to a second vacuum level of less than or equal to 10°C. -3 Pa; specifically, it can be 1×10 -3 Pa, 8×10 -4 Pa, 5×10 -4 Pa, 3×10-4 Pa, 1×10 -4 Pa, etc., can also be any value within the above range. A high vacuum environment can reduce the contamination of the alloy surface by impurity gases such as oxygen, nitrogen, and water vapor, and avoid element oxidation.

[0029] The temperature is raised to the fourth temperature within a third time period and held for a fourth time; the third time period is 2 hours, and the fourth temperature is 1000±20℃, specifically 980℃, 985℃, 990℃, 995℃, 1000℃, 1005℃, 1010℃, 1015℃ or 1020℃, etc.; the fourth time period is 40~60 minutes, specifically 40 minutes, 45 minutes, 50 minutes, 55 minutes or 60 minutes, etc., to achieve uniform heating of the welded joint, so that the temperature of the weld area and the heat-affected zone is evenly distributed, and the recovery of magnetism is promoted.

[0030] The temperature is raised to a fifth temperature within a fifth time period and held for a sixth time period. The fifth time period is 30 minutes, and the fifth temperature is 1160±20℃, which can be 1140℃, 1145℃, 1150℃, 1155℃, 1160℃, 1165℃, 1170℃, 1175℃, or 1180℃, etc. The sixth time period is 40~60 minutes, which can be 40 minutes, 45 minutes, 50 minutes, 55 minutes, or 60 minutes, etc. Under high temperature conditions, the columnar crystal, dendritic structure and element segregation formed in the weld zone are fully improved, and sufficient diffusion occurs between the weld and the base material, promoting grain reformation and tending to be uniform. At the same time, a large number of dislocations and lattice distortions formed by welding thermal cycling are eliminated, so that the weld structure gradually recovers to a state close to the base material and restores magnetism.

[0031] The furnace is cooled to a sixth temperature, and then held for a seventh time. The sixth temperature is 800~900℃, specifically 800℃, 820℃, 840℃, 850℃, 860℃, 880℃, or 900℃, etc.; the seventh time is 60~90min, specifically 60min, 65min, 70min, 75min, 80min, 85min, or 90min, etc. The holding stage further promotes the release of residual welding stress, gradually stabilizes the magnetic domain structure inside the grains, reduces stress concentration near grain boundaries, avoids new thermal stress caused by rapid cooling, helps reduce coercivity, improves magnetic permeability, and makes the magnetic properties of the weld zone and the base metal zone tend to be consistent.

[0032] The furnace is cooled to a seventh temperature, which is 600℃. Once the furnace temperature reaches 600℃, furnace cooling is stopped, and high-purity nitrogen is used for cooling. The nitrogen cooling rate is no less than 200℃ / h, specifically 200℃ / h, 220℃ / h, 250℃ / h, 300℃ / h, 350℃ / h, or 400℃ / h, until it cools to room temperature. This cooling method can shorten the time the material spends in the medium-high temperature range, prevent abnormal grain growth, maintain the uniform structure and magnetism after recrystallization, and reduce high-temperature oxidation and dimensional deformation.

[0033] Iron-nickel based high-permeability soft magnetic alloys, with Ni content of 43.5%–46.5% and Ce content of 0.1%–0.2%, are prone to microstructure inhomogeneity, increased residual stress, and decreased magnetic properties in the weld area during welding. This embodiment effectively suppresses grain coarsening and elemental segregation in the weld and heat-affected zone by controlling the electron beam welding heat input, reducing welding residual stress and welding deformation of thin-walled parts, and improving welding quality and dimensional accuracy. Corresponding annealing processes are adopted according to different magnetic property requirements to promote the homogenization of the weld joint microstructure. Post-weld magnetic properties are restored through heat treatment, increasing initial and maximum permeability and reducing coercivity. This achieves synergistic optimization of welding formation, dimensional accuracy, and magnetic property recovery, making it suitable for manufacturing complex structural parts made of high-permeability soft magnetic alloys.

[0034] Example 1 The soft magnetic alloy contains 0.05% C, 0.80% Mn, 0.05% Si, 0.030% P, 0.010% S, 0.30% Cr, 0.30% Mo, 0.30% Cu, 0.50% Co, 45% Ni, 0.15% Ce, with the balance being Fe and unavoidable impurities.

[0035] The soft magnetic alloy is pretreated to obtain a pretreated soft magnetic alloy, which is an oil-free and rust-free strip. The pretreated soft magnetic alloy is clamped and fixed in the welding chamber, and electron beam welding is performed under preset first conditions. The heat input of the electron beam welding is within a preset heat input threshold range to obtain a first weld alloy. Vacuum is then applied to 5×10⁻⁶ mm. -3 Pa, accelerating voltage 85KV, electron beam current 25mA, welding speed 180cm / min.

[0036] When the target magnetic properties meet the first magnetic property requirement, the first welding alloy is annealed according to the preset second conditions to obtain the second welding alloy. The first magnetic property requirement includes: μi≥3.1mH / m; maximum permeability μm≥31.3mH / m; coercivity Hc≤14.4A / m; magnetic induction intensity B (8000~40000)≥1.5T at room temperature; the furnace is heated to the first temperature and held for the first time, and then cooled with the furnace. The first temperature is 450℃ and held for 5h.

[0037] The second welding alloy is heat-treated to obtain the finished soft magnetic alloy. The heat treatment includes: The second welding alloy was placed in a hydrogen furnace with an ambient dew point less than -60°C. The temperature was raised to a fourth temperature within a third time period and held for a fourth time. The third time was 2 hours, the fourth temperature was 1000°C, and the fourth time was 50 minutes. The temperature was then raised to a fifth temperature within a fifth time period and held for a sixth time. The fifth time was 30 minutes, the fifth temperature was 1160°C, and the sixth time was 50 minutes. The furnace was then cooled to a sixth temperature and held for a seventh time. The sixth temperature was 850°C, the seventh time was 60-90 minutes, and the furnace was then cooled to a seventh temperature using nitrogen at a cooling rate of 200°C / h. The seventh temperature was 600°C.

[0038] Example 2 The soft magnetic alloy contains 0.05% C, 0.70% Mn, 0.05% Si, 0.030% P, 0.010% S, 0.20% Cr, 0.20% Mo, 0.20% Cu, 0.50% Co, 46% Ni, 0.15% Ce, with the balance being Fe and unavoidable impurities.

[0039] The soft magnetic alloy is pretreated to obtain a pretreated soft magnetic alloy, which is an oil-free and rust-free strip. The pretreated soft magnetic alloy is clamped and fixed in a welding chamber, and electron beam welding is performed under preset first conditions. The heat input of the electron beam welding is within a preset heat input threshold range to obtain a first weld alloy. The vacuum is then reduced to 4 × 10⁻⁶. -3 Pa, accelerating voltage 87KV, electron beam current 23mA, welding speed 160cm / min.

[0040] When the target magnetic properties meet the first magnetic property requirement, the first welding alloy is annealed according to the preset second conditions to obtain the second welding alloy. The first magnetic property requirement includes: μi≥3.1mH / m; maximum permeability μm≥31.3mH / m; coercivity Hc≤14.4A / m; magnetic induction intensity B (8000~40000)≥1.5T at room temperature; the furnace is heated to the first temperature and held for the first time, and then cooled in the furnace. The first temperature is 420℃ and the holding time is 4.5h.

[0041] The second welding alloy is heat-treated to obtain a soft magnetic alloy product. The heat treatment includes: placing the second welding alloy in a vacuum furnace with a vacuum degree less than or equal to a second vacuum degree; the second vacuum degree is equal to 10... -3 Pa, in the third time period, the temperature is raised to the fourth temperature and held for the fourth time; the third time period is 2 hours, the fourth temperature is 990℃, and the fourth time period is 40 minutes; in the fifth time period, the temperature is raised to the fifth temperature and held for the sixth time; the fifth time period is 30 minutes, the fifth temperature is 1140℃, and the sixth time period is 60 minutes; the temperature is lowered to the sixth temperature in the furnace and held for the seventh time; the sixth temperature is 900℃, the seventh time period is 90 minutes, the temperature is lowered to the seventh temperature in the furnace, and the furnace is cooled using nitrogen at a cooling rate of 220℃ / h, and the seventh temperature is 600℃.

[0042] Example 3 The soft magnetic alloy contains 0.05% C, 0.60% Mn, 0.05% Si, 0.030% P, 0.010% S, 0.30% Cr, 0.30% Mo, 0.30% Cu, 0.50% Co, 43.5% Ni, 0.1% Ce, with the balance being Fe and unavoidable impurities.

[0043] The soft magnetic alloy is pretreated to obtain a pretreated soft magnetic alloy, which is an oil-free and rust-free strip. The pretreated soft magnetic alloy is clamped and fixed in a welding chamber, and electron beam welding is performed under preset first conditions. The heat input of the electron beam welding is within a preset heat input threshold range to obtain a first weld alloy. The vacuum is then reduced to 3 × 10⁻⁶. -3 Pa, accelerating voltage of 80KV, electron beam current of 20mA, welding speed of 150cm / min.

[0044] When the target magnetic properties meet the first magnetic property requirement, the first welding alloy is annealed according to the preset second conditions to obtain the second welding alloy. The first magnetic property requirement includes: μi≥3.1mH / m; maximum permeability μm≥31.3mH / m; coercivity Hc≤14.4A / m; magnetic induction intensity B (8000~40000)≥1.5T at room temperature; the furnace is heated to the first temperature and held for the first time, and then cooled with the furnace. The first temperature is 400℃ and held for 4h.

[0045] The second welding alloy is heat-treated to obtain a soft magnetic alloy product. The heat treatment includes: placing the second welding alloy in a hydrogen furnace with an ambient dew point of less than -60°C; heating to a fourth temperature within a third time period and holding at that temperature for a fourth time period; the third time period is 2 hours, the fourth temperature is 1020°C, and the fourth time period is 40 minutes; heating to a fifth temperature within a fifth time period and holding at that temperature for a sixth time period; the fifth time period is 30 minutes, the fifth temperature is 1140°C, and the sixth time period is 40 minutes; cooling to a sixth temperature in the furnace and holding at that temperature for a seventh time period; the sixth temperature is 800°C, the seventh time period is 60 minutes, cooling to a seventh temperature in the furnace, and then cooling with nitrogen at a cooling rate of 200°C / h until the seventh temperature reaches 600°C.

[0046] Example 4 The soft magnetic alloy contains 0.05% C, 0.80% Mn, 0.05% Si, 0.030% P, 0.010% S, 0.30% Cr, 0.30% Mo, 0.30% Cu, 0.50% Co, 46.5% Ni, 0.2% Ce, with the balance being Fe and unavoidable impurities.

[0047] The soft magnetic alloy is pretreated to obtain a pretreated soft magnetic alloy, which is an oil-free and rust-free strip. The pretreated soft magnetic alloy is clamped and fixed in a welding chamber, and electron beam welding is performed under preset first conditions. The heat input of the electron beam welding is within a preset heat input threshold range to obtain a first weld alloy. The vacuum is then reduced to 7 × 10⁻⁶. -3 Pa, accelerating voltage of 90KV, electron beam current of 30mA, welding speed of 200cm / min.

[0048] When the target magnetic properties meet the first magnetic property requirement, the first welding alloy is annealed according to the preset second conditions to obtain the second welding alloy. The first magnetic property requirement includes: μi≥3.1mH / m; maximum permeability μm≥31.3mH / m; coercivity Hc≤14.4A / m; magnetic induction intensity B (8000~40000)≥1.5T at room temperature; the furnace is heated to the first temperature and held for the first time, and then cooled with the furnace. The first temperature is 500℃ and the holding time is 6h.

[0049] The second welding alloy is heat-treated to obtain a soft magnetic alloy product. The heat treatment includes: placing the second welding alloy in a vacuum furnace with a vacuum degree less than or equal to a second vacuum degree; the second vacuum degree is equal to 10... -3Pa, in the third time period, the temperature is raised to the fourth temperature and held for the fourth time; the third time period is 2 hours, the fourth temperature is 980℃, and the fourth time period is 50 minutes; in the fifth time period, the temperature is raised to the fifth temperature and held for the sixth time; the fifth time period is 30 minutes, the fifth temperature is 1180℃, and the sixth time period is 50 minutes; the temperature is lowered to the sixth temperature in the furnace and held for the seventh time; the sixth temperature is 900℃, the seventh time period is 90 minutes, the temperature is lowered to the seventh temperature in the furnace, and cooled with nitrogen at a cooling rate of 200℃ / h, the seventh temperature is 600℃.

[0050] Example 5 The soft magnetic alloy contains 0.05% C, 0.80% Mn, 0.05% Si, 0.030% P, 0.010% S, 0.30% Cr, 0.30% Mo, 0.30% Cu, 0.50% Co, 45% Ni, 0.15% Ce, with the balance being Fe and unavoidable impurities.

[0051] The soft magnetic alloy is pretreated to obtain a pretreated soft magnetic alloy, which is an oil-free and rust-free strip. The pretreated soft magnetic alloy is clamped and fixed in the welding chamber, and electron beam welding is performed under preset first conditions. The heat input of the electron beam welding is within a preset heat input threshold range to obtain a first weld alloy. Vacuum is then applied to 4×10⁻⁶. -3 Pa, accelerating voltage of 82KV, electron beam current of 22mA, welding speed of 160cm / min.

[0052] The target magnetic properties are the second magnetic property requirements, which are higher than the first magnetic property requirements. The first welding alloy is annealed according to a preset third condition to obtain the second welding alloy. It is held at a first vacuum level and a second temperature for a second time, then cooled in the furnace to a third temperature, and finally cooled to room temperature at a preset cooling rate. The first vacuum level is equal to 10. -3 Pa, the second temperature is 900℃, the second time is 5h, the third temperature is 550℃, and the preset cooling rate is 200℃ / h.

[0053] The second welding alloy is heat-treated to obtain a soft magnetic alloy product. The heat treatment includes: placing the second welding alloy in a hydrogen furnace with an ambient dew point less than -60°C; heating to a fourth temperature within a third time period and holding at that temperature for a fourth time period; the third time period is 2 hours, the fourth temperature is 1000°C, and the fourth time period is 50 minutes; heating to a fifth temperature within a fifth time period and holding at that temperature for a sixth time period; the fifth time period is 30 minutes, the fifth temperature is 1160°C, and the sixth time period is 50 minutes; cooling to a sixth temperature in the furnace and holding at that temperature for a seventh time period; the sixth temperature is 900°C, the seventh time period is 90 minutes, cooling to a seventh temperature in the furnace, and then cooling with nitrogen at a cooling rate of 200°C / h. The seventh temperature is 600°C.

[0054] Example 6 The soft magnetic alloy contains 0.05% C, 0.70% Mn, 0.05% Si, 0.030% P, 0.010% S, 0.20% Cr, 0.20% Mo, 0.20% Cu, 0.50% Co, 46% Ni, 0.15% Ce, with the balance being Fe and unavoidable impurities.

[0055] The soft magnetic alloy is pretreated to obtain a pretreated soft magnetic alloy, which is an oil-free and rust-free strip. The pretreated soft magnetic alloy is clamped and fixed in the welding chamber, and electron beam welding is performed under preset first conditions. The heat input of electron beam welding is within a preset heat input threshold range to obtain a first weld alloy. Vacuum is then applied to 6×10⁻⁶. -3 Pa, accelerating voltage 87KV, electron beam current 27mA, welding speed 170cm / min.

[0056] The target magnetic properties are the second magnetic property requirements, which are higher than the first magnetic property requirements. The first welding alloy is annealed according to a preset third condition to obtain the second welding alloy. It is held at a first vacuum level and a second temperature for a second time, then cooled in the furnace to a third temperature, and finally cooled to room temperature at a preset cooling rate. The first vacuum level is less than 10... -3 Pa, the second temperature is 850℃, the second time is 4.5h, the third temperature is 580℃, and the preset cooling rate is 190℃ / h.

[0057] The second welding alloy is heat-treated to obtain a soft magnetic alloy product. The heat treatment includes placing the second welding alloy in a vacuum furnace with a vacuum level less than or equal to a second vacuum level of less than or equal to 10... -3Pa, in the third time period, the temperature is raised to the fourth temperature and held for the fourth time; the third time period is 2 hours, the fourth temperature is 990℃, and the fourth time period is 55 minutes; in the fifth time period, the temperature is raised to the fifth temperature and held for the sixth time; the fifth time period is 30 minutes, the fifth temperature is 1150℃, and the sixth time period is 55 minutes; the temperature is lowered to the sixth temperature in the furnace and held for the seventh time; the sixth temperature is 850℃, the seventh time period is 80 minutes, the temperature is lowered to the seventh temperature in the furnace, and the furnace is cooled using nitrogen at a cooling rate of 230℃ / h, and the seventh temperature is 600℃.

[0058] Example 7 The soft magnetic alloy contains 0.05% C, 0.60% Mn, 0.05% Si, 0.030% P, 0.010% S, 0.30% Cr, 0.30% Mo, 0.30% Cu, 0.50% Co, 43.5% Ni, 0.1% Ce, with the balance being Fe and unavoidable impurities.

[0059] The soft magnetic alloy is pretreated to obtain a pretreated soft magnetic alloy, which is an oil-free and rust-free strip. The pretreated soft magnetic alloy is clamped and fixed in a welding chamber, and electron beam welding is performed under preset first conditions. The heat input of the electron beam welding is within a preset heat input threshold range to obtain a first weld alloy. The vacuum is then reduced to 3 × 10⁻⁶. -3 Pa, accelerating voltage of 80KV, electron beam current of 20mA, welding speed of 150cm / min.

[0060] The target magnetic properties are the second magnetic property requirements, which are higher than the first magnetic property requirements. The first welding alloy is annealed according to a preset third condition to obtain the second welding alloy. It is held at a first vacuum level and a second temperature for a second time, then cooled in the furnace to a third temperature, and finally cooled to room temperature at a preset cooling rate. The first vacuum level is less than or equal to 10. -3 Pa, the second temperature is 800℃, the second time is 4h, the third temperature is 500℃, and the preset cooling rate is 180℃ / h.

[0061] The second welding alloy is heat-treated to obtain a soft magnetic alloy product. The heat treatment includes: placing the second welding alloy in a hydrogen furnace with an ambient dew point of less than -60°C; heating to a fourth temperature within a third time period and holding at that temperature for a fourth time period; the third time period is 2 hours, the fourth temperature is 1000°C, and the fourth time period is 40 minutes; heating to a fifth temperature within a fifth time period and holding at that temperature for a sixth time period; the fifth time period is 30 minutes, the fifth temperature is 1160°C, and the sixth time period is 40 minutes; cooling to a sixth temperature in the furnace and holding at that temperature for a seventh time period; the sixth temperature is 900°C, the seventh time period is 90 minutes, cooling to a seventh temperature in the furnace, and then cooling with nitrogen at a cooling rate of 200°C / h until the seventh temperature reaches 600°C.

[0062] Example 8 The soft magnetic alloy contains 0.05% C, 0.80% Mn, 0.05% Si, 0.030% P, 0.010% S, 0.30% Cr, 0.30% Mo, 0.30% Cu, 0.50% Co, 46.5% Ni, 0.2% Ce, with the balance being Fe and unavoidable impurities.

[0063] The soft magnetic alloy is pretreated to obtain a pretreated soft magnetic alloy, which is an oil-free and rust-free strip. The pretreated soft magnetic alloy is clamped and fixed in the welding chamber, and electron beam welding is performed under preset first conditions. The heat input of the electron beam welding is within a preset heat input threshold range to obtain a first weld alloy. Vacuum is then applied to 7×10⁻⁶. -3 Pa, accelerating voltage of 90KV, electron beam current of 30mA, welding speed of 200cm / min.

[0064] The target magnetic properties are the second magnetic property requirements, which are higher than the first magnetic property requirements. The first welding alloy is annealed according to a preset third condition to obtain the second welding alloy. It is held at a first vacuum level and a second temperature for a second time, then cooled in the furnace to a third temperature, and finally cooled to room temperature at a preset cooling rate. The first vacuum level is less than or equal to 10. -3 Pa, the second temperature is 1000℃, the second time is 6h, the third temperature is 600℃, and the preset cooling rate is 220℃ / h.

[0065] The second welding alloy is heat-treated to obtain a soft magnetic alloy product. The heat treatment includes: placing the second welding alloy in a vacuum furnace with a vacuum degree less than or equal to a second vacuum degree; the second vacuum degree is less than or equal to 10... -3Pa; The temperature is raised to the fourth temperature within the third time period and held for the fourth time period; the third time period is 2 hours, the fourth temperature is 1020℃, and the fourth time period is 60 minutes; The temperature is raised to the fifth temperature within the fifth time period and held for the sixth time period; the fifth time period is 30 minutes, the fifth temperature is 1180℃, and the sixth time period is 40 minutes; The temperature is lowered to the sixth temperature in the furnace and held for the seventh time period; the sixth temperature is 800℃, the seventh time period is 60 minutes, and the temperature is lowered to the seventh temperature in the furnace. The temperature is then cooled using nitrogen at a cooling rate of 200℃ / h, and the seventh temperature is 600℃.

[0066] Comparative Example 1 Conventional welding.

[0067] Comparative Example 2 No annealing is performed; otherwise, it is the same as in Example 1.

[0068] Performance tests were conducted on Examples 1-8 and Comparative Examples 1-2 using the national standard method for measuring the DC magnetic properties of soft magnetic materials.

[0069] Table 1 shows the performance test results of Examples 1-8 and Comparative Examples 1-2. Table 1 Performance test results of Examples 1-8 and Comparative Examples 1-2 In summary, the performance test results of Examples 1-8 are all better than those of the comparative examples, indicating that the welding method of this embodiment can effectively reduce the adverse effects of welding heat input on alloy microstructure and magnetic properties, and improve residual stress and magnetic domain structure in the welding area.

[0070] It should be understood that the specific embodiments described above are merely illustrative or explanatory of the principles of the invention and do not constitute a limitation thereof. Therefore, any modifications, equivalent substitutions, improvements, etc., made without departing from the spirit and scope of the invention should be included within the protection scope of the invention. Furthermore, the appended claims are intended to cover all variations and modifications falling within the scope and boundaries of the appended claims, or equivalent forms of such scope and boundaries.

[0071] The present invention has been described above with reference to embodiments thereof. However, these embodiments are merely illustrative and not intended to limit the scope of the invention. The scope of the invention is defined by the appended claims and their equivalents. Various substitutions and modifications can be made by those skilled in the art without departing from the scope of the invention, and all such substitutions and modifications should fall within the scope of the invention.

[0072] Although embodiments of the present invention have been described in detail, it should be understood that various changes, substitutions, and modifications can be made to the embodiments of the present invention without departing from the spirit and scope of the invention.

[0073] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.

Claims

1. A method for welding and forming a high-permeability soft magnetic alloy, characterized in that, include: The soft magnetic alloy is clamped and fixed in the welding chamber, and electron beam welding is performed under preset first conditions and then cooled to obtain the first welding alloy. According to the target magnetic properties, the first welding alloy is annealed to obtain a second welding alloy, comprising: If the target magnetic properties are the first magnetic property requirements, the first welding alloy is annealed according to the preset second conditions to obtain the second welding alloy. If the target magnetic properties are the second magnetic property requirements, the first welding alloy is annealed according to the preset third conditions to obtain the second welding alloy. The second welding alloy is heat-treated to obtain a soft magnetic alloy product.

2. The method for welding and forming high-permeability soft magnetic alloys according to claim 1, characterized in that, The soft magnetic alloy comprises: C, Mn, Si, P, S, Cr, Mo, Cu, Co, Ni, Ce, Fe and unavoidable impurities, in mass percentage as follows: C≤0.05%, Mn≤0.80%, Si≤0.05%, P≤0.030%, S≤0.010%, Cr≤0.30%, Mo≤0.30%, Cu≤0.30%, Co≤0.50%, Ni is 43.5%~46.5%, Ce is 0.1%~0.2%, and the balance is Fe and unavoidable impurities.

3. The method for welding and forming high-permeability soft magnetic alloys according to claim 1, characterized in that, The preset first condition includes: vacuum to 3×10 -3 Pa ~ 7×10 -3 Pa, accelerating voltage of 80KV~90KV, electron beam current of 20mA~30mA, welding speed of 150cm / min~200cm / min.

4. The method for welding and forming high-permeability soft magnetic alloys according to claim 1, characterized in that, Also includes: The soft magnetic alloy is pretreated before welding to obtain the pretreated soft magnetic alloy.

5. The method for welding and forming high-permeability soft magnetic alloys according to claim 4, characterized in that, The first magnetic performance requirements include: μi≥3.1mH / m; maximum permeability μm≥31.3mH / m; coercivity Hc≤14.4A / m; and magnetic flux density B (8000~40000)≥1.5T at room temperature. The preset second condition includes: heating the furnace to the first temperature and holding it at that temperature for a first time, then cooling the furnace.

6. The method for welding and forming high-permeability soft magnetic alloys according to claim 5, characterized in that, The first temperature is 400℃~500℃, and the temperature is maintained for 4h~6h.

7. The method for welding and forming high-permeability soft magnetic alloys according to claim 5, characterized in that, The second magnetic performance requirement is higher than the first magnetic performance requirement; The preset third condition includes: After being held at a first vacuum level and a second temperature for a second time, the furnace is cooled to a third temperature and then cooled to room temperature at a preset cooling rate.

8. The method for welding and forming high-permeability soft magnetic alloys according to claim 8, characterized in that, The first vacuum degree is less than or equal to 10 -3 Pa, the second temperature is 800℃~1000℃, the second time is 4h~6h, the third temperature is 500℃~600℃, and the preset cooling rate is 180℃ / h~220℃ / h.

9. The method for welding and forming high-permeability soft magnetic alloys according to claim 1, characterized in that, The heat treatment includes placing the second welding alloy in a hydrogen furnace with an ambient dew point of less than -60°C or a vacuum furnace with a vacuum degree of less than or equal to the second vacuum degree. The temperature is raised to the fourth temperature within the third time period, and then maintained at that temperature for the fourth time. The temperature is raised to the fifth temperature within the fifth time period, and then maintained at that temperature for the sixth time. The furnace temperature is lowered to the sixth temperature, and then held for the seventh time. The furnace is cooled to the seventh temperature, and nitrogen is used for cooling at a rate of ≥200℃ / h.

10. The method for welding and forming high-permeability soft magnetic alloys according to claim 9, characterized in that, The second vacuum degree is less than or equal to 10. -3 Pa, the third time is 2h, the fourth temperature is 1000±20℃, the fourth time is 40~60min; the fifth time is 30min, the fifth temperature is 1160±20℃, the sixth time is 40~60min; the sixth temperature is 800~900℃, the seventh time is 60~90min, the seventh temperature is 600℃.