A method for preparing an exploded composite plate based on an SA542TypeDCL4a substrate
By combining calcined corundum abrasive belt polishing with explosive welding of specific composite explosives on the SA542TypeDCL4a substrate, the welding problem of SA542TypeDCL4a substrate composite plate was solved, realizing efficient and low-cost composite plate production, improving the cleanliness and strength of the bonding interface, and ensuring the mechanical properties and resistance to intergranular corrosion of the composite plate.
Patent Information
- Application Number
- CN202611342957.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-17
AI Technical Summary
In the prior art, the exploded composite plate based on the SA542TypeDCL4a substrate has problems such as a small weldable window, uneven bonding strength and precipitation of embrittled phases at the interface during the welding process. In addition, it is sensitive to heat treatment and it is difficult to obtain a reliable composite interface bond without damaging the substrate performance.
The substrate and cover plate are polished using calcined corundum abrasive belts. Explosive welding is performed using a composite explosive consisting of powdered emulsion explosives, quartz sand particles, and wood flour. Specific heat treatments, including segmented cooling and heat preservation, are then applied to ensure the cleanliness and strength of the interface bonding.
This technology enables efficient production of large-area composite panels, reduces production cycles and costs, improves the cleanliness and strength of the bonding interface, and ensures the mechanical properties and resistance to intergranular corrosion of the composite panels.
Smart Images

Figure CN123103151A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of composite plate technology, and in particular to a method for preparing an exploded composite plate based on an SA542TypeDCL4a substrate. Background Technology
[0002] SA542TypeDCL4a steel plate is a chromium-molybdenum-vanadium (Cr-Mo-V) alloy steel under the ASME standard, mainly used in the manufacture of pressure vessels for high-temperature, high-pressure hydrogen-containing environments. Compared with the 2.25Cr-1Mo steel commonly used in the petrochemical industry, this material, through the addition of vanadium and strict quenching and tempering heat treatment, can obtain a fine tempered bainitic structure, exhibiting superior overall performance in terms of resistance to hydrogen corrosion, temper embrittlement, and hydrogen-induced delamination. In the manufacturing of core equipment such as hydrogenation reactors and hot high-pressure separators, domestic enterprises currently mainly use plate welding, forging welding, or corrosion-resistant surfacing welding. Existing processes have high requirements for equipment manufacturing capabilities and welding technology, and the equipment manufacturing cycle is long. The use of composite plate structures, i.e., using chromium-molybdenum steel as the base material and composited with a layer of stainless steel or nickel-based alloy corrosion-resistant layer on the hydrogen-containing side, has been applied in similar equipment both domestically and internationally. However, there are currently no practical application cases in China of explosion-proof composite plates produced based on SA542TypeDCL4a steel plate as the base material.
[0003] Explosive welding is one of the main processes for achieving large-area bonding of dissimilar metals. Its principle involves using the impact energy released instantaneously by an explosive detonation to propel the cladding metal towards the substrate at high speed, forming a solid metallurgical bond at the interface. This process has been industrially applied in China for decades, with composite plates combining stainless steel / steel and titanium / steel already in mass production. However, when SA542TypeDCL4a is used as the substrate, the explosive bonding process lacks a research foundation, and existing explosive welding technologies still face some practical problems. For example, the weldable window for explosive bonding of special materials is relatively small, and the precipitation of embrittled phases at the interface leads to uneven bonding strength. Furthermore, these materials are quite sensitive to heat treatment regimes. How to obtain reliable composite interface bonding without damaging the original properties of the substrate, while effectively eliminating residual deformation stress, is a crucial technical problem that must be solved.
[0004] Therefore, conducting research on the preparation technology of the exploded composite plate with SA542TypeDCL4a as the substrate, clarifying its exploded composite process window and subsequent heat treatment specifications, is of practical value for promoting the application of such composite plates in the field of hydrogenation reactors. Summary of the Invention
[0005] In view of this, the present invention provides a method for preparing an exploded composite plate based on an SA542TypeDCL4a substrate, in order to solve the problem that there are no relevant reports on the existing exploded composite plates produced based on the SA542TypeDCL4a substrate, as well as the problems that exist in the exploded welding process, such as a small weldable window for the exploded composite and the easy occurrence of uneven bonding strength.
[0006] To achieve the above objectives, the present invention adopts the following technical solution: A method for preparing an exploded composite plate based on an SA542TypeDCL4a substrate includes the following steps: 1) Polish the SA542TypeDCL4a substrate and cladding using calcined corundum abrasive belt; 2) The polished SA542TypeDCL4a substrate and the cover plate are explosively welded to obtain an explosive composite plate precursor based on the SA542TypeDCL4a substrate; 3) The exploded composite plate precursor based on SA542TypeDCL4a substrate is heat-treated to obtain the exploded composite plate based on SA542TypeDCL4a substrate. The composite explosive used in the explosive welding includes powdered emulsion explosives, quartz sand particles, and wood powder. The mass ratio of the powdered emulsion explosive to quartz sand particles and wood flour is 42~58:38~50:2~8.
[0007] Preferably, the surface roughness of the SA542TypeDCL4a substrate and the cladding after polishing in step 1) is 1~1.6μm.
[0008] Preferably, the cover plate includes SS321, SS347, SS316L, 2205, 2507, N08825 or N06625.
[0009] Preferably, the explosive welding operation in step 2) is as follows: S1: The polished SA542TypeDCL4a substrate, support layer, polished cover plate and explosive frame are sequentially stacked on the detonation bed; S2: Fill the explosive box with composite explosives. After the composite explosives are filled, add powdered emulsion explosives as detonators in the explosive box. Place a detonator in the center of the detonator. S3: Control the detonator to initiate the explosion, and the explosion is completed to achieve explosive welding.
[0010] Preferably, in step S1, the support sheet layer includes a support sheet at the edge and a support sheet at the center. The support pieces at the edge are arranged linearly along the periphery of the substrate, and the distance between two adjacent support pieces is 300~500mm; The support plates in the center are arranged in a crisscross pattern, with a spacing of 300~500mm between adjacent support plates.
[0011] Preferably, in step S2, the orthographic projection of the medicine frame has the same shape as the cover plate; The filling height of the composite explosive is 38~50mm; The additional powdered emulsion explosive is 50-60 g in weight.
[0012] Preferably, the heat treatment operation in step 3) includes: First, the exploded composite board precursor based on the SA542TypeDCL4a substrate is heated to the processing temperature and kept at that temperature. After the heat preservation is completed, it is cooled in stages to complete the heat treatment.
[0013] Preferably, the heating rate is 55~90℃ / h, the processing temperature is 580~630℃, and the ratio of the holding time to the thickness of the exploded composite plate precursor based on the SA542TypeDCL4a substrate is 2~2.5min:1mm. The segmented cooling process involves first cooling the furnace to 480-520°C, and then allowing it to cool naturally in the air to room temperature.
[0014] As can be seen from the above technical solution, compared with the prior art, the present invention has the following beneficial effects: 1. The explosive welding (explosive composite method) of the present invention can achieve a maximum single composite area of up to 45m². 2 Compared with traditional corrosion-resistant surfacing welding process, the production cycle is shortened by about 70%, and welding defects and other uncontrollable quality problems caused by repeated multi-layer surfacing welding can be effectively avoided. Therefore, it has significant advantages such as excellent product quality, high production efficiency, low overall cost and short delivery cycle. 2. The present invention uses calcined corundum abrasive belts for grinding the substrate and the cover plate. The abrasive belts are prepared by high-temperature calcination process, which can improve the purity of the abrasive and optimize the grinding performance from the source, thereby obtaining a cleaner and more efficient grinding effect, improving the cleanliness of the bonding interface, and minimizing the precipitation of embrittled phases at the interface during the explosive bonding process. 3. The explosive used in this invention is different from traditional mixed explosives. It has the characteristics of good dispersion and high detonator sensitivity. At the same time, the addition of wood powder improves the detonation sensitivity of the mixed explosive. While reducing the detonation velocity to meet the requirements of explosive composite, it also makes up for the shortcomings of low detonation sensitivity and poor detonation transmission stability of the mixed explosive. This explosive composite explosive is also suitable for the production of other ultra-long, ultra-wide and large-format explosive welding composite plates. 4. The present invention also performs heat treatment after explosive welding. Heat treatment can effectively ensure the mechanical properties and resistance to intergranular corrosion of the composite plate. Attached Figure Description
[0015] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the provided drawings without creative effort.
[0016] Figure 1 This is a schematic diagram of the explosive welding installation in Embodiment 1 of the present invention; Figure 2 This is a schematic diagram of the distribution of the explosive welding support plates in Embodiment 1 of the present invention. Detailed Implementation
[0017] This invention provides a method for preparing an exploded composite plate based on an SA542TypeDCL4a substrate, comprising the following steps: 1) Polish the SA542TypeDCL4a substrate and cladding using calcined corundum abrasive belt; 2) The polished SA542TypeDCL4a substrate and the cover plate are explosively welded to obtain an explosive composite plate precursor based on the SA542TypeDCL4a substrate; 3) The exploded composite plate precursor based on the SA542TypeDCL4a substrate is heat-treated to obtain the exploded composite plate based on the SA542TypeDCL4a substrate.
[0018] In this invention, the polishing in step 1) is preferably performed by using calcined corundum abrasive belt to remove oxide scale, exposing the bonding surface with a metallic luster; the surface roughness of the SA542TypeDCL4a substrate and the cladding after polishing is independently 1~1.6μm. Specifically, it can be 1.1μm, 1.2μm, 1.3μm, 1.4μm, or 1.5μm.
[0019] In this invention, traditional abrasives (silicon carbide, zirconium corundum, brown corundum, etc.) are used for grinding the mating surfaces. However, the following problems exist: Silicon carbide abrasives, due to their high chemical reactivity, are prone to chemical reactions with the workpiece during high-speed friction and high temperatures, causing surface contamination. Zirconium corundum abrasives, with their high toughness, are prone to generating high temperatures during high-speed grinding, leading to surface burns or damage, commonly seen as blackening or bluing of alloy steel workpieces during grinding. Brown corundum abrasives contain many impurities; while effective for grinding ordinary carbon steel, they easily contaminate the grinding area when grinding alloy steel or special-purpose workpieces. This is especially true for special materials like SA542TypeDCL4a used in hydrogen sulfide environments, where surface cleanliness is paramount.
[0020] In this invention, the cover plate includes SS321, SS347, SS316L, 2205, 2507, N08825 or N06625.
[0021] In this invention, the explosive welding operation in step 2) is as follows: S1: The polished SA542TypeDCL4a substrate, support layer, polished cover plate and explosive frame are sequentially stacked on the detonation bed; S2: Fill the explosive box with composite explosives. After the composite explosives are filled, add powdered emulsion explosives as detonators in the explosive box. Place a detonator in the center of the detonator. S3: Control the detonator to initiate the explosion, and the explosion is completed to achieve explosive welding.
[0022] In this invention, in step S1, the support sheet layer includes support sheets at the edge and support sheets at the center; the support sheets at the edge are arranged linearly along the periphery of the substrate, and the distance between two adjacent support sheets is 300-500mm, specifically 320mm, 350mm, 380mm, 400mm, 420mm, 450mm, or 480mm; the support sheets at the center are arranged in a crisscross pattern, and the distance between two adjacent support sheets is 300-500mm, specifically 320mm, 350mm, 380mm, 400mm, 420mm, 450mm, or 480mm.
[0023] In this invention, in step S2, the orthographic projection of the medicine frame has the same shape as the cover plate, and the medicine frame is arranged along the edge of the cover plate.
[0024] In this invention, the filling height of the composite explosive is 38~50mm, specifically 40mm, 42mm, 44mm, 45mm, 46mm, or 48mm.
[0025] In this invention, the mass of the additional powdered emulsion explosive is 50-60g, specifically 52g, 54g, 55g, 56g, or 58g; the location where the additional powdered emulsion explosive is added is the detonation point.
[0026] In this invention, the composite explosive used in the explosive welding comprises powdered emulsion explosive, quartz sand particles, and wood flour; the mass ratio of the powdered emulsion explosive to the quartz sand particles and wood flour is 42~58:38~50:2~8, preferably 45~55:40~48:4~6, and more preferably 50:45:5; the density of the composite explosive is 0.90~0.93 g / cm³. 3 Specifically, it can be 0.91 g / cm³. 3 0.92g / cm 3 0.93g / cm 3 The detonation velocity ranges from 1930 to 2100 m / s, specifically 1950 m / s, 1980 m / s, 2000 m / s, and 2050 m / s; the saturation is between 8.7 and 9.6 mm, specifically 8.8 mm, 9 mm, 9.2 mm, 9.4 mm, and 9.5 mm.
[0027] In this invention, traditional explosive composite materials typically involve separately mixing powdered emulsion explosives with industrial salt, quartz sand, dispersants, talc, etc., and adjusting the mass ratio to obtain the required parameters such as density, detonation velocity, and saturation. This method can be applied to different material combinations. However, adjusting these parameters inevitably reduces the explosive's sensitivity and detonation propagation stability. This invention avoids this drawback by adding wood flour. Because wood flour is flammable and its particles are relatively uniform, it can be effectively and evenly distributed within the powdered emulsion explosives and quartz sand particles, acting as a sensitizer. The explosive composite materials prepared using this method are not limited to this invention; industry professionals can apply them to the production of more material combinations and larger-format explosive composite panels through adjustments to the mass ratio and details.
[0028] In this invention, the powdered emulsion explosive is a powdered emulsion explosive that meets the GB28286-2024 standard, specifically named: rock powdered emulsion explosive, and is packaged in a bag for easy preparation of explosive composite explosives.
[0029] In this invention, the heat treatment operation in step 3) includes: First, the exploded composite board precursor based on the SA542TypeDCL4a substrate is heated to the processing temperature and kept at that temperature. After the heat preservation is completed, it is cooled in stages to complete the heat treatment.
[0030] In this invention, the heating rate is 55~90℃ / h, specifically 60℃ / h, 65℃ / h, 70℃ / h, 75℃ / h, 80℃ / h, or 85℃ / h; the processing temperature is 580~630℃, specifically 590℃, 600℃, 610℃, or 620℃; the ratio of the holding time to the thickness of the exploded composite plate precursor based on the SA542TypeDCL4a substrate is 2~2.5min:1mm, preferably 2.1~2.4min:1mm, and more preferably 2.2~2.3min:1mm.
[0031] In this invention, the segmented cooling involves first cooling the furnace to 480~520℃, specifically 490℃, 500℃, and 510℃; then naturally cooling it to room temperature in the air.
[0032] In this invention, the heating stage of the heat treatment employs slow heating to ensure a uniform temperature distribution within the furnace and to achieve simultaneous temperature increases inside and outside the workpiece. The holding temperature is intentionally set to avoid the sensitization range of stainless steel (650℃ and 675℃). The cooling process adopts a two-stage strategy of "slow cooling in the furnace + air cooling." First, the workpiece is slowly cooled inside the furnace to minimize the temperature difference between the inside and outside, which helps to fully release the residual stress generated by the explosive welding. Then, after the temperature drops to around 500℃, the workpiece is removed from the furnace and air-cooled, utilizing natural cooling to quickly pass through the sensitive temperature range of 475℃ brittle phase precipitation. Through the above temperature control method, the mechanical properties and resistance to intergranular corrosion of the composite plate can be effectively guaranteed.
[0033] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0034] Example 1
[0035] A foreign clean and efficient coal utilization project uses SS321+SA542TypeDCL4a composite plates in its rotary kiln, with dimensions of (3+100) mm × 2120 mm × 10290 mm. The specific implementation is as follows: 1. The substrate, SA542TypeDCL4a, which meets the ASME SA-542 / SA-542M standard and has passed the physical and chemical performance test, is selected as the base plate. Its dimensions are 101mm×2160mm×10490mm. The cladding plate, SS321, which meets the ASME SA-240 / SA-240M standard and has passed the physical and chemical performance test, is selected as the cladding plate. The plates are welded according to the design requirements. The dimensions are 3mm×2200mm×10530mm. The upper and lower surfaces of the weld are polished with a 50# flap wheel to make them flush with the base material on both sides. The bonding surfaces of the base plate and cladding plate are polished with P60 and P80 calcined corundum abrasive belts to remove oxide scale and expose the metallic luster. The roughness Ra of the base plate and cladding plate is controlled to 1.2μm after polishing. 2. The blasting bed material is a combination of sand and soil in a 1:1 mass ratio, with a moisture content controlled at 10%. An engineering loader is used to lay and compact this composition into a blasting bed 11000mm long and 3000mm wide. Before laying, ensure there are no hard boulders or wooden blocks or other debris under the blasting bed. After compaction, the surface of the blasting bed should be flat and free of unevenness or tilting. Then, the polished substrate is placed horizontally on the blasting bed. The mating surfaces of the substrate and the cover plate are cleaned with ethanol. Next, "V"-shaped support pieces are placed at 350mm intervals around the edge of the substrate, with a height of 8mm and a distance of 1mm from the edge. "V"-shaped support pieces are then placed side-by-side at 500mm intervals within the edge area. The cleaned cover plate is then placed horizontally on the support pieces, ensuring that the four edges of the cover plate are proportionally offset from the substrate, and that the centers of both are aligned. After placement, the support pieces at the mating surfaces are checked for collapse or deformation. A schematic diagram of the explosive welding installation is shown below. Figure 1 As shown in the diagram, the distribution pattern of the support plates is as follows: Figure 2 As shown; 3. A 2mm thick gray cardboard is vertically fixed along the edge of the cover plate to form an explosive frame. The explosive frame is 50mm high and is used to prevent the explosives laid on the board from leaking outward. The joints between the sections of the explosive frame are sealed with transparent tape to prevent the explosives from leaking out of the gaps. At the same time, bamboo strips are vertically fixed on the outside of the explosive frame to keep the explosive frame at a 90° angle with the cover plate, thereby avoiding unstable energy distribution of the explosives at the edge due to the tilt of the explosive frame. 4. Mix powdered emulsion explosive (rock powdered emulsion explosive conforming to GB28286-2024 standard) with quartz sand particles and wood flour at a mass ratio of 50:45:5. After sieving twice and manually mixing twice, a mixture with a density of 0.92 g / cm³ is obtained. 31. Use explosive welding-specific explosive with a detonation velocity of 2056 m / s and a briss of 8.90 mm. 2. Spread the explosive evenly on the surface of the cover plate and level it to the designed height of 40 mm using a special tool. 3. Measure and verify the height with a stainless steel ruler, with an allowable deviation of ±2 mm. After confirming the height is correct, notify other workers to evacuate. 4. Inject 50 g of powdered emulsion explosive raw material into the edge of one long side of the cover plate. Press the raw material down moderately so that it is slightly higher than the surrounding explosive by 2-3 mm. 5. Vertically insert a digital electronic detonator at the center of the raw material as the detonation point. It is worth noting that placing the detonation point in this position effectively extends the detonator area outside the effective delivery size of the product, ensuring 100% bonding within the effective delivery size. 6. Connect the detonator lead wire to the blasting main line. 7. All personnel safely evacuate to the blasting area. 5. Using a special detonator to ignite the explosive, an SS321+SA542TypeDCL4a explosively welded composite plate for the rotary kiln of the clean coal energy project was produced. The composite plate was subjected to 100% ultrasonic non-destructive testing (UT) according to ASME SA-578 standard. The test results showed that the entire plate was 100% bonded and met the requirements of ASME SA-264 Class 1. 6. After cleaning the dirt and debris from the upper and lower surfaces of the composite board, place it into the heat treatment furnace at room temperature. Set the holding temperature to 620℃ (620℃±10℃) and the heating rate to 55℃ / h. After reaching the holding temperature, hold it for 206 minutes. After the holding is completed, implement segmented cooling. Slowly cool it to 500℃ in the furnace and then remove it from the furnace. Allow it to cool naturally to room temperature. 7. After the composite board is removed from the furnace, it should be allowed to cool naturally in the air. Once the surface temperature drops to approximately 30℃, leveling should be performed. During leveling, care should be taken to protect the surface and avoid localized surface defects or imperfections. After leveling, the flatness of the transverse ends of the composite board should be less than 5mm, and the flatness of the longitudinal long side should be 3mm / m, with no localized deformation or undulation along the entire long side. Then, 100% ultrasonic non-destructive testing should be performed again according to ASME SA-578 standard. The test results should meet the Class 1 requirements of ASME SA-264. 8. Mechanical property tests were conducted on samples of the composite plate. The yield strength of the substrate SA542TypeDCL4a was 480 MPa, the tensile strength was 689 MPa, the elongation was 29%, and the Charpy pendulum impact strength at -20℃ was 237 J, 226 J, and 229 J, respectively. The SS321 cladding layer underwent intergranular corrosion performance testing according to ASTM A262 E method, and the results showed that it was qualified, meeting the respective standard requirements and performance specifications. The shear strength of the composite plate reached 295 MPa. Metallographic examination of the composite plate showed good bonding at the composite interface, with a fine and uniform small wavy microstructure at the bonding surface, and no excessive embrittlement phase precipitation at the bonding surface. 9. The composite plate is flame-cut at the edges, and then the stainless steel surface is polished to a roughness of Ra=1.6μm. After the surface quality is visually inspected and qualified, it is packaged with vapor phase rust-preventive paper and put into storage. Finally, a SS321+SA542TypeDCL4a explosion-welded composite plate for rotary kilns in coal clean energy projects is obtained, which has passed all tests and meets the requirements of ASME SA-264 Class 1.
[0036] Example 2
[0037] A hydrotreating reactor in a foreign oil refinery project uses SA-240 SS347+SA542TypeDCL4a composite plates with dimensions of (4+108) mm × 2860 mm × 9870 mm. The specific implementation is as follows: 1. The substrate is SA542TypeDCL4a, which has passed the physical and chemical performance test and meets the ASME SA-542 / SA-542M standard. The specifications are 110mm×2900mm×10070mm. The cladding plate is SS347, which has passed the physical and chemical performance test and meets the ASME SA-240 / SA-240M standard. The substrate and cladding plate are welded according to the design requirements. The specifications are 4mm×2950mm×10110mm. The upper and lower surfaces of the weld are polished with a flap wheel to make them flush with the base material on both sides. The bonding surfaces of the substrate and cladding plate are polished with P60 and P80 calcined corundum abrasive belts to remove oxide scale and expose the metallic luster. The roughness Ra of the substrate and cladding plate is controlled to 1.2μm after polishing. 2. The blasting bed material is a combination of sand and soil in a 1:1 mass ratio, with a moisture content controlled at 10%. An engineering loader is used to lay and compact this composition into a blasting bed 11000mm long and 3500mm wide. Before laying, ensure there are no hard boulders or wooden blocks or other debris under the blasting bed. After compaction, the surface of the blasting bed should be flat and free of unevenness or tilting. Then, the polished substrate is placed horizontally on the blasting bed. The mating surfaces of the substrate and the cover plate are cleaned with ethanol. Next, "V"-shaped support pieces are placed at 350mm intervals around the edge of the substrate, with a height of 10mm and a distance of 1mm from the edge. Within the edge area, "V"-shaped support pieces are arranged in an equilateral triangle pattern at 500mm intervals. The cleaned cover plate is then placed horizontally on the support pieces, ensuring that the four edges of the cover plate are proportionally offset from the substrate, and that the centers of both are aligned. After placement, the support pieces at the mating surfaces are checked for collapse or deformation. The installation method and support piece distribution are the same as in Example 1. 3. A 2mm thick gray cardboard is vertically fixed along the edge of the cover plate to form an explosive frame. The explosive frame is 60mm high and is used to prevent the explosive laid on the board from leaking outward. The joints between the explosive frames are sealed with transparent tape to prevent the explosive from leaking out of the gaps. At the same time, bamboo strips are vertically fixed on the outside of the explosive frame to keep the explosive frame at a 90° angle with the cover plate, thereby avoiding unstable energy distribution of the explosive at the edge due to the tilt of the explosive frame. 4. Mix the powdered emulsion explosive (same as in Example 1) with quartz sand particles and wood flour at a mass ratio of 50:45:5. The mixture is then sieved twice and manually turned twice to obtain a density of 0.91 g / cm³. 3 A special composite explosive for explosive welding with a detonation velocity of 2047 m / s and a briss of 8.80 mm was prepared. The special composite explosive was then evenly spread on the surface of the cover plate and leveled to the designed height of 46 mm with a special tool. The height was measured and verified with a stainless steel ruler, with an allowable deviation of ±2 mm. After confirming that the explosive placement height was correct, other workers were notified to evacuate. Then, 55 g of powdered emulsion explosive raw material was injected into the center of the cover plate (different from the long edge of Example 1. Because the plate width of this example is larger, placing the detonation point at the edge is likely to cause large ripples at the final detonation end, affecting the bonding quality). The raw material was moderately pressed down so that it was slightly higher than the surrounding special explosive by 2-3 mm. A digital electronic detonator was vertically inserted into the center of the raw material and the detonator lead wire was connected to the blasting main line. All personnel were safely evacuated to the blasting area. 5. A special detonator was used to ignite the explosive, producing an SS347+SA542TypeDCL4a explosively welded composite plate for the hydrogenation reactor in the oil refinery project. The composite plate underwent 100% ultrasonic non-destructive testing (UT) according to ASME SA-578 standard. The test results showed that, except for the detonator zone at the detonation point (diameter...) The area outside the 20mm diameter area is fully bonded. The unbonded area of the detonator zone at the detonation point is a circular area with a diameter of 20mm. The unbonded area accounts for 0.001% of the total coverage area, which meets the requirements of ASME SA-264 Class 1 regarding unbonded areas, that is, there is no single unbonded area with an area greater than 1 in. (25mm) in the longest dimension direction of the product, and the total unbonded area does not exceed 1% of the total coverage surface area. 6. After cleaning the dirt and debris from the upper and lower surfaces of the composite board, place it into the heat treatment furnace at room temperature. Set the holding temperature to 600℃ (600℃±10℃) and the heating rate to 55℃ / h. After reaching the holding temperature, hold it for 225 minutes. After the holding is completed, implement segmented cooling. Slowly cool it to 500℃ in the furnace and then remove it from the furnace. Allow it to cool naturally to room temperature. 7. After the composite board is removed from the furnace, it is allowed to cool naturally in the air. Once the surface temperature drops to approximately 30℃, leveling is performed. During leveling, care is taken to protect the surface and avoid localized surface defects or imperfections. After leveling, the flatness of the transverse ends of the composite board should be less than 4mm, and the flatness of the longitudinal long side should be 2.53mm / m, with no localized deformation or undulation along the entire long side. Then, 100% ultrasonic non-destructive testing is performed again according to ASME SA-578 standard. The test results meet the Class 1 requirements of ASME SA-264. 8. Samples of the composite board were taken for physical and chemical performance tests. The SS347 coating was tested for intergranular corrosion performance according to ASTM A262 E method, and the results showed that it was qualified.
[0038] The substrate SA542TypeDCL4a has a yield strength of 514 MPa, a tensile strength of 699 MPa, an elongation of 23%, and Charpy impact strengths of 216 J, 221 J, and 209 J at -29°C at 1 / 4 thickness, respectively. At 1 / 2 thickness, the Charpy impact strengths are 203 J, 198 J, and 199 J at -29°C.
[0039] After undergoing 705℃×32h Max PWHT (maximum simulated post-weld heat treatment), the substrate sample exhibited a yield strength of 472 MPa, a tensile strength of 613 MPa, an elongation of 20%, and Charpy impact test results at -30℃ at 1 / 4 thickness of 211 J, 202 J, and 205 J, respectively. At 1 / 2 thickness, the Charpy impact test results at -30℃ were 201 J, 197 J, and 196 J, respectively.
[0040] The composite panel specimens were subjected to peel tests according to ASTM G146-01 to evaluate the sensitivity of the composite interface to hydrogen-induced peeling. The test conditions are as follows: a) Test temperature: 482℃; b) Test hydrogen pressure: 20 MPa; c) Hydrogen charging time: 48 hours; d) Cooling rate: not less than 300℃ / h; e) The test specimens shall be subjected to Max. PWHT.
[0041] The test specimens were of the type specified in ASTM G146-01. After being cooled by hydrogen purging, the specimens were placed for 168 hours before ultrasonic testing. The test results showed no peeling.
[0042] The composite plate was tested according to the shear test specified in SA-264 and SA-370, and the shear strength reached 304 MPa. Metallographic examination of the composite plate showed good bonding at the composite interface, with the metallographic structure of the bonding surface being a fine and uniform small wavy morphology, and no excessive embrittlement phase precipitation at the bonding surface; 9. Flame-cut the composite plate according to the delivery dimensions, clean off the cutting oxides and residues, and then polish the stainless steel surface to achieve a roughness of Ra=1.2μm or less. After the surface quality passes visual inspection, it is packaged and stored in the warehouse with vapor phase rust-preventive paper. Finally, a SA-240 SS347+SA542TypeDCL4a explosion-welded composite plate for the hydrogenation reactor of a foreign oil refinery project is obtained, which has passed all tests and meets the requirements of ASME SA-264 Class 1.
[0043] Example 3
[0044] The hydrocracking reactor in a certain residue oil hydrocracking project uses SB-424 N08825+SA542TypeDCL4a composite plates with dimensions of (3.3+92) mm × 3630 mm × 12810 mm. The specific implementation is as follows: 1. The substrate, SA542TypeDCL4a, which meets the ASME SA-542 / SA-542M standard and has passed the physical and chemical performance test, is selected as the base plate. Its dimensions are 94mm×3680mm×12950mm. The cladding plate, N08825, which meets the ASME SB-424 standard and has passed the physical and chemical performance test, is selected as the cladding plate. The substrate and cladding plate are welded according to the design requirements. The dimensions are 3.5mm×3720mm×13000mm. The upper and lower surfaces of the weld are polished with a flap wheel to make them flush with the base material on both sides. The bonding surfaces of the base plate and cladding plate are polished with P60 and P80 calcined corundum abrasive belts to remove oxide scale and expose the metallic luster. Considering the large plate size, P120 calcined corundum abrasive belts are used for final polishing. The roughness Ra of both the base plate and cladding plate is controlled to 1.0μm after polishing. 2. The blasting bed material is a combination of sand and soil in a 1:1 mass ratio, with a moisture content controlled at 10%. An engineering loader is used to lay and compact this composition into a blasting bed 14000mm long, 4000mm wide, and 300mm thick. Before laying, ensure there are no hard boulders or wooden blocks or other debris under the blasting bed. After compaction, the surface of the blasting bed should be flat and free of unevenness or tilting. Then, the polished substrate is placed horizontally on the blasting bed. The mating surfaces of the substrate and the cover plate are cleaned with ethanol. Next, "V"-shaped support pieces are placed at 350mm intervals around the edge of the substrate, with a height of 10mm and a distance of 1mm from the edge. Within the edge area, "V"-shaped support pieces are arranged in an equilateral triangle pattern at 500mm intervals. The cleaned cover plate is then placed horizontally on the support pieces, ensuring that the four edges of the cover plate are proportionally offset from the substrate, and that the centers of both are aligned. After placement, the support pieces at the mating surfaces are checked for collapse or deformation. The installation method and support piece distribution are the same as in Example 1. 3. A 2mm thick gray cardboard is vertically fixed along the edge of the cover plate to form an explosive frame. The explosive frame is 60mm high and is used to prevent the explosive laid on the board from leaking outward. The joints between the explosive frames are sealed with transparent tape to prevent the explosive from leaking out of the gaps. At the same time, bamboo strips are vertically fixed on the outside of the explosive frame to keep the explosive frame at a 90° angle with the cover plate, thereby avoiding unstable energy distribution of the explosive at the edge due to the tilt of the explosive frame. 4. Mix the powdered emulsion explosive (same as in Example 1) with quartz sand particles and wood flour at a mass ratio of 50:45:5. The mixture is then sieved twice and manually turned twice to obtain a density of 0.93 g / cm³. 3 A special composite explosive for explosive welding with a detonation velocity of 2068 m / s and a briss of 8.98 mm was prepared. The special composite explosive was then evenly spread on the surface of the cover plate and leveled to the designed height of 42 mm with a special tool. The height was measured and verified with a stainless steel ruler, with an allowable deviation of ±2 mm. After confirming that the explosive height was correct, other workers were notified to evacuate. Then, 50 g of powdered emulsion explosive raw material was injected into the center of the cover plate (different from the long edge of Example 1. Because the plate width of this example is larger, placing the detonation point at the edge is likely to cause large ripples at the final detonation end, affecting the bonding quality). The raw material was moderately pressed down so that it was slightly higher than the surrounding special explosive by 2-3 mm. A digital electronic detonator was vertically inserted into the center of the raw material and the detonator lead wire was connected to the blasting main line. All personnel were safely evacuated to the blasting area. 5. A special detonator was used to ignite the explosive, producing an ASME SB-424N08825+SA542TypeDCL4a explosively welded composite plate for the hydrocracking reactor in the residue oil hydrocracking project. The composite plate underwent 100% ultrasonic non-destructive testing (UT) according to ASME SA-578 standard. The test results showed that, except for the detonator zone at the detonation point (diameter...) The area outside the 25mm diameter area is fully bonded. The unbonded area of the detonator zone at the detonation point is a circular area with a diameter of 25mm. The unbonded area accounts for 0.001% of the total coverage area, which meets the requirements of ASME SA-265 Class 1 regarding unbonded areas, namely, there is no single unbonded area with an area greater than 1 in. (25mm) in the longest dimension direction of the product, and the total unbonded area does not exceed 1% of the total coverage surface area. 6. After cleaning the dirt and debris from the upper and lower surfaces of the composite board, place it into the heat treatment furnace at room temperature. Set the holding temperature to 590℃ (590℃±10℃) and the heating rate to 55℃ / h. After reaching the holding temperature, hold it for 240 minutes. After the holding is completed, implement segmented cooling. Slowly cool it to 480℃ in the furnace and then remove it from the furnace. Allow it to cool naturally to room temperature. 7. After the composite board is removed from the furnace, it is allowed to cool naturally in the air. Once the surface temperature has dropped to room temperature, leveling is performed. During leveling, care is taken to protect the surface to avoid localized surface defects or imperfections. After leveling, the flatness of the transverse ends of the composite board should be less than 5mm, and the flatness of the longitudinal long side should be 2.5mm / m, with no localized deformation or undulation along the entire long side. Then, 100% ultrasonic non-destructive testing is performed again according to ASME SA-578 standard. The test results meet the Class 1 requirements of ASME SA-265. 8. Samples of the composite board were taken for physical and chemical performance tests. The N08825 coating was subjected to intergranular corrosion performance tests according to ASTM G28 A method. The test time was 120 hours and the test temperature was 100℃. The mass losses were 0.0159g, 0.0211g, and 0.184g, and the corrosion rates were 0.08mm / a, 0.1mm / a, and 0.09mm / a, respectively. All of these met the customer requirement of ≤0.5mm / a, and the results showed that they were qualified.
[0045] The N08825 coating was subjected to a ferric chloride pitting corrosion test according to ASTM G48 A method. The test temperature was 22℃ and the test time was 72 hours. After the test, the sample was observed under 20x magnification. Slight corrosion was observed on the surface, and the corrosion rate was 2.70 g / m². 2 3.00g / m 2 3.60g / m 2 All meet customer requirements ≤4 g / m 2 The results showed that it was qualified.
[0046] The substrate SA542TypeDCL4a has a yield strength of 524 MPa, a tensile strength of 691 MPa, an elongation of 25%, and Charpy impact strengths of 228 J, 219 J, and 233 J at -30°C at 1 / 4 thickness, respectively. At -30°C at 1 / 2 thickness, the Charpy impact strengths are 201 J, 203 J, and 197 J, respectively.
[0047] The substrate SA542TypeDCL4a sample was subjected to high-temperature performance testing using a high-temperature tensile testing machine. The results showed that the substrate had a high-temperature yield strength of 496 MPa and a high-temperature tensile strength of 612 MPa at 440℃, which meets the requirements of the customer's technical documents that the yield strength is ≥462.8 MPa and the tensile strength is ≥514.2 MPa at 440℃.
[0048] 9. Flame-cut the composite plate according to the delivery dimensions, clean off the cutting oxides and residues, and then polish the nickel alloy surface to achieve a roughness of Ra=1.2μm or less. After the surface quality passes visual inspection, package it with vapor phase rust-preventive paper and put it into storage. Finally, a composite plate of SB-424 N08825+SA542TypeDCL4a explosion-welded plate for a hydrocracking project of a certain residue oil has been obtained, which has passed all tests and meets the requirements of ASME SA-265 Class 1.
[0049] The various embodiments in this specification are described in a progressive manner, with each embodiment focusing on the differences from other embodiments. The same or similar parts between the various embodiments can be referred to each other.
[0050] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing an exploded composite plate based on an SA542TypeDCL4a substrate, characterized in that, Includes the following steps: 1) Polish the SA542TypeDCL4a substrate and cladding using calcined corundum abrasive belt; 2) The polished SA542TypeDCL4a substrate and the cover plate are explosively welded to obtain an explosive composite plate precursor based on the SA542TypeDCL4a substrate; 3) The exploded composite plate precursor based on SA542TypeDCL4a substrate is heat-treated to obtain the exploded composite plate based on SA542TypeDCL4a substrate. The composite explosive used in the explosive welding includes powdered emulsion explosives, quartz sand particles, and wood powder. The mass ratio of the powdered emulsion explosive to quartz sand particles and wood flour is 42~58:38~50:2~8.
2. The method for preparing an exploded composite plate based on an SA542TypeDCL4a substrate according to claim 1, characterized in that, The surface roughness of the SA542TypeDCL4a substrate and the cladding after polishing in step 1) is 1~1.6μm.
3. The method for preparing an exploded composite plate based on an SA542TypeDCL4a substrate according to claim 2, characterized in that, The cover plate includes SS321, SS347, SS316L, 2205, 2507, N08825 or N06625.
4. A method for preparing an exploded composite plate based on an SA542TypeDCL4a substrate according to any one of claims 1 to 3, characterized in that, The explosive welding operation described in step 2) is as follows: S1: The polished SA542TypeDCL4a substrate, support layer, polished cover plate and explosive frame are sequentially stacked on the detonation bed; S2: Fill the explosive box with composite explosives. After the composite explosives are filled, add powdered emulsion explosives as detonators in the explosive box. Place a detonator in the center of the detonator. S3: Control the detonator to initiate the explosion, and the explosion is completed to achieve explosive welding.
5. The method for preparing an exploded composite plate based on an SA542TypeDCL4a substrate according to claim 4, characterized in that, In step S1, the support sheet layer includes support sheets at the edge and support sheets at the center. The support pieces at the edge are arranged linearly along the periphery of the substrate, and the distance between two adjacent support pieces is 300~500mm; The support plates in the center are arranged in a crisscross pattern, with a spacing of 300~500mm between adjacent support plates.
6. The method for preparing an exploded composite plate based on an SA542TypeDCL4a substrate according to claim 5, characterized in that, In step S2, the orthographic projection of the medicine frame has the same shape as the cover plate; The filling height of the composite explosive is 38~50mm; The additional powdered emulsion explosive is 50-60 g in weight.
7. The method for preparing an exploded composite plate based on an SA542TypeDCL4a substrate according to claim 6, characterized in that, The heat treatment operation described in step 3) includes: First, the exploded composite board precursor based on the SA542TypeDCL4a substrate is heated to the processing temperature and kept at that temperature. After the heat preservation is completed, it is cooled in stages to complete the heat treatment.
8. The method for preparing an exploded composite plate based on an SA542TypeDCL4a substrate according to claim 7, characterized in that, The heating rate is 55~90℃ / h, the processing temperature is 580~630℃, and the ratio of the holding time to the thickness of the exploded composite plate precursor based on the SA542TypeDCL4a substrate is 2~2.5min:1mm. The segmented cooling process involves first cooling the furnace to 480-520°C, and then allowing it to cool naturally in the air to room temperature.