A method for friction welding of dissimilar metals based on displacement and timing control
By employing a displacement and timing-based friction welding method for dissimilar metals, and using a four-stage process of non-planar interface prefabrication, micro-displacement pre-friction arc initiation, deceleration rheological filling, and over-stroke upsetting, the problem of inefficient manufacturing of dissimilar metals in rotary friction welding was solved, and stable welding initiation and full-section metallurgical bonding of dissimilar metals were achieved.
Patent Information
- Application Number
- CN202611208260.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-10
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies make it difficult to safely and densely manufacture dissimilar metal components with parameterized non-planar rotating body interfaces during rotary friction welding. Problems exist, such as crushing instability due to uneven contact, insufficient contact area, central dead zone, and flash control.
A dissimilar metal friction welding method based on displacement and timing control is adopted. Through a four-stage process of non-planar bonding interface prefabrication, micro-displacement pre-friction arc initiation, deceleration rheological filling, and over-stroke upsetting, the step changes of axial pressure and rotation speed are controlled to form an initial viscoplastic rheological layer and eliminate the central dead zone, thus achieving full-section metallurgical bonding.
It effectively avoids brittle crushing instability caused by stress concentration, realizes stable welding of dissimilar metals and full-section metallurgical bonding, and solves the problem of inefficient manufacturing of non-planar interfaces in rotary friction welding.
Smart Images

Figure CN123103153A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of solid-state welding of metals and advanced manufacturing forming technology, and in particular to a method for friction welding of dissimilar metals based on displacement and timing control. Background Technology
[0002] In aerospace, automotive, and heavy machinery industries, hybrid material components (such as steel-stainless steel composite shafts) are often required to meet the combined demands of lightweight design and high local load-bearing capacity. Existing research on custom forming proposes using non-planar, customized complex interfaces at the junction of the two materials, which can significantly improve the mechanical performance of components in service. For example, some studies have used static simulations to establish theoretical functions for non-planar interfaces constrained by both radial length and volume parameters.
[0003] However, this theoretical research mainly focuses on geometric optimization under static stress conditions, which has serious limitations at the practical physical manufacturing process level. When attempting to directly apply dissimilar metals with the aforementioned macroscopic non-planar theoretical interfaces to conventional rotary friction welding, the following engineering bottlenecks are encountered: Extremely uneven contact leads to crushing instability. The non-planar model means that initial contact during welding is limited to the curved tip, with a contact area of less than 5% of the total end face. If the constant speed and high pressure of conventional friction welding are used, the tip will instantly experience brittle crushing or local overheating and melting due to stress concentration, causing severe eccentric vibration and resulting in processing failure. There are also challenges in controlling the central dead zone and flash. The friction linear velocity of the non-planar interface increases non-linearly with radial distance in a complex manner. Without a matching dynamic pressure application process, severe flash is easily generated at the interface edge, while the low-speed zone in the center forms an irreversible incomplete penetration "dead zone" due to insufficient heat.
[0004] In summary, the engineering community still lacks a reliable manufacturing solution that can safely and densely transform such specific parametric geometric surfaces with excellent mechanical properties into real physical components through friction welding. Summary of the Invention
[0005] The purpose of this invention is to provide a method for friction welding of dissimilar metals based on displacement and timing control, which aims to solve the problem of inefficient manufacturing of dissimilar metals with parameterized non-planar rotating body interfaces during the rotation friction welding process.
[0006] To address the aforementioned technical problems, a method for friction welding of dissimilar metals based on displacement and timing control is provided, comprising the following steps: S1. Prefabrication of non-planar interface: The mating surfaces of the first and second parts to be welded are machined to form a convex non-planar rotational interface and a concave non-planar rotational interface that match each other; the convex non-planar rotational interface and the concave non-planar rotational interface are constrained by the interface radial length parameter. and interface volume constraint parameters They are jointly limited and satisfy the constraints. In the formula The outer diameter of the shaft body at the mating surface; S2. Micro-displacement pre-friction arc ignition: Clamp the first workpiece to be welded on the rotating spindle end, and clamp the second workpiece to be welded on the axial feed end; start the spindle corresponding to the rotating spindle end to rotate and control the axial feed end to axially advance towards the rotating spindle end at a first feed speed, within a set micro-displacement threshold. Within the interval, the initial viscoplastic rheological layer is formed by dry frictional heat generated at the interface tips of the convex non-planar rotating body interface and the concave non-planar rotating body interface. S3. Deceleration and rheological filling: When the axial displacement of the axial feed end relative to the rotating spindle end reaches the micro-displacement threshold... Then, the braking command of the spindle is triggered, causing the spindle speed to decrease nonlinearly from the current speed to zero within a preset window period; within the preset window period, the axial pressure is controlled to step up to the filling pressure, so that the softened metal at the contact interface between the first workpiece and the second workpiece is filled radially and axially along the geometric gap between the interface of the convex non-planar rotating body and the interface of the concave non-planar rotating body. S4. Over-stroke upsetting: After the spindle stops, the axial pressure is controlled to increase again to the upsetting pressure, and the axial feed end is controlled to perform over-stroke propulsion towards the rotating spindle end. The axial feed stroke is set. The initial oxide and low-temperature zone material between the convex non-planar rotating body interface and the concave non-planar rotating body interface are completely extruded radially to form flash, thereby completing the metallurgical bonding between the first workpiece to be welded and the second workpiece to be welded.
[0007] Furthermore, in the prefabrication of the non-planar interface, the generatrice contours of the convex non-planar rotational interface and the concave non-planar rotational interface satisfy the following relationship: ; in, The depth coordinates are along the axial direction.
[0008] Furthermore, in the prefabrication of the non-planar interface, the radial length constraint parameter of the interface is L=10mm, and the volume constraint parameter of the interface is V=1845mm³.
[0009] Furthermore, the first workpiece to be welded is 1045 steel, and the second workpiece to be welded is 304L stainless steel.
[0010] Furthermore, the initial axial pressure P1 in the micro-displacement pre-friction arc ignition, the filling pressure P2 in the deceleration rheological filling, and the upsetting pressure P3 in the over-stroke upsetting increase sequentially, and satisfy P3 > P2 > P1.
[0011] Furthermore, the initial axial pressure P1 is set to 30 MPa; the filling pressure P2 is set to 100 MPa; and the upsetting pressure P3 is set to 200 MPa.
[0012] Furthermore, the micro-displacement threshold The following relation is satisfied: = .
[0013] Furthermore, the axial feed stroke .
[0014] Furthermore, S2 to S4 constitute a segmented CNC process with dual closed-loop characteristics of spatial displacement and temporal sequence; in the micro-displacement pre-friction arc ignition, micro-displacement control is used as the closed-loop condition; in the deceleration rheological filling, the timing control triggered by the micro-displacement threshold is used as the closed-loop condition; and in the over-stroke upsetting, the spindle stops as the trigger condition and axial feed is implemented under constant pressure propulsion conditions.
[0015] Furthermore, in the micro-displacement pre-friction arc ignition, the spindle speed linearly increases from rest to 2200 rpm within 0.1 s and remains constant for 1.9 s; in the deceleration rheological filling, the preset window period is 0.5 s; in the over-stroke upsetting, the upsetting maintenance time after the spindle stops is 1.5 s.
[0016] Implementing the embodiments of the present invention will have the following beneficial effects: In this embodiment of the dissimilar metal friction welding method, the interface between the convex nonplanar rotating body and the interface between the concave nonplanar rotating body are constrained by the interface radial length parameter. and interface volume constraint parameters Commonly limited, micro-displacement pre-friction arc initiation, within a set micro-displacement threshold. Within the range, heat is generated through dry friction at the interface tip, forming an initial viscoplastic rheological layer. This is followed by decelerated rheological filling, causing the spindle speed to nonlinearly decrease to zero within a preset window period. The axial pressure is then stepped up to the filling pressure, allowing the softened metal to undergo radial and axial rheological filling along the geometric gaps between the interfaces. Over-stroke upsetting further increases the axial pressure to the upsetting pressure, and over-stroke propulsion completely extrudes the initial oxides and low-temperature materials between the interfaces radially. This avoids brittle crushing instability caused by stress concentration in the early stages of non-planar interface contact, achieving smooth welding initiation. Furthermore, the synergistic effect of the nonlinear decrease in speed during the deceleration phase and the step increase in axial pressure reconstructs the interface thermal field distribution, eliminates the central dead zone, and achieves full-section metallurgical bonding. This overcomes the problem of inefficient manufacturing of dissimilar metals with parameterized non-planar rotating body interfaces during rotary friction welding. Attached Figure Description
[0017] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0018] Figure 1 This is a flowchart illustrating the steps of the dissimilar metal friction welding method based on displacement and timing control as described in an embodiment of the present invention. Figure 2 This is a schematic diagram of the heat-generating region during the initial welding stage as described in an embodiment of the present invention; Figure 3 This is a schematic diagram of the plastic viscous rheological layer in the constant-speed quasi-steady-state friction stage as described in an embodiment of the present invention; Figure 4 This is a time-temperature comparison diagram of the central region during the friction stage between the embodiment of the present invention and a traditional flat-end structure; Figure 5 This is a time-temperature comparison diagram of the edge region during the friction stage between the embodiment of the present invention and a traditional flat-end structure; Figure 6 This is a schematic diagram of the static over-stroke upsetting end morphology according to an embodiment of the present invention; Figure 7 This is a two-dimensional schematic diagram of the theoretical profile of the non-planar parametric interface described in an embodiment of the present invention; Figure 8 This is a flowchart of the four-stage dynamic CNC process control logic and dual closed-loop timing switching described in an embodiment of the present invention; Figure 9 This is a graph showing the relationship between the piecewise nonlinear spindle speed and the process time as described in an embodiment of the present invention. Figure 10 This is a graph showing the relationship between the four-stage Z-axis feed rate / displacement and time as described in an embodiment of the present invention. Detailed Implementation
[0019] To facilitate understanding of the present invention, a more complete description will be given below with reference to the accompanying drawings. Preferred embodiments of the invention are shown in the drawings. However, the invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a thorough and complete understanding of the disclosure of the invention.
[0020] It should be noted that when a component is said to be "fixed to" another component, it can be directly attached to the other component or there may be an intervening component. When a component is said to be "connected to" another component, it can be directly connected to the other component or there may be an intervening component. The terms "vertical," "horizontal," "left," "right," and similar expressions used in this document are for illustrative purposes only.
[0021] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0022] Please refer to Figures 1-10 This invention provides a method for friction welding of dissimilar metals based on displacement and timing control. The method for friction welding of dissimilar metals in this embodiment includes the following steps: S1. Prefabrication of non-planar interface: The mating surfaces of the first and second parts to be welded are machined to form a convex non-planar rotational interface and a concave non-planar rotational interface that match each other; the convex non-planar rotational interface and the concave non-planar rotational interface are constrained by the interface radial length parameter. and interface volume constraint parameters They are jointly limited and satisfy the constraints. In the formula The outer diameter of the shaft body at the mating surface; S2. Micro-displacement pre-friction arc ignition: Clamp the first workpiece to be welded on the rotating spindle end, and clamp the second workpiece to be welded on the axial feed end; start the spindle corresponding to the rotating spindle end to rotate and control the axial feed end to advance axially towards the rotating spindle end at the first feed speed, within the set micro-displacement threshold. Within the interval, the initial viscoplastic rheological layer is formed by dry frictional heat generation at the interface tips of the convex nonplanar rotating body interface and the concave nonplanar rotating body interface. S3. Decelerated rheological filling: When the axial displacement of the axial feed end relative to the rotating spindle end reaches the micro-displacement threshold... Then, the spindle braking command is triggered, causing the spindle speed to decrease nonlinearly from the current speed to zero within a preset window period; within the preset window period, the axial pressure is stepped up to the filling pressure, so that the softened metal at the contact interface between the first and second workpieces is filled radially and axially along the geometric gap between the convex non-planar rotating body interface and the concave non-planar rotating body interface. S4. Over-stroke upsetting: After the spindle stops, the axial pressure is stepped up again to the upsetting pressure, and the axial feed end is controlled to perform over-stroke propulsion towards the rotating spindle end. The axial feed stroke is set. The initial oxides and low-temperature materials between the convex and concave nonplanar rotating body interfaces are completely extruded radially to form flash, completing the metallurgical bonding of the first and second workpieces to be welded. In specific applications, the first and second workpieces to be welded are respectively clamped at the rotating spindle end and the axial feed end of the friction welding machine. The mating end faces of the two are machined to form matching convex and concave nonplanar rotating body interfaces. The generatrix profile of the convex interface rises nonlinearly from the center of the end face to the edge, while the generatrix profile of the concave interface sinks mirror-symmetrically from the center of the end face to the edge. The difference in cross-sectional radii between the two interfaces at different axial depths remains continuously changing, forming a self-positioning rotating body fitting structure during assembly. After the spindle rotation is started, the axial feed end advances towards the rotating spindle end at a first feed speed. Within the micro-displacement threshold range, dry friction and heat generation occur at the contact tips of the two interfaces. Because the non-planar model limits initial contact to the curved tip, the contact area is less than 5% of the total end face. This micro-displacement control causes axial plastic adaptive running-in in the tip contact area, forming an initial viscoplastic rheological layer. Please refer to [reference needed]. Figure 2 Within the micro-displacement threshold range, heat is generated first at the interface tip contact area. Please refer to... Figure 3 A viscoplastic rheological transition layer, formed during the constant-speed quasi-steady-state friction stage, covers the central region of the interface. When the axial displacement reaches the micro-displacement threshold, a spindle braking command is triggered. The spindle speed nonlinearly decays to zero within a preset window period, while the axial pressure is stepped up to the filling pressure. The softened metal at the interface undergoes radial and axial rheological filling along the geometric gap between the convex and concave interfaces. Please refer to [reference needed]. Figure 4 and Figure 5 Due to the preferential contact at the tip of the non-planar interface, the central region rapidly rises to the steady-state viscoplastic rheological range within a very short time after welding, while the edge region maintains a cold, rigid constraint at medium to low temperatures. After the spindle stops rotating, the axial pressure increases again to the upsetting pressure, and the axial feed end continues to advance beyond the rotating spindle end, completely extruding the initial oxide and low-temperature material between the interfaces radially to form flash. Please refer to [reference needed]. Figure 6After static over-stroke upsetting is completed, the oxides and low-temperature metals at the original non-planar interface are completely extruded radially outward, forming curled flash at the outer edge of the composite component.
[0023] In one possible implementation, in the prefabrication of the nonplanar interface, the generatrix contours of the convex nonplanar body of revolution interface and the concave nonplanar body of revolution interface satisfy the following relationship: ; in, This represents the depth coordinates along the axial direction. For specific applications, please refer to [reference needed]. Figure 7 Under this function constraint, the surface elevation height of the convex interface from the center to the edge is mirror-symmetrical to the surface depression depth of the concave interface from the center to the edge. This ensures that the difference in cross-sectional radii between the two interfaces at different axial depths remains continuously variable, thus forming a geometrically matched rotating body interlocking structure before welding. The contact area at the tip of the interface is located near the center of the end face. As the axial depth x increases, the interface radius changes nonlinearly, ensuring that the contact area is limited to the microscopic tip in the initial stage of welding.
[0024] In one possible implementation, in the prefabrication of the nonplanar interface, the radial length constraint parameter of the interface is L=10mm, and the interface volume constraint parameter is V=1845mm³. In specific applications, under this parameter combination, the axial engagement depth and radial extension range of the convex nonplanar revolution interface and the concave nonplanar revolution interface are precisely defined, and the ratio of the contact area at the interface tip to the total volume is controlled within a specific range. The radial length constraint parameter defines the radial extension scale of the interface from the center of the end face to the edge, and the interface volume constraint parameter defines the volume space enclosed by the raised portion of the convex interface and the sunken portion of the concave interface; both together constrain the nonlinear curvature change of the generatrix profile.
[0025] In one possible implementation, the first workpiece to be welded is 1045 steel, and the second workpiece to be welded is 304L stainless steel. In a specific application, the first workpiece to be welded is made of 1045 steel and clamped at the end of the rotating spindle, while the second workpiece to be welded is made of 304L stainless steel and clamped at the axial feed end. Due to the difference in the coefficients of linear expansion between 1045 steel and 304L stainless steel, the two materials shrink differently at the joint during the cooling stage after welding. The uneven surface structure of the non-planar rotating body interface provides geometric constraints on this differential shrinkage, resulting in a deep interference-lock effect inside the joint.
[0026] In one possible implementation, the initial axial pressure P1 in the micro-displacement pre-friction arc ignition, the filling pressure P2 in the deceleration rheological filling, and the upsetting pressure P3 in the over-stroke upsetting are increased sequentially, satisfying P3 > P2 > P1. In specific applications, the initial axial pressure P1, filling pressure P2, and upsetting pressure P3 are applied in a three-stage progressively increasing manner. In the micro-displacement pre-friction arc ignition stage, the initial axial pressure P1 is maintained at a low level, causing only localized dry frictional heating at the contact tips of the convex non-planar rotating body interface and the concave non-planar rotating body interface. Upon entering the deceleration rheological filling stage, the axial pressure is stepped up to the filling pressure P2, driving the softened metal to rheologically fill along the interface gap. In the over-stroke upsetting stage, the axial pressure is further stepped up to the upsetting pressure P3, and axial feeding is implemented under constant pressure conditions, extruding the oxides and low-temperature materials at the interface radially.
[0027] In one possible implementation, the initial axial pressure P1 is set to 30 MPa; the filling pressure P2 is set to 100 MPa; and the upsetting pressure P3 is set to 200 MPa. In specific applications, the initial axial pressure P1 causes only microscopic viscoplastic rheology to occur at the tip contact area of the convex-concave interface during the initial stage of friction. The filling pressure P2 is set during the spindle deceleration window; this pressure works in conjunction with the deceleration process to allow the interface metal to complete radial and axial rheological filling along the geometric gap. The upsetting pressure P3 is set during the static extrusion process after the spindle stops; this pressure completely extrudes the low-temperature region material and initial oxides at the center of the interface radially as flash.
[0028] In one possible implementation, the micro-displacement threshold The following relation is satisfied: = In practical applications, within this range, the axial feed displacement relative to the rotating spindle end is strictly limited. The contact tips of the convex non-planar rotating body interface and the concave non-planar rotating body interface only undergo axial plastic adaptive running-in, forming a continuous viscoplastic rheological transition layer. Please refer to... Figure 2 Within the micro-displacement threshold range, heat is generated first at the interface tip contact area, and frictional heat extends from the tip to both radial sides.
[0029] In one possible implementation, the axial feed stroke In practical applications, within this stroke range, the axial feed end continuously advances towards the rotating spindle end, providing sufficient radial extrusion space for the initial oxide and central low-temperature zone material between the convex non-planar rotating body interface and the concave non-planar rotating body interface, thus forming a curled flash at the outer edge of the composite component. Please refer to... Figure 6 Through this large-stroke out-of-bounds deformation, the initial oxide scale and low-temperature metal at the original non-planar interface are completely extruded radially outward.
[0030] In one possible implementation, S2 to S4 constitute a segmented CNC process with dual closed-loop characteristics of spatial displacement and temporal sequence. In the micro-displacement pre-friction arc ignition stage, micro-displacement control is used as the closed-loop condition; in the deceleration rheological filling stage, timing control triggered by a micro-displacement threshold is used as the closed-loop condition; and in the over-stroke upsetting stage, spindle stop is used as the trigger condition, and axial feed is implemented under constant pressure propulsion conditions. Specifically, in the micro-displacement pre-friction arc ignition stage, micro-displacement control is used as the closed-loop condition, and the displacement of the axial feed end relative to the rotating spindle end is monitored in real time. When the displacement reaches the micro-displacement threshold... The next stage command is triggered at the specified time. The deceleration and rheological filling stage uses timing control triggered by a micro-displacement threshold as a closed-loop condition. The spindle speed decreases non-linearly within a preset window period, while the axial pressure increases stepwise. The over-stroke upsetting stage is triggered by the spindle stopping, implementing axial feed under constant pressure until metallurgical bonding is completed. Please refer to [reference needed]. Figure 8 The four-stage dynamic numerical control process control logic forms a dual closed-loop feature of spatial displacement and time sequence.
[0031] In one possible implementation, during micro-displacement pre-friction arc ignition, the spindle speed linearly increases from rest to 2200 rpm within 0.1 s and remains constant for 1.9 s; during deceleration rheological filling, the preset window period is 0.5 s; and during over-stroke upsetting, the upsetting duration after the spindle stops is 1.5 s. In specific applications, the spindle speed linearly increases from rest to 2200 rpm within 0.1 s, and this increase causes transient shear friction at the tips of the convex and concave interfaces. During the 1.9 s constant speed operation, frictional heat extends radially from the tips to both sides, and the interface metal reaches the thermomechanical softening critical point. Please refer to [reference needed]. Figure 9 After the spindle speed reaches a constant speed, it enters a nonlinear decay phase. When the axial displacement reaches a micro-displacement threshold, the spindle speed nonlinearly decays from 2200 rpm to zero within a preset window of 0.5 seconds, during which time the filling pressure increases stepwise. Please refer to... Figure 10 After the deceleration phase, the Z-axis feed speed enters the constant pressure propulsion phase. After the spindle stops, the upsetting pressure is maintained for 1.5 seconds, and the axial feed end performs over-stroke propulsion under constant pressure to complete the large plastic discharge.
[0032] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of the patent application. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the scope of protection of the present invention. Therefore, the scope of protection of this patent should be determined by the appended claims.
Claims
1. A method for friction welding of dissimilar metals based on displacement and timing control, characterized in that, Includes the following steps: S1. Prefabrication of non-planar interface: The mating surfaces of the first and second parts to be welded are machined to form a convex non-planar rotational interface and a concave non-planar rotational interface that match each other; the convex non-planar rotational interface and the concave non-planar rotational interface are constrained by the interface radial length parameter. and interface volume constraint parameters They are jointly limited and satisfy the constraints. In the formula The outer diameter of the shaft body at the mating surface; S2. Micro-displacement pre-friction arc ignition: clamp the first workpiece to be welded on the end of the rotating spindle and clamp the second workpiece to be welded on the axial feed end. The spindle corresponding to the rotating spindle end is started to rotate, and the axial feed end is controlled to axially advance towards the rotating spindle end at a first feed speed, within a set micro-displacement threshold. Within the interval, the initial viscoplastic rheological layer is formed by dry frictional heat generated at the interface tips of the convex non-planar rotating body interface and the concave non-planar rotating body interface. S3. Deceleration and rheological filling: When the axial displacement of the axial feed end relative to the rotating spindle end reaches the micro-displacement threshold... Then, a braking command is triggered on the spindle, causing the spindle speed to decrease non-linearly from the current speed to zero within a preset window period; Within the preset window period, the axial pressure is stepped up to the filling pressure, so that the softened metal at the contact interface between the first workpiece and the second workpiece is filled radially and axially along the geometric gap between the convex non-planar rotating body interface and the concave non-planar rotating body interface. S4. Over-stroke upsetting: After the spindle stops, the axial pressure is controlled to increase again to the upsetting pressure, and the axial feed end is controlled to perform over-stroke propulsion towards the rotating spindle end. The axial feed stroke is set. The initial oxide and low-temperature zone material between the convex non-planar rotating body interface and the concave non-planar rotating body interface are completely extruded radially to form flash, thereby completing the metallurgical bonding between the first workpiece to be welded and the second workpiece to be welded.
2. The method for friction welding dissimilar metals according to claim 1, characterized in that, In the prefabrication of the non-planar interface, the generatrice contours of the convex non-planar rotational interface and the concave non-planar rotational interface satisfy the following relationship: ; in, The depth coordinates are along the axial direction.
3. The method for friction welding of dissimilar metals according to claim 2, characterized in that, In the prefabrication of the non-planar interface, the radial length constraint parameter of the interface is L=10mm, and the volume constraint parameter of the interface is V=1845mm³.
4. The method for friction welding of dissimilar metals according to claim 1, characterized in that, The first workpiece to be welded is 1045 steel, and the second workpiece to be welded is 304L stainless steel.
5. The method for friction welding of dissimilar metals according to claim 1, characterized in that, The initial axial pressure P1 in the micro-displacement pre-friction arc ignition, the filling pressure P2 in the deceleration rheological filling, and the upsetting pressure P3 in the over-stroke upsetting increase sequentially, and satisfy P3 > P2 > P1.
6. The method for friction welding dissimilar metals according to claim 5, characterized in that, The initial axial pressure P1 is set to 30 MPa; the filling pressure P2 is set to 100 MPa; and the upsetting pressure P3 is set to 200 MPa.
7. The method for friction welding of dissimilar metals according to claim 1, characterized in that, The micro-displacement threshold The following relation is satisfied: = .
8. The method for friction welding of dissimilar metals according to claim 1, characterized in that, The axial feed stroke .
9. The method for friction welding of dissimilar metals according to claim 8, characterized in that, S2 to S4 constitute a segmented CNC process with dual closed-loop characteristics of spatial displacement and time sequence; in the micro-displacement pre-friction arc ignition, micro-displacement control is used as the closed-loop condition; in the deceleration rheological filling, the time sequence control triggered by the micro-displacement threshold is used as the closed-loop condition; in the over-stroke upsetting, the spindle stops as the trigger condition and axial feed is implemented under constant pressure propulsion conditions.
10. The method for friction welding of dissimilar metals according to claim 9, characterized in that, In the micro-displacement pre-friction arc ignition, the spindle speed linearly increases from rest to 2200 rpm within 0.1 s and remains constant for 1.9 s; in the deceleration rheological filling, the preset window period is 0.5 s; in the over-stroke upsetting, the upsetting maintenance time after the spindle stops is 1.5 s.