A high-strength precipitation-hardening stainless steel welding wire alloy and its processing method
By controlling the Al content and introducing the Zr+Ce+La composite rare earth system, the problems of Al oxidation and burn-off and grain boundary inclusions in the welding wire during the welding process were solved, improving the resistance to hot cracking and low-temperature toughness of the weld, ensuring the high strength and stability of the welding wire during the welding process, and meeting the high performance requirements of aerospace and other fields.
Patent Information
- Application Number
- CN202611479789.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-22
- Publication Date
- 2026-11-17
AI Technical Summary
Existing ultra-high strength welding wires suffer from Al oxidation burn-off and insufficient toughness and crack resistance due to grain boundary inclusions during the welding process, making it difficult to meet the requirements of aerospace and other fields for ultra-high strength and corrosion resistance.
By controlling the Al content, introducing the Zr+Ce+La composite rare earth system, and strictly controlling the Nb content, fine rare earth oxysulfides are formed, which purify the grain boundaries, improve the hot crack resistance and low temperature toughness of the weld, and ensure the high-density nucleation and precipitation of the NiAl(B2) strengthening phase.
It achieves improved weld strength, crack resistance, and low-temperature toughness. The welding wire exhibits excellent fatigue resistance and a stable primary strengthening system during the welding process, meeting the welding requirements of ultra-high strength load-bearing structures.
Smart Images

Figure CN123103250A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of welding wire alloys for gas shielded welding, and in particular to an ultra-high strength precipitation hardening stainless steel welding wire alloy and its processing method. Background Technology
[0002] With the increasing demands for welding quality of load-bearing structures in aerospace, high-end mold and marine engineering fields, the market urgently needs a gas shielded welding wire that combines ultra-high strength (tensile strength of weld metal ≥1700MPa) and stainless steel-grade corrosion resistance.
[0003] Existing ultra-high strength welding wires are mainly classified into the following categories: (1) 18Ni series martensitic aging steel welding wire (such as 18Ni-8Co-4.9Mo-0.40Ti-0.10Al specified in SAE AMS 6501E) can achieve a tensile strength of 255ksi (about 1758MPa) after aging treatment. However, the chromium content is <1%. After welding, the weld and heat-affected zone are very easy to rust in atmospheric or weakly corrosive environments. It is necessary to add a coating or plating for protection, which increases the process cost and maintenance burden, and is difficult to use in corrosive conditions.
[0004] (2) Conventional precipitation hardening stainless steel welding wire (such as AWS A5.9 ER630, corresponding to 17-4PH base material) is subjected to aging treatment at 480-620℃ after welding. The tensile strength of the deposited metal is about 1030-1100MPa. Although its corrosion resistance is close to that of 304 stainless steel, its strength is far lower than the welding requirements of ultra-high strength load-bearing parts and cannot replace 18Ni series or low alloy high strength steel welding wire.
[0005] (3) Custom465 series welding wire (UNS S46500, corresponding to US patents US5681528 and US5855844). Custom465 is a Ti-strengthened martensitic precipitation hardening stainless steel with the following chemical composition (wt%): Cr 11.00-12.50, Ni 10.75-11.25, Mo 0.75-1.25, Ti 1.50-1.80, C≤0.02, Mn≤0.25, Si≤0.25, P≤0.015, S≤0.010, with the balance being Fe. Its solution treatment temperature is 982℃±8℃, followed by rapid cooling after holding at that temperature. Custom465 can achieve extremely high strength under cold working and aging conditions: after 71% cold drawing and aging at 482℃, the tensile strength can reach approximately 2089MPa, and the hardness reaches 55HRC. This alloy has been used in GTA welding processes, and Carpenter recommends using PyrometX-23 alloy as filler metal for GMA welding to avoid weld cracking.
[0006] Carpenter Custom 475 (UNS S14750, corresponding to US Patent US6630103B2) is a Cr-Co-Ni-Mo-Al martensitic precipitation-hardening stainless steel. The base metal exhibits a tensile strength of approximately 1930-2000 MPa under aging conditions at 525°C, while also possessing stainless steel-grade corrosion resistance imparted by 10.5-11.5% Cr. It is one of the strongest grades of existing precipitation-hardening stainless steels. This patent discloses the alloy's application in bars, strips, golf club heads, and aerospace structural components, but does not cover welding wire products, nor does it provide a composition adjustment scheme suitable for welding conditions.
[0007] If the composition of Custom475 base material (Al 1.5%, Ti 0.005–0.05%) is directly used for φ1.2mm grade MIG welding wire, the following technical problems exist: First, the Al content is at the nominal value of the base material (1.5%). Under the high temperature of the welding arc, Al is easily oxidized and burned off (Al2O3 has a very negative Gibbs free energy), which leads to a decrease in the effective Al content in the weld metal, thereby weakening the NiAl content. The nucleation density of the B2 strengthening phase; simultaneously, if the Al2O3 inclusions formed by oxidation are distributed in a thin film at the grain boundaries, they will reduce the ductility and crack resistance of the deposited metal. Conventional PH stainless steel welding wire (such as ER630) refines the grains and assists in strengthening by adding 0.15–0.30% Nb to form Nb(C,N), but this idea originates from the Ni3Ti system and is directly transplanted to NiAl... In the 475 system dominated by B2+R coprecipitation, Nb preferentially combines with Ni to form the γ″ phase, competing with B2 for Ni atoms, which in turn impairs the peak aging intensity. Second, the Ti content is only 0.005–0.05%, which is much lower than that of 18Ni welding wire (0.40% Ti in AMS 6501E) and Custom465 (1.5–1.8% Ti). The weld pool lacks sufficient TiN / TiC heterogeneous nucleation particles, the cast columnar crystals are coarse, and the weld toughness and crack resistance are insufficient. Third, although the control of C, N, and O in the base material (C≤0.015%, N≤0.010%, O≤0.003%) is already low, it has not been further tightened for the fine-diameter drawing of welding wire (total area reduction rate ≥97%) and the high-temperature working conditions of the welding pool: high C content will aggravate the embrittlement of HAZ grain boundary carbides; N has a strong affinity for Al, which easily forms AlN inclusions and deteriorates toughness; even if the O content is 30ppm, it will still consume a lot of Al to generate Al2O3, reduce the nucleation density of B2, and affect the surface quality of the welding wire (oxide intrusion leads to poor wire feeding).
[0008] The inventors recognized that there was still room for further improvement in such solutions in the prior art. Summary of the Invention
[0009] The main objective of this invention is to provide an ultra-high strength precipitation-hardening stainless steel welding wire alloy and its processing method. By controlling the Al content, high-density nucleation and precipitation of the NiAl(B2) strengthening phase is ensured. By controlling the content of Mn, Cu, P, and S, the formation of low-melting-point eutectic and harmful inclusions is eliminated from the source, improving the weld's resistance to hot cracking and low-temperature toughness. A Zr+Ce+La (0.002–0.020%) composite rare earth system is introduced. Zr, Ce, and La have extremely strong deoxidation and desulfurization capabilities, which can further capture O and S and form fine, spherical rare earth oxysulfides, replacing harmful strip-shaped Al2O3 or MnS. This not only purifies the grain boundaries but also significantly improves the weld's ductility and fatigue resistance. Nb is strictly controlled at an extremely low level, serving only as a trace stabilizing element for grain boundaries, inhibiting the coarsening of the B2 phase during long-term aging, and never forming a γ″ phase to compete with B2 for Ni, thus ensuring the stability of the primary strengthening system. According to one aspect of the present invention, an ultra-high strength precipitation-hardening stainless steel welding wire alloy is provided, comprising, by mass percentage, the following components: Cr: 10.5~11.8%, Ni: 8.5~9.0%, Mo: 4.75~6.25%, Co: 8.0~11.0%, Ti: 0.03~1.0%, Al: 1.00~1.65%, C≤0.015%, Mn≤0.01%, Si≤0.10%, P≤0.002%, S≤0.002%, Cu≤0.01%, Nb: 0.005~0.02%, B: 0.0015~0.0035%, N≤0.001%, O≤0.001%, Zr+Ce+La: 0.002~0.020%, with the balance being Fe and unavoidable impurities.
[0010] According to one embodiment of the present invention, the content of Al in the ultra-high strength precipitation hardening stainless steel welding wire alloy is 1.50~1.65% by mass percentage.
[0011] According to one embodiment of the present invention, the content of Ti in the ultra-high strength precipitation hardening stainless steel welding wire alloy is 0.03~0.08% by mass percentage.
[0012] According to another aspect of the present invention, a method for processing ultra-high strength precipitation-hardening stainless steel welding wire alloy is provided, comprising the following steps: S1. The ultra-high strength precipitation hardening stainless steel welding wire alloy is smelted by VIM+VAR to obtain consumable ingots. The consumable ingots are homogenized at 1200-1280℃ and held for 20-28 hours. S2. The homogenized consumable ingot is hot forged and / or hot rolled to form a wire rod. The wire rod is then subjected to solution treatment at a temperature of 900-950°C, followed by heat treatment and air cooling. S3. The solution-treated wire blank is subjected to multiple cold drawing passes, and after solution softening, the surface is polished to obtain welding wire.
[0013] According to one embodiment of the present invention, in step S2, the diameter of the wire blank is in the range of 8.0~9.0 mm.
[0014] According to one embodiment of the present invention, in step S2, the duration of the solution treatment is 3 to 8 hours.
[0015] According to one embodiment of the present invention, in step S3, the solution softening is performed when the wire diameter is cold drawn to 3.0~3.5mm, and the temperature range is 900~950℃.
[0016] According to one embodiment of the present invention, the diameter of the welding wire is 0.8~1.6mm.
[0017] According to one embodiment of the present invention, the surface roughness Ra of the welding wire is ≤0.4μm.
[0018] According to one embodiment of the present invention, the hardness of the welding wire in the solution-treated state is HRC 28~33.
[0019] In an embodiment of the present invention, an ultra-high strength precipitation-hardening stainless steel welding wire alloy and its processing method are described. By controlling the Al content, high-density nucleation and precipitation of the NiAl(B2) strengthening phase are ensured. By controlling the content of Mn, Cu, P, and S, the formation of low-melting-point eutectics and harmful inclusions is eliminated from the source, improving the weld's resistance to hot cracking and low-temperature toughness. The introduction of a Zr+Ce+La (0.002–0.020%) composite rare earth system, where Zr, Ce, and La possess extremely strong deoxidation and desulfurization capabilities, can further capture O and S and form fine, spherical rare earth oxysulfides, replacing harmful strip-shaped Al2O3 or MnS. This not only purifies the grain boundaries but also significantly improves the weld's ductility and fatigue resistance. Nb is strictly controlled at extremely low levels, serving only as a trace stabilizing element for grain boundaries, inhibiting the coarsening of the B2 phase during long-term aging, and never forming a γ″ phase to compete with B2 for Ni, ensuring the stability of the primary strengthening system. Attached Figure Description To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some implementation examples of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0020] Figure 1 A process flow diagram of a method for processing an ultra-high strength precipitation hardening stainless steel welding wire alloy according to an exemplary embodiment of the present invention is shown. Detailed Implementation
[0021] The following detailed description of the embodiments is intended to exemplify the principles of the present invention, but should not be construed as limiting the scope of the invention. The present invention can be implemented in many different forms and is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.
[0022] These embodiments are provided to make this disclosure thorough and complete, and to fully express the scope of the invention to those skilled in the art. It should be noted that, unless otherwise specifically stated, the relative arrangement of components and steps, material composition, numerical expressions, and values set forth in these embodiments should be interpreted as merely exemplary and not as limiting.
[0023] It should be noted that, in the description of this invention, unless otherwise stated, "a plurality of" means two or more; the terms "upper," "lower," "left," "right," "inner," and "outer," etc., indicating orientation or positional relationships, are only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this invention. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.
[0024] It should also be noted that, in the description of this invention, unless otherwise explicitly specified and limited, the terms "installation," "connection," and "joining" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a direct connection or an indirect connection through an intermediate medium. Those skilled in the art can understand the specific meaning of the above terms in this invention depending on the specific circumstances. When a specific device is described as being located between a first device and a second device, an intermediary device may or may not be present between the specific device and the first or second device.
[0025] All terms used in this invention have the same meaning as understood by one of ordinary skill in the art to which this disclosure pertains, unless otherwise specifically defined. It should also be understood that terms defined in general dictionaries should be interpreted as having meanings consistent with their meanings in the context of the relevant art, and not as idealized or highly formalized, unless expressly defined herein.
[0026] Techniques, methods, and equipment known to those skilled in the art may not be discussed in detail, but where appropriate, such techniques, methods, and equipment should be considered part of the specification.
[0027] like Figure 1 As shown, the present invention provides an ultra-high strength precipitation hardening stainless steel welding wire alloy, which comprises the following components by mass percentage: Cr: 10.5~11.8%, Ni: 8.5~9.0%, Mo: 4.75~6.25%, Co: 8.0~11.0%, Ti: 0.03~1.0%, Al: 1.00~1.65%, C≤0.015%, Mn≤0.01%, Si≤0.10%, P≤0.002%, S≤0.002%, Cu≤0.01%, Nb: 0.005~0.02%, B: 0.0015~0.0035%, N≤0.001%, O≤0.001%, Zr+Ce+La: 0.002~0.020%, with the balance being Fe and unavoidable impurities.
[0028] In the ultra-high strength precipitation-hardening stainless steel welding wire alloy and its processing method according to embodiments of the present invention, the formation of low-melting-point eutectic and harmful inclusions is eliminated from the source by controlling the content of Mn, Cu, P and S, thereby improving the hot crack resistance and low-temperature toughness of the weld. The introduction of a Zr+Ce+La (0.002–0.020%) composite rare earth system, in which Zr, Ce and La have extremely strong deoxidation and desulfurization capabilities, can further capture O and S and form fine, spherical rare earth oxysulfides, replacing harmful strip-shaped Al2O3 or MnS. This not only purifies the grain boundaries but also significantly improves the ductility and fatigue resistance of the weld. Nb is strictly controlled at an extremely low level, serving only as a trace stabilizing element for grain boundaries, suppressing the coarsening of the B2 phase during long-term aging, and never forming a γ″ phase to compete with B2 for Ni, thus ensuring the stability of the primary strengthening system. In some specific embodiments, the Al content in the ultra-high strength precipitation hardening stainless steel welding wire alloy is 1.50~1.65% by mass percentage. The Al content is slightly increased from about 1.19% in the base material to 1.50~1.65% to compensate for the oxidation loss (about 0.10~0.15%) during the welding arc process, ensuring that the effective Al content in the deposited metal is maintained at a sufficient level of 1.35~1.50%, thereby ensuring the high-density nucleation and precipitation of the NiAl(B2) strengthening phase.
[0029] Based on the above embodiments, the Ti content in the ultra-high strength precipitation-hardening stainless steel welding wire alloy is 0.03~0.08% by mass percentage. By controlling Ni in the range of 8.5~9.0% of the base material and maintaining the Ti content at a trace level of 0.03~0.08%, the primary co-precipitation system of NiAl-B2+R is not disturbed, while an appropriate amount of TiN particles are formed to assist in grain refinement.
[0030] This invention also provides a method for processing ultra-high strength precipitation-hardening stainless steel welding wire alloy, which includes the following steps: S1. The ultra-high strength precipitation hardening stainless steel welding wire alloy is smelted by VIM+VAR to obtain consumable ingots. The consumable ingots are homogenized at 1200-1280℃ and held for 20-28 hours. S2. The homogenized consumable ingot is hot forged and / or hot rolled to form a wire rod. The wire rod is then solution treated at a temperature of 900-950℃, held at the temperature, and then air-cooled. S3. The solution-treated wire blank is subjected to multiple cold drawing passes, and after solution softening, the surface is polished to obtain welding wire.
[0031] In some specific embodiments, in step S2, the diameter of the wire blank ranges from 8.0 to 9.0 mm.
[0032] Based on the above embodiments, in step S2, the solution treatment time is 3~8 hours.
[0033] In some specific embodiments, in step S3, solution softening is performed when the wire diameter is cold-drawn to 3.0~3.5mm, and the temperature range is 900~950℃.
[0034] Based on the above embodiments, the diameter of the welding wire is 0.8~1.6mm.
[0035] In some specific embodiments, the surface roughness Ra of the welding wire is ≤0.4μm.
[0036] Based on the above embodiments, the hardness of the welding wire in the solution-treated state is HRC 28~33.
[0037] This application optimizes the alloy composition based on the Custom475 base metal composition for welding wire applications, enabling it to leverage the combined advantages of the 475 series' ultra-high strength and corrosion resistance while meeting the process requirements of crack resistance, weld microstructure refinement, and small-diameter welding wire preparation in MIG welding. This solves the problems of insufficient B2 strengthening phase due to Al oxidation burn-off, coarse weld microstructure, and difficulty in preparing small-diameter welding wire when the existing Custom475 base metal composition is directly used for welding wire.
[0038] The present application will be described in detail below through specific embodiments.
[0039] Example 1 Custom 475 series modified welding wire alloy is prepared according to the following composition (wt%): Cr 11.2%, Ni 8.8%, Mo 5.0%, Co 8.5%, Ti 0.03%, Al 1.58%, C 0.012%, Mn 0.008%, Si 0.05%, P 0.0015%, S 0.0017%, Cu 0.008%, Nb 0.01%, B 0.0025%, N 0.0007%, O 0.0007%, (Zr+Ce+La): 0.009%, balance being Fe and unavoidable impurities.
[0040] Preparation process: VIM+VAR melting; self-consumable ingot homogenized at 1250℃ for 24h; hot forging / hot rolling to φ8.5mm wire rod; solution treatment: 925℃×5h, air cooling; multiple cold drawing to φ1.2mm, with a 925℃ solution softening at φ3.2mm in between; surface polishing; coiled into D300mm welding wire spool, net weight 5kg.
[0041] Welding wire properties: solution-treated state, hardness HRC30; surface roughness Ra, 0.30μm; welding performance (MIG welding, Ar+2%O2 protection, heat input 1.2kJ / mm). In the as-welded state, after aging at 520℃ for 4h, the weld tensile strength is 1930MPa; the weld area reduction is 38%; Y-groove crack resistance test shows no cracks (moderate restraint); weld grain size is ASTM grade 9; deposited metal O content is 0.0012% (12ppm).
[0042] Example 2 The welding wire alloy was prepared according to the following composition (wt%): Ti 0.07%, Al 1.62%, Nb 0.015%, (Zr+Ce+La): 0.008%, and the remaining composition and preparation process were the same as in Example 1.
[0043] Welding wire properties: Solution hardness, HRC29; Surface roughness Ra: 0.32μm.
[0044] Welding performance. In the as-welded state, after aging at 520℃ for 4 hours, the tensile strength of the weld is 1920 MPa; the reduction of area of the weld is 40%; in the Y-groove crack resistance test, no cracks were found.
[0045] Comparative Example 1 Using the base material composition of Example 1 in US6630103B2 (Al 1.19%, Ti 0.02%, O 7ppm, no B / RE / Zr), a φ1.2mm welding wire was prepared according to the same process.
[0046] Welding performance: In the as-welded state, the tensile strength of the weld after aging at 520℃ for 4 hours is 1810 MPa. Due to Al burn-off, the strength is lower than that of the example. The weld area reduction rate is 22%. In the Y-groove crack resistance test, visible microcracks appeared. The weld grain size is ASTM 5-6, with coarse columnar grains.
[0047] Conclusion: Comparative Example 1 suffered from insufficient nucleation of the B2 phase due to Al oxidation and burn-off, and lacked rare earth purification and microalloying. Its strength, plasticity, and crack resistance were significantly inferior to those of Examples 1 and 2. This confirms the necessity of the composition optimization of the present invention, which involves "Al micro-lifting, extreme purity, and microalloying of multiple active metals (Zr, La, Ce)".
[0048] The beneficial effects of implementing this invention include: (1) Ensuring ultra-high strength (compensating for Al burn-off): The Al content is slightly increased from approximately 1.19% of the base metal to 1.50~1.65% to compensate for oxidation burn-off during the welding arc process (approximately 0.10~0.15%), ensuring that the effective Al content in the weld metal is maintained at a sufficient level of 1.35~1.50%, thereby guaranteeing high-density nucleation and precipitation of the NiAl(B2) strengthening phase. After aging at 520℃, the tensile strength of the weld metal can reach 1900~1960MPa, matching more than 95% of the strength of the base metal, meeting the requirements of ultra-high strength load-bearing weldments.
[0049] (2) Extreme purity and microstructure refinement: By compressing Mn and Cu to ≤0.01% and P and S to ≤0.002%, the formation of low-melting-point eutectics and harmful inclusions is eliminated from the source, greatly improving the weld's resistance to hot cracking and low-temperature toughness. At the same time, Ni is controlled in the mother material at a content of 7.0~9.0% (preferably 8.5~9.0%), and Ti content is maintained at a trace level of 0.03~0.08%, which neither interferes with the primary co-precipitation system of NiAl-B2+R, but also forms an appropriate amount of TiN particles to assist in grain refinement.
[0050] (3) Synergistic purification and strengthening of multiple rare earth elements: A Zr+Ce+La (0.002~0.020%) composite rare earth system is introduced. Zr, Ce, and La have extremely strong deoxidation and desulfurization capabilities, which can further capture O and S and form fine, spherical rare earth oxides and sulfides, replacing harmful strip-shaped Al2O3 or MnS. This not only purifies the grain boundaries but also significantly improves the ductility and fatigue resistance of the weld.
[0051] (4) Precise microalloying: Nb is strictly controlled at an extremely low level of 0.005~0.02%, and is used only as a trace stabilizing element at the grain boundary to suppress the coarsening of the B2 phase during long-term aging, and never forms the γ″ phase to compete with B2 for Ni, thus ensuring the stability of the original strengthening system.
[0052] (5) Extreme gas control: Both N and O are strictly controlled to ≤0.001% (10ppm), which is the highest purity level of industrial welding wire. The extremely low N eliminates the formation of AlN inclusions, and the extremely low O minimizes the consumption of effective Al by Al2O3, ensuring that every bit of Al is used for the precipitation of the B2 phase.
[0053] (6) Improved processability of filament preparation: The extremely pure matrix and very few hard inclusions make the cold drawing process of φ0.8~φ1.6mm filament smoother, with higher surface smoothness and excellent wire feeding stability.
[0054] The above are exemplary embodiments disclosed in this invention. The order of the disclosed embodiments is merely for descriptive purposes and does not represent the superiority or inferiority of the embodiments. However, it should be noted that the discussion of any of the above embodiments is merely exemplary and is not intended to imply that the scope of the disclosed embodiments of this invention (including the claims) is limited to these examples. Various changes and modifications can be made without departing from the scope defined by the claims. The functions, steps, and / or actions of the methods according to the disclosed embodiments described herein do not need to be performed in any particular order. Furthermore, although the elements disclosed in the embodiments of this invention may be described or claimed individually, they may be understood as multiple unless explicitly limited to a singular.
[0055] Those skilled in the art should understand that the discussion of any of the above embodiments is merely exemplary and is not intended to imply that the scope of the invention (including the claims) is limited to these examples. Within the framework of the invention, technical features of the above embodiments or different embodiments can be combined, and many other variations of the different aspects of the invention as described above exist, which are not provided in the details for the sake of brevity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the invention should be included within the protection scope of the invention.
Claims
1. A high-strength precipitation-hardening stainless steel welding wire alloy, characterized in that, By mass percentage, it comprises the following components: Cr: 10.5~11.8%, Ni: 8.5~9.0%, Mo: 4.75~6.25%, Co: 8.0~11.0%, Ti: 0.03~1.0%, Al: 1.00~1.65%, C≤0.015%, Mn≤0.01%, Si≤0.10%, P≤0.002%, S≤0.002%, Cu≤0.01%, Nb: 0.005~0.02%, B: 0.0015~0.0035%, N≤0.001%, O≤0.001%, Zr+Ce+La: 0.002~0.020%, with the balance being Fe and unavoidable impurities.
2. The ultra-high strength precipitation-hardening stainless steel welding wire alloy according to claim 1, characterized in that, In the ultra-high strength precipitation hardening stainless steel welding wire alloy, the Al content is 1.50~1.65% by mass percentage.
3. The ultra-high strength precipitation-hardening stainless steel welding wire alloy according to claim 1, characterized in that, In the ultra-high strength precipitation hardening stainless steel welding wire alloy, the Ti content is 0.03~0.08% by mass percentage.
4. A method for processing the ultra-high strength precipitation-hardening stainless steel welding wire alloy as described in any one of claims 1-3, characterized in that, Includes the following steps: S1. Perform VIM+VAR smelting according to the composition ratio of the ultra-high strength precipitation hardening stainless steel welding wire alloy to obtain consumable ingots, and perform homogenization treatment on the consumable ingots at 1200-1280℃. S2. The homogenized consumable ingot is hot forged and / or hot rolled to form a wire rod. The wire rod is then solution treated at a temperature of 900-950°C, held at the temperature, and then air-cooled. S3. The solution-treated wire blank is subjected to multiple cold drawing passes to obtain welding wire.
5. The processing method of the ultra-high strength precipitation hardening stainless steel welding wire alloy according to claim 4, characterized in that, In step S2, the diameter of the wire blank is in the range of 8.0~9.0mm.
6. The processing method of the ultra-high strength precipitation-hardening stainless steel welding wire alloy according to claim 4, characterized in that, In step S2, the heat treatment duration for homogenization is 20-28 hours, and the solution treatment duration is 3-8 hours.
7. The processing method of the ultra-high strength precipitation-hardening stainless steel welding wire alloy according to claim 4, characterized in that, In step S3, when the wire is cold-drawn to a diameter of 3.0~3.5mm, solution softening is performed at a temperature range of 900~950℃.
8. The ultra-high strength precipitation-hardening stainless steel welding wire alloy according to claim 4, characterized in that, The diameter of the welding wire is 0.8~1.6mm.
9. The ultra-high strength precipitation-hardening stainless steel welding wire alloy according to claim 4, characterized in that, In step S3, after multiple cold drawing passes, the surface is polished, and the surface roughness Ra of the welding wire is ≤0.4μm.
10. The ultra-high strength precipitation-hardening stainless steel welding wire alloy according to claim 4, characterized in that, The hardness of the welding wire in the solution-treated state is HRC 28~33.
Citation Information
Patent Citations
High-strength, notch-ductile precipitation-hardening stainless steel alloy
US5681528A
High-strength, notch-ductile precipitation-hardening stainless steel alloy and method of making
US5855844A
Ultra-high-strength precipitation-hardenable stainless steel and strip made therefrom
US6630103B2