A high-strength steel welding electrode for Q690 steel with a strength of 800MPa and its preparation method

By using a C-Mn-Si-Ni-Mo-Cr multi-element alloy system and a segmented drying process, the problems of insufficient weld strength, poor low-temperature toughness, and high diffusible hydrogen content in Q690 steel welding were solved, thereby improving the stability of high-strength steel welding electrodes and the welding quality.

CN123103252APending Publication Date: 2026-11-17SHANDONG JULI WELDING CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611546104.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-08
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

When welding Q690 steel with existing high-strength steel welding electrodes, the weld strength margin is insufficient, the low-temperature toughness is severely reduced, the diffusible hydrogen content is too high, and delayed cracks and coarse hardened structures are easily generated after welding.

Method used

The C-Mn-Si-Ni-Mo-Cr multi-element alloy system is adopted to precisely control the deoxidation, alloy strengthening and grain refinement of the weld. By strictly controlling the content of harmful impurities such as S and P, Ni element is combined to improve low-temperature toughness, Mo and Cr elements are used to strengthen precipitation, Mn and Si are used to achieve deoxidation and desulfurization, and segmented drying and gradient dehydration processes are adopted to reduce the content of diffusible hydrogen, and the mixing and pressure coating processes are optimized.

Benefits of technology

It improves the strength and toughness of the weld, reduces the diffusible hydrogen content, suppresses cold cracking defects, ensures the consistency of electrode formation and batch stability, has good arc stability, and produces a smooth weld without porosity, cracks, or slag inclusions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123103252A_ABST
    Figure CN123103252A_ABST
Patent Text Reader

Abstract

This invention provides an 800 MPa grade high-strength steel welding electrode for Q690 steel and its preparation method, relating to the field of welding materials. The welding electrode of this invention comprises a core and a coating covering the surface of the core. The coating comprises the following raw materials in parts by weight: marble 41-45 parts, fluorite 16-20 parts, potassium titanate 3-5 parts, quartz 6-8 parts, rutile 4-6 parts, reduced iron powder 7-10 parts, titanium dioxide 3-4 parts, ferrosilicon 6-7 parts, low-carbon ferromanganese 7-9 parts, nickel powder 3-5 parts, micro-carbon ferrochrome 1-2 parts, ferromolybdenum 1-2 parts, graphite 0.3-0.5 parts, soda ash 0.3-0.6 parts, cellulose 0.4-0.6 parts, and sodium carboxymethyl cellulose 0.2-0.4 parts. The welding electrode prepared by this invention matches the multi-element low-alloy high-strength and high-toughness system of Q690 steel, improving the problems of poor strength-toughness matching and weak crack resistance existing in existing welding electrodes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of welding materials technology, and in particular to an 800MPa grade high-strength steel welding electrode for Q690 steel and its preparation method. Background Technology

[0002] Q690 steel is a commonly used ultra-high strength low-alloy structural steel in engineering, widely used in the manufacture of heavy-duty steel structures. It places extremely high demands on the strength, toughness, crack resistance, and low-temperature performance of its welding materials. Currently, many high-strength steel welding electrodes are replaced with general-purpose high-strength electrodes. When welding Q690 high-strength steel, common problems include insufficient weld strength margin, severe low-temperature toughness degradation, high diffusible hydrogen content, and a tendency to develop delayed cracks and coarse hardened structures after welding. Summary of the Invention

[0003] This invention provides an 800MPa grade high-strength steel welding electrode for Q690 steel and its preparation method, which meets the welding requirements of Q690 steel.

[0004] This invention provides an 800MPa grade high-strength steel welding electrode for Q690 steel, comprising a core and a coating covering the surface of the core. The coating comprises the following raw materials in parts by weight: 41-45 parts marble, 16-20 parts fluorite, 3-5 parts potassium titanate, 6-8 parts quartz, 4-6 parts rutile, 7-10 parts reduced iron powder, 3-4 parts titanium dioxide, 6-7 parts ferrosilicon, 7-9 parts low-carbon ferromanganese, 3-5 parts nickel powder, 1-2 parts micro-carbon ferrochrome, 1-2 parts ferromolybdenum, 0.3-0.5 parts graphite, 0.3-0.6 parts soda ash, 0.4-0.6 parts cellulose, and 0.2-0.4 parts sodium carboxymethyl cellulose.

[0005] In one embodiment of the present invention, the welding core comprises the following components by mass percentage, based on the total mass of the welding core: C≤0.10%, Mn: 1.30%~1.80%, Si≤0.50%, Ni: 2.4%~3.2%, Mo: 0.25%~0.50%, Cr: 0.20%~0.40%, S≤0.020%, P≤0.025%, with the balance being Fe and unavoidable impurities.

[0006] In one embodiment of the present invention, the marble contains ≥96wt% calcium carbonate, the fluorite contains ≥95wt% calcium fluoride, the titanium dioxide contains ≥98wt% titanium dioxide, the ferrosilicon is 45 ferrosilicon, the low-carbon ferromanganese contains 77~79wt% manganese, the nickel powder contains ≥99wt% nickel, the micro-carbon ferrochrome contains 62~64wt% chromium, the ferromolybdenum contains 59~61wt% molybdenum, the graphite contains ≥99wt% carbon, and the soda ash contains ≥98wt% sodium carbonate.

[0007] In one embodiment of the present invention, the marble, the fluorite, the potassium titanate, the rutile, and the quartz have a particle size of 80-120 mesh.

[0008] In one embodiment of the present invention, the diameter of the welding core is 3.2 mm.

[0009] This invention also provides a method for preparing 800MPa grade high-strength steel welding electrodes for Q690 steel, comprising the following steps: Weigh each component of the medicinal peel according to the formula and mix them evenly to obtain the medicinal peel powder; A binder is added to the powdered drug coating, and the mixture is stirred until homogeneous to form a drug coating mixture; The flux mixture is pressed onto the surface of the welding core and dried to obtain the 800MPa grade high-strength steel welding electrode for Q690 steel.

[0010] In one embodiment of the present invention, the binder is a potassium-sodium composite water glass with a modulus of 2.6 to 2.9 and a Baume degree of 42 to 44 Be′.

[0011] In one embodiment of the present invention, the amount of the binder added is 18% to 24% of the total mass of the drug coating powder.

[0012] In one embodiment of the present invention, after adding a binder to the drug coating powder, the drug coating mixture is obtained by wet stirring for 15-20 minutes.

[0013] In one embodiment of the present invention, the drying process is carried out in stages. The first stage of drying is at a temperature of 80~100℃ and a drying time of 2~3h; the second stage of drying is at a temperature of 320~380℃ and a drying time of 1.5~2.5h.

[0014] The 800MPa high-strength steel welding electrode for Q690 steel of this invention precisely controls the deoxidation, alloy strengthening, and grain refinement mechanisms of the weld by using a C-Mn-Si-Ni-Mo-Cr multi-element alloy system with precise proportions. It avoids hot cracking caused by grain boundary segregation by strictly controlling the content of harmful impurities such as S and P. Ni element enhances low-temperature toughness, Mo and Cr elements strengthen the precipitation strengthening effect, and Mn and Si achieve deoxidation and desulfurization, ensuring weld purity and mechanical stability. The segmented drying and gradient dehydration process minimizes residual moisture in the coating, controls diffusible hydrogen content, and suppresses cold cracking defects in high-strength steel welding. Simultaneously, the optimized mixing and coating processes ensure consistent electrode formation and batch stability. Attached Figure Description

[0015] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with this application and, together with the description, serve to explain the principles of this application. It is obvious that the drawings described below are merely some embodiments of this application, and those skilled in the art can obtain other drawings based on these drawings without any inventive effort.

[0016] In the attached diagram: Figure 1 This is a flowchart illustrating the preparation process of 800MPa grade high-strength steel welding electrodes for Q690 steel, provided in an embodiment of the present invention. Detailed Implementation

[0017] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments. Various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.

[0018] In the following description, numerous details are explored to provide a more thorough explanation of embodiments of the invention. However, it will be apparent to those skilled in the art that embodiments of the invention may be practiced without these specific details. In other embodiments, well-known structures and devices are shown in block diagram form rather than in detail to avoid obscuring embodiments of the invention.

[0019] In this document, when referring to numerical ranges, unless otherwise specified, the distribution of selectable values ​​within a numerical range is considered continuous, including the two endpoints of the range (i.e., the minimum and maximum values), and every value between these two endpoints. When multiple numerical ranges are provided to describe a feature or property, these numerical ranges can be combined.

[0020] This invention provides a high-strength steel welding electrode for Q690 steel with a grade of 800MPa. The electrode includes a core and a coating covering the surface of the core. The coating comprises the following raw materials in parts by weight: 41-45 parts marble, 16-20 parts fluorite, 3-5 parts potassium titanate, 6-8 parts quartz, 4-6 parts rutile, 7-10 parts reduced iron powder, 3-4 parts titanium dioxide, 6-7 parts ferrosilicon, 7-9 parts low-carbon ferromanganese, 3-5 parts nickel powder, 1-2 parts micro-carbon ferrochrome, 1-2 parts ferromolybdenum, 0.3-0.5 parts graphite, 0.3-0.6 parts soda ash, 0.4-0.6 parts cellulose, and 0.2-0.4 parts sodium carboxymethyl cellulose.

[0021] The functions of each component in the herbal peel of this application are as follows: Marble: It mainly plays the role of slag and gas generation. When heated during the welding process, marble decomposes into CO2 gas and CaO. CaO participates in the molten slag to form an alkaline slag system, and CO2 forms a protective gas to isolate the air and prevent the molten pool from oxidizing.

[0022] Fluorite: Its main component is CaF2; it is used for slag formation and hydrogen removal. - It can combine with free H in the molten pool to generate HF gas, reducing the diffusible hydrogen content in the weld metal. It is a key raw material for high-strength steel welding electrodes to suppress delayed cracking, isolate air and control the chemical composition of the weld metal, ensure the mechanical properties of the weld metal, and reduce the generation of defects such as porosity, cracks and inclusions.

[0023] Potassium titanate: A strong arc stabilizer that refines molten droplets and improves AC arc ignition performance. Potassium's low ionization potential enhances arc continuity, reduces arc interruption, and improves re-ignition performance; the high-temperature TiO2 formation participates in slag formation, refining molten droplets and reducing spatter; it also helps regulate slag surface tension, resulting in finer weld ripples.

[0024] Quartz: an acidic slag-forming regulator and slag conditioner, used to adjust the melting point, viscosity and solidification range of molten slag, balance the high alkalinity of marble and fluorite, and prevent slag inclusions caused by excessively rapid solidification of molten slag.

[0025] Rutile: An improved slag-forming and arc-stabilizing agent. Its component TiO2 has a moderate melting point, which stabilizes the electric arc, refines weld ripples, and improves surface finish; it improves vertical and overhead welding formation and reduces undercut defects; it works synergistically with titanium dioxide to regulate the solidification characteristics of molten slag.

[0026] Reduced iron powder: a plasticizer, a conductive and thermally conductive agent, and improves deposition efficiency. It enhances the electrical and thermal conductivity of the flux coating, ensures uniform arc heat distribution, and reduces core burn-off; it increases deposition speed and improves welding efficiency; and it balances the thermal expansion coefficient of the flux coating, reducing cracking and peeling during drying and welding.

[0027] Titanium dioxide: refines slag, improves weld smoothness, and acts as an arc stabilizing agent. Ultrafine TiO2 particles are finely dispersed in the slag, reducing slag surface tension and ensuring clean slag removal without sticking; it also helps stabilize the arc and improves the formation of thin-walled and narrow-groove welds; when combined with rutile, it reduces orange peel texture in welds.

[0028] Ferrosilicon: a composite deoxidizer and solid solution strengthening alloying agent. Si has a strong affinity for O in the molten pool, preferentially deoxidizing to form SiO2 which enters the slag, reducing oxide inclusions; after deoxidation, some Si transitions into the weld, and solid solution strengthening improves tensile strength; it forms a Si-Mn combined deoxidation with ferromanganese, and the deoxidation efficiency is much higher than that of a single deoxidizing element.

[0029] Low-carbon ferromanganese: deoxidizing, desulfurizing, and a primary strengthening alloying agent. A strong desulfurizing element, it generates MnS which enters the slag, eliminating S-induced intergranular hot cracks; it works synergistically with ferrosilicon for deep deoxidation, purifying the deposited metal; Mn can be transferred in large quantities into the weld, expanding the austenite region and improving strength and low-temperature toughness, forming the basis for 800MPa-level strength; the low-carbon grade avoids the hardening of the weld and increased tendency for cold cracking caused by increased carbon content.

[0030] Nickel powder: a core alloying element for low-temperature toughening, while also improving strength. Ni expands the austenite stability range, refines the acicular ferrite structure of the weld, significantly improves the impact energy at -40℃, and addresses the problem of balancing strength and toughness in high-strength steel welds. Solid solution strengthening helps achieve a tensile strength of 800MPa.

[0031] Microcarbon ferrochrome: Precipitation strengthening, corrosion resistance, and tempering stabilizing element. Cr transitions to the weld to form fine carbides, precipitation strengthening and improving tensile and yield strength; it also improves weld hardenability and tempering resistance, and the strength does not decrease after post-weld stress relief heat treatment; microcarbon specifications strictly control C to avoid high-carbon Cr inducing hardened martensite and reducing toughness.

[0032] Ferromolybdenum: A high-strength, toughening, and temper brittle-resistant core alloy. Mo is a strong carbide-forming element, and dispersed carbides significantly improve weld strength and creep resistance; inhibit the formation of coarse bainite and martensite, refining the microstructure; and counteract the low-temperature embrittlement caused by the addition of Cr alone.

[0033] Graphite: Provides trace amounts of carbon addition and assists in conductivity and deoxidation. It slightly replenishes carbon in the weld to ensure the minimum strength; it also improves the conductivity of the flux coating, making arc ignition easier.

[0034] Soda ash: a low-ionization arc stabilizer and paste modifier. Na element improves arc ionization, resulting in a more stable arc when welding with AC welding machines; it adjusts the plasticity of the paste and optimizes pressure coating molding; high-temperature decomposition generates trace amounts of gas to assist in protection.

[0035] Cellulose: an organic plasticizer, gas generator, and coating modifier. In the preparation stage, it improves the plasticity and lubricity of the coating, ensuring uniform coating thickness and no cracks during coating. High-temperature decomposition produces small amounts of CO and CO2, which help protect the molten pool. When combined with CMC, it enhances the toughness of the coating after drying, making it less prone to peeling during transport.

[0036] Sodium carboxymethyl cellulose (CMC): An organic flexible binder and plasticizer. An ultrafine polymer that bridges and binds powder particles, improving the overall strength of the dried drug coating and reducing powder loss due to impact; significantly improving the rheological properties of the ointment, resulting in smooth application and high concentricity; and reducing the probability of cracking during drying.

[0037] In one embodiment of the present invention, the welding core comprises the following components by mass percentage, based on the total mass of the welding core: C≤0.10%, Mn: 1.30%~1.80%, Si≤0.50%, Ni: 2.4%~3.2%, Mo: 0.25%~0.50%, Cr: 0.20%~0.40%, S≤0.020%, P≤0.025%, with the balance being Fe and unavoidable impurities.

[0038] In one embodiment of the present invention, the marble contains ≥96wt% calcium carbonate, the fluorite contains ≥95wt% calcium fluoride, the titanium dioxide contains ≥98wt% titanium dioxide, the ferrosilicon is 45 ferrosilicon, the low-carbon ferromanganese contains 77~79wt% manganese, the nickel powder contains ≥99wt% nickel, the micro-carbon ferrochrome contains 62~64wt% chromium, the ferromolybdenum contains 59~61wt% molybdenum, the graphite contains ≥99wt% carbon, and the soda ash contains ≥98wt% sodium carbonate.

[0039] In one embodiment of the present invention, the marble, fluorite, potassium titanate, rutile, and quartz have a particle size of 80-120 mesh.

[0040] Please see Figure 1 The present invention also provides a method for preparing 800MPa grade high-strength steel welding electrodes for Q690 steel, comprising the following steps: S1. Weigh each component of the medicinal peel according to the ratio and mix them evenly to obtain the medicinal peel powder; S2. Add binder to the drug coating powder and stir evenly to form a drug coating mixture; S3. Press the coating mixture onto the surface of the welding core and dry it to obtain a high-strength steel welding electrode for Q690 steel with a grade of 800MPa.

[0041] In step S1, the coating comprises the following raw materials in parts by weight: 41-45 parts marble, 16-20 parts fluorite, 3-5 parts potassium titanate, 6-8 parts quartz, 4-6 parts rutile, 7-10 parts reduced iron powder, 3-4 parts titanium dioxide, 6-7 parts ferrosilicon, 7-9 parts low-carbon ferromanganese, 3-5 parts nickel powder, 1-2 parts micro-carbon ferrochrome, 1-2 parts ferromolybdenum, 0.3-0.5 parts graphite, 0.3-0.6 parts soda ash, 0.4-0.6 parts cellulose, and 0.2-0.4 parts sodium carboxymethyl cellulose.

[0042] In step S2, after adding a binder to the drug coating powder, a drug coating mixture is obtained by wet stirring for 15-20 minutes. It should be noted that wet stirring refers to adding potassium-sodium composite water glass to the drug coating powder and then stirring the resulting mixture to ensure the binder is uniformly wetted and dispersed among the powder particles. The binder used is potassium-sodium composite water glass with a modulus of 2.6-2.9 and a Baume degree of 42-44 Be′. The amount of binder added is 18%-24% of the total mass of the drug coating powder.

[0043] In step S3, based on the total mass of the welding core, the welding core comprises the following components by mass percentage: C ≤ 0.10%, Mn: 1.30%~1.80%, Si ≤ 0.50%, Ni: 2.4%~3.2%, Mo: 0.25%~0.50%, Cr: 0.20%~0.40%, S ≤ 0.020%, P ≤ 0.025%, with the balance being Fe and unavoidable impurities. The diameter of the welding core is, for example, 3.2 mm. The coating process employs conventional coating equipment and methods, such as a commonly used coating machine, which will not be elaborated here, ensuring uniform coating thickness and concentricity deviation ≤ 0.1 mm. Drying is performed in stages: the first stage drying temperature is 80~100℃, and the drying time is 2~3 hours; the second stage drying temperature is 320~380℃, and the drying time is 1.5~2.5 hours, to thoroughly remove crystal water and adsorbed water and inhibit the generation of diffusing hydrogen. After drying, the electrodes are allowed to cool naturally to room temperature in the furnace to avoid cracking due to sudden cooling. In some embodiments, the cooled electrodes are ground, straightened, and visually inspected to remove defective products with peeling coating, eccentricity, or cracks.

[0044] In some embodiments, the process further includes a core pretreatment step and a flux powder pretreatment step before pressure coating.

[0045] The pretreatment steps for the welding core are as follows: straighten, grind, degrease, and derust the welding core in sequence to remove surface oxide scale and impurities, and set it aside for later use.

[0046] The pretreatment steps for the pharmaceutical coating powder are as follows: The solid raw materials—marble, fluorite, potassium titanate, rutile, and quartz—are dried, crushed, and sieved through an 80-120 mesh sieve to remove lumps and large particles. It should be noted that sieving through an 80-120 mesh sieve means using both 80-mesh and 120-mesh sieves to collect the powder that passes through the 80-mesh sieve but not the 120-mesh sieve, resulting in a powder with a particle size of 80-120 mesh. This sieving process removes lumps, excessively large particles, and overly fine powder, which helps improve the mixing uniformity and coating stability of the pharmaceutical coating powder.

[0047] In some embodiments, during mixing, the sieved marble, fluorite, potassium titanate, rutile, and quartz solid raw materials are first dry-mixed for 10-15 minutes, then reduced iron powder, titanium dioxide, ferrosilicon, low-carbon ferromanganese, nickel powder, ferromolybdenum, micro-carbon ferrochrome, and graphite powder are added in sequence and dry-mixed for another 20-30 minutes. Finally, soda ash, cellulose, and sodium carboxymethyl cellulose binder are added and stirred evenly to obtain the drug coating powder.

[0048] The technical solution of the present invention will be described in detail below through several specific embodiments. Unless otherwise stated, the raw materials and reagents used in the following embodiments are all commercially available products, or can be prepared by conventional methods in the art, and the instruments used in the embodiments are all commercially available.

[0049] Example 1 The Q690 steel 800MPa grade high-strength steel welding electrode of this embodiment includes a core and a coating covering the surface of the core. The coating includes the following components and their respective weight parts: marble 43 parts, fluorite 18 parts, potassium titanate 4 parts, quartz 7 parts, rutile 5 parts, reduced iron powder 8 parts, titanium dioxide 3 parts, ferrosilicon 7 parts, low-carbon ferromanganese 8 parts, nickel powder 4 parts, micro-carbon ferrochrome 1 part, ferromolybdenum 1 part, graphite 0.4 parts, soda ash 0.4 parts, cellulose 0.5 parts, and sodium carboxymethyl cellulose 0.3 parts. Based on the total mass of the core, the core includes the following components by mass percentage: C 0.06%, Mn 1.30%, Si 0.30%, Ni 2.4%, Mo 0.25%, Cr 0.20%, S 0.010%, P 0.015%, with the balance being Fe and unavoidable impurities.

[0050] The preparation method of the 800MPa grade high-strength steel welding electrode for Q690 steel in this embodiment is as follows: The oxide scale on the welding core was removed by mechanical grinding, ultrasonically cleaned with anhydrous ethanol for 8 minutes, and then dried at 100℃ for later use. Marble, fluorite, potassium titanate, rutile, and quartz were dried at 130℃ for 2.5 hours, crushed, and passed through a 100-mesh sieve. The above inorganic powders were first dry-mixed at 250 r / min for 12 minutes, then alloy powders were added and dry-mixed for another 25 minutes. Finally, additives such as soda ash, cellulose, and sodium carboxymethyl cellulose were added and stirred for 6 minutes to obtain a uniformly mixed coating powder. A binder was added to the coating powder and wet-stirred for 15 minutes to form a coating mixture. The coating mixture was pressed onto the surface of the welding core at a speed of 10 m / min. Then, it was pre-baked at 90℃ for 2.5 hours and dried at 350℃ for 2 hours to obtain a high-strength steel welding electrode for Q690 steel with a grade of 800 MPa.

[0051] In this embodiment, the core diameter is 3.2 mm, the binder is potassium-sodium composite water glass with a modulus of 2.7 and a Baume degree of 42Be′, and the amount of water glass binder added is 21% of the total mass of the coating powder.

[0052] The electrode test results in this embodiment are as follows: tensile strength of deposited metal 835 MPa, yield strength 765 MPa, average impact energy at -40℃ 78 J, and diffusible hydrogen content 4.2 mL / 100g; the welding process is characterized by stable arc, minimal spatter, thorough slag removal, smooth weld formation, and absence of porosity, cracks, or slag inclusions.

[0053] Example 2 The Q690 steel 800MPa grade high-strength steel welding electrode of this embodiment includes a core and a coating covering the surface of the core. The coating includes the following components and their respective weight parts: marble 41 parts, fluorite 16 parts, potassium titanate 3 parts, quartz 6 parts, rutile 4 parts, reduced iron powder 7 parts, titanium dioxide 3 parts, ferrosilicon 6 parts, low-carbon ferromanganese 7 parts, nickel powder 3 parts, micro-carbon ferrochrome 1 part, ferromolybdenum 1 part, graphite 0.3 parts, soda ash 0.3 parts, cellulose 0.4 parts, and sodium carboxymethyl cellulose 0.2 parts. Based on the total mass of the core, the core includes the following components by mass percentage: C 0.10%, Mn 1.80%, Si 0.50%, Ni 3.2%, Mo 0.50%, Cr 0.40%, S 0.020%, P 0.025%, with the balance being Fe and unavoidable impurities.

[0054] The difference between the preparation method of this embodiment and that of Example 1 is as follows: the inorganic powder is first dry-mixed for 10 minutes, then the alloy powder is added and dry-mixed for another 20 minutes, followed by wet stirring for 20 minutes. The first stage of drying is at 80°C for 2 hours, and the second stage of drying is at 320°C for 1.5 hours. The modulus of the potassium-sodium composite water glass is 2.6 and the Baume degree is 42Be′. The amount of water glass binder added is 18% of the total mass of the drug coating powder.

[0055] The electrode test results in this embodiment are as follows: tensile strength of deposited metal 821MPa, yield strength 722MPa, average impact energy at -40℃ 75J, diffusible hydrogen content 4.5mL / 100g. All performance indicators meet the standards, and the electrode exhibits excellent stability under heavy loads.

[0056] Example 3 The Q690 steel 800MPa grade high-strength steel welding electrode of this embodiment includes a core and a coating covering the surface of the core. The coating includes the following components and their respective weight parts: marble 45 parts, fluorite 20 parts, potassium titanate 5 parts, quartz 8 parts, rutile 6 parts, reduced iron powder 10 parts, titanium dioxide 4 parts, ferrosilicon 7 parts, low-carbon ferromanganese 9 parts, nickel powder 5 parts, micro-carbon ferrochrome 2 parts, ferromolybdenum 2 parts, graphite 0.5 parts, soda ash 0.6 parts, cellulose 0.6 parts, and sodium carboxymethyl cellulose 0.4 parts. Based on the total mass of the core, the core includes the following components by mass percentage: C 0.08%, Mn 1.55%, Si 0.25%, Ni 2.8%, Mo 0.375%, Cr 0.30%, S 0.010%, P 0.0125%, with the balance being Fe and unavoidable impurities.

[0057] The difference between the preparation method of this embodiment and that of Example 1 is as follows: the inorganic powder is first dry-mixed for 15 minutes, then the alloy powder is added and dry-mixed for another 30 minutes, followed by wet stirring for 18 minutes. The first stage of drying is at 100°C for 3 hours, and the second stage of drying is at 380°C for 2.5 hours. The modulus of the potassium-sodium composite water glass is 2.9 and the Baume degree is 44Be′. The amount of water glass binder added is 24% of the total mass of the drug coating powder.

[0058] The electrode test results in this embodiment are as follows: tensile strength of deposited metal 841MPa, yield strength 752MPa, average impact energy at -40℃ 80J, diffusible hydrogen content 4.5mL / 100g, all performance indicators meet the standards, and the electrode exhibits excellent stability under heavy load welding.

[0059] Example 4 The Q690 steel 800MPa grade high-strength steel welding electrode of this embodiment includes a core and a coating covering the surface of the core. The coating includes the following components and their respective weight parts: marble 44 parts, fluorite 17 parts, potassium titanate 5 parts, quartz 6 parts, rutile 4 parts, reduced iron powder 8 parts, titanium dioxide 4 parts, ferrosilicon 7 parts, low-carbon ferromanganese 7 parts, nickel powder 5 parts, micro-carbon ferrochrome 1 part, ferromolybdenum 2 parts, graphite 0.5 parts, soda ash 0.4 parts, cellulose 0.4 parts, and sodium carboxymethyl cellulose 0.2 parts. Based on the total mass of the core, the core includes the following components by mass percentage: C 0.07%, Mn 1.65%, Si 0.40%, Ni 3.0%, Mo 0.40%, Cr 0.35%, S 0.015%, P 0.020%, with the balance being Fe and unavoidable impurities.

[0060] The preparation method of this embodiment differs from that of Example 1 in that: the inorganic powder is first dry-mixed for 12.5 min, then the alloy powder is added and dry-mixed for another 25 min, followed by wet stirring for 20 min; the first stage drying temperature is 90℃ and the time is 2.5 h; the second stage drying temperature is 350℃ and the time is 2 h; the modulus of the potassium-sodium composite water glass is 2.75 and the Baume degree is 43Be′; and the amount of water glass binder added is 21% of the total mass of the drug coating powder.

[0061] The electrode test results in this embodiment are as follows: tensile strength of deposited metal 834MPa, yield strength 747MPa, average impact energy at -40℃ 74J, diffusible hydrogen content 4.4mL / 100g. All performance indicators meet the standards, and the electrode exhibits excellent stability under heavy loads.

[0062] The components of the flux coating in the 800MPa grade high-strength steel welding electrodes for Q690 steel in Examples 1-4 are shown in Table 1. The 800MPa welding electrodes for Q690 steel of this invention were used for all-position welding. Welding process tests, weld metal chemical composition analysis, and weld metal mechanical property tests were conducted on the welding electrodes provided in Examples 1-4 according to GB / T 32533-2016. The composition of the deposited metal is shown in Table 2, the mechanical properties of the deposited metal are shown in Table 3, and the welding process performance is shown in Table 4.

[0063] Table 1: Coating composition of 800MPa grade high-strength steel welding electrodes for Q690 steel in Examples 1 to 4

[0064] Table 2: Chemical composition of weld metal from 800MPa grade high-strength steel welding electrodes for Q690 steel in Examples 1 to 4

[0065] Table 3: Properties of weld metal from 800MPa grade high-strength steel welding electrodes for Q690 steel in Examples 1 to 4

[0066] Table 4: Process performance of 800MPa grade high-strength steel welding electrodes for Q690 steel in Examples 1 to 4

[0067] As can be seen from Tables 3 and 4, the 800MPa grade high-strength steel welding electrode for Q690 steel of the present invention can be used for all-position welding. During welding, the arc is stable, spatter is small, and the welding process is good in terms of forming and slag removal. The deposited metal has good tensile strength, low-temperature toughness and crack resistance.

[0068] The 800MPa grade high-strength steel welding electrode for Q690 steel of this invention uses a C-Mn-Si-Ni-Mo-Cr alloy system, combined with an alkaline ultra-low hydrogen coating formula, to precisely control the deoxidation, alloy strengthening, and grain refinement mechanisms of the weld. Simultaneously, the electrode's segmented drying and gradient mixing processes are optimized, reducing the diffusible hydrogen content in the weld, refining the microstructure, and balancing strength and toughness. Therefore, this invention effectively overcomes some practical problems in the prior art, thus possessing high utilization value and practical significance.

[0069] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the invention. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in the present invention should still be covered by the claims of the present invention.

Claims

1. An 800MPa grade high strength steel electrode for Q690 steel, characterized in that, The coating includes a welding core and a flux coating covering the surface of the welding core. The flux coating comprises the following raw materials in parts by weight: 41-45 parts marble, 16-20 parts fluorite, 3-5 parts potassium titanate, 6-8 parts quartz, 4-6 parts rutile, 7-10 parts reduced iron powder, 3-4 parts titanium dioxide, 6-7 parts ferrosilicon, 7-9 parts low-carbon ferromanganese, 3-5 parts nickel powder, 1-2 parts micro-carbon ferrochrome, 1-2 parts ferromolybdenum, 0.3-0.5 parts graphite, 0.3-0.6 parts soda ash, 0.4-0.6 parts cellulose, and 0.2-0.4 parts sodium carboxymethyl cellulose.

2. The 800MPa grade high-strength steel electrode for Q690 steel according to claim 1, characterized in that, Based on the total mass of the welding core, the welding core comprises the following components by mass percentage: C ≤ 0.10%, Mn: 1.30%~1.80%, Si ≤ 0.50%, Ni: 2.4%~3.2%, Mo: 0.25%~0.50%, Cr: 0.20%~0.40%, S ≤ 0.020%, P ≤ 0.025%, with the balance being Fe and unavoidable impurities. 3.The 800 MPa grade high-strength steel electrode for Q690 steel according to claim 1, characterized in that, The marble contains ≥96wt% calcium carbonate, the fluorite contains ≥95wt% calcium fluoride, the titanium dioxide contains ≥98wt% titanium dioxide, the ferrosilicon is 45% ferrosilicon, the low-carbon ferromanganese contains 77-79wt% manganese, the nickel powder contains ≥99wt% nickel, the micro-carbon ferrochrome contains 62-64wt% chromium, the ferromolybdenum contains 59-61wt% molybdenum, the graphite contains ≥99wt% carbon, and the soda ash contains ≥98wt% sodium carbonate.

4. The 800 MPa grade high-strength steel electrode for Q690 steel according to claim 1, characterized in that, The marble, fluorite, potassium titanate, rutile, and quartz have a particle size of 80-120 mesh.

5. The 800 MPa grade high-strength steel electrode for Q690 steel according to claim 1, characterized in that, The diameter of the welding core is 3.2 mm.

6. A method for preparing the 800 MPa grade high-strength steel electrode for the Q690 steel according to any one of claims 1-5, characterized in that, Includes the following steps: Weigh each component of the medicinal peel according to the formula and mix them evenly to obtain the medicinal peel powder; A binder is added to the powdered drug coating, and the mixture is stirred until homogeneous to form a drug coating mixture; The flux mixture is pressed onto the surface of the welding core and dried to obtain the 800MPa grade high-strength steel welding electrode for Q690 steel.

7. The preparation method according to claim 6, characterized in that, The binder is a potassium-sodium composite water glass with a modulus of 2.6 to 2.9 and a Baume degree of 42 to 44 Be′.

8. The preparation method according to claim 6, characterized in that, The amount of binder added is 18% to 24% of the total mass of the drug coating powder.

9. The preparation method according to claim 6, characterized in that, After adding a binder to the drug coating powder, the drug coating mixture is prepared by wet stirring for 15-20 minutes.

10. The preparation method according to claim 6, characterized in that, The drying process is carried out in stages. The first stage of drying is at a temperature of 80~100℃ and a drying time of 2~3 hours; the second stage of drying is at a temperature of 320~380℃ and a drying time of 1.5~2.5 hours.