A method for making coated abrasives using black corundum

By performing multi-stage modification and composite treatment on black fused alumina, combined with high-voltage electrostatic sand planting and stepped temperature curing processes, the problems of poor adhesion and insufficient durability of black fused alumina in the field of coated abrasives have been solved, achieving efficient grinding and high-precision polishing, and avoiding thermal burns on the workpiece.

CN123103535APending Publication Date: 2026-11-17ZHENGZHOU YEDA HIGH TECH MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611335546.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-31
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The application of black corundum in coated abrasives suffers from several problems, including numerous impurities on the abrasive surface, poor adhesion to resin, insufficient durability, high brittleness of traditional phenolic resins, and a lack of complete production processes.

Method used

Modified black corundum was prepared by alkali washing to remove impurities, ferrous salt passivation and sealing, and double-layer coating with composite coupling agent. It was then compounded with calcined brown corundum and single-crystal corundum, and combined with high-voltage electrostatic vertical sand planting process and three-stage stepped temperature rise curing to form a composite abrasive. Finally, a modified phenolic resin composite and a functional super coating were applied to obtain a coated abrasive.

Benefits of technology

It improves the interfacial bonding strength and durability of the abrasive, adapts to different working conditions, constructs internal heat dissipation channels, eliminates porosity and internal stress, improves grinding efficiency and polishing accuracy, and avoids thermal burns to the workpiece.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention provides a method for manufacturing coated abrasives using black corundum, belonging to the field of wear-resistant materials technology. First, black corundum undergoes a series of processes including alkaline washing to remove impurities, ferrous salt passivation and sealing, and double-layer coating with a composite coupling agent to obtain modified black corundum. Then, it is compounded with calcined brown corundum and single-crystal corundum to obtain a composite abrasive. A primer is applied to a pre-treated substrate, followed by sand planting and pre-baking for shaping. Next, a top coat is applied to the abrasive layer, wrapping the roots of the abrasive grains, filling gaps, and compacting and leveling. After vacuum pre-curing and degassing, the adhesive layer undergoes three-stage stepped heating for curing, releasing resin internal stress and achieving integrated bonding of the primer, top coat, and abrasive. Finally, two layers of functional supercoating are applied, followed by post-treatment to obtain the final product. This invention improves interfacial bonding through multi-stage modification of the abrasive, balances grinding efficiency and polishing precision with the ternary composite abrasive, dissipates heat to prevent workpiece thermal burns, and reduces porosity and improves production stability through vacuum pre-curing and stepped heating processes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of wear-resistant materials technology, and specifically to a method for making coated abrasives using black corundum. Background Technology

[0002] Coated abrasives, as an important grinding and polishing tool, are widely used in the surface processing of materials such as metals, wood, ceramics, and plastics. With the continuous improvement of automation in modern industrial production, coated abrasives, as key consumables of automated production equipment, are seeing their market demand increase year by year, and their share in the overall abrasive market is becoming increasingly significant.

[0003] Black corundum, as a high-performance flexible wear-resistant material, possesses unique physicochemical properties such as moderate hardness, high toughness, and strong self-sharpening ability. Especially in the polishing of metal materials such as stainless steel, black corundum plays an irreplaceable role, effectively reducing heat generation during processing, preventing surface burns or color differences, and resulting in a uniform, bright bluish-green surface with high gloss.

[0004] Currently, black fused alumina is widely used in resin abrasives, wear-resistant and anti-slip road paving, and other fields. However, although black fused alumina is mature in the fields of free grinding and resin abrasives, its application in coated abrasives still faces significant technical bottlenecks: First, the abrasive surface has many impurities and poor adhesion to resin, making it prone to shedding; second, pure black fused alumina lacks durability; third, traditional phenolic resin is brittle and not suitable for repeated bending of abrasive belts; and fourth, there is a lack of complete production processes suitable for black fused alumina. Summary of the Invention

[0005] The purpose of this invention is to provide a method for manufacturing coated abrasives using black corundum, so as to solve the problems mentioned in the background art.

[0006] To achieve the above objectives, the present invention provides the following technical solution: A method for making coated abrasives using black corundum includes the following steps: S1. Black corundum is subjected to alkali washing to remove impurities, ferrous salt passivation and sealing, and double-layer coating with composite coupling agent to obtain modified black corundum. S2. Modified black corundum is combined with calcined brown corundum and single-crystal corundum to obtain composite abrasive; S3. Apply 20~30μm epoxy resin primer to the pretreated substrate surface, and implant composite abrasive using high voltage electrostatic vertical sand planting process. After sand planting is completed, pre-bake and shape it so that the abrasive grains are initially fixed to the primer layer. S4. Apply modified phenolic resin evenly to the surface of the shaped abrasive layer to completely wrap the root of the abrasive grains and fill the gaps between the abrasive grains, and then compact and level the resin layer. S5. First, perform negative pressure vacuum pre-curing to remove air bubbles from the adhesive layer, then perform three-stage stepped temperature rise curing to eliminate internal stress in the resin and achieve integrated curing and bonding of the base adhesive, top adhesive and abrasive. S6. Two functional super coating layers are sequentially applied to the surface of the abrasive layer. After aging and curing, and cutting into strips, finished abrasive cloth, sandpaper, or closed-loop abrasive belt are obtained.

[0007] Preferably, the alkaline washing and impurity removal in S1 involves immersing P-grade black corundum in a 4%–6% sodium hydroxide aqueous solution at room temperature for 10–20 minutes, rinsing with pure water, and then drying at 100–110°C.

[0008] Preferably, the passivation sealing in S1 involves immersing the black corundum, after alkaline washing and impurity removal, in a 0.3%–0.8% ferrous sulfate aqueous solution at room temperature for 25–35 minutes to generate a dense passivation film in the micropores of the iron oxide, followed by drying.

[0009] Preferably, the composite coupling agent in S1 comprises, by weight ratio, KH-550 silane coupling agent: KR-TTS titanate coupling agent = 2:1, and the total amount of composite coupling agent added is 0.8% to 1.5% of the mass of black corundum. The coating is carried out by dry stirring for 15 to 25 minutes and then cured and dried at 115 to 130°C.

[0010] Preferably, in S2, the compound ratio of modified black corundum, calcined brown corundum, and single-crystal corundum, by weight, includes any one of the following: Coarsely ground P60~P120: 55~65 parts modified black corundum, 30~40 parts calcined brown corundum, and 3~8 parts single crystal corundum; Medium-milled P150~P220: 65~75 parts modified black corundum, 20~30 parts calcined brown corundum, and 2~6 parts single crystal corundum; Fine polishing P240~P600: 75~85 parts modified black corundum, 10~20 parts calcined brown corundum, and 1~5 parts single crystal corundum.

[0011] Preferably, the substrate in S3 is a fabric-based, paper-based, or non-woven fabric-based material, and the pretreatment is degreasing, napping, and dehumidification.

[0012] Preferably, in S3, the epoxy resin primer comprises, by weight, 100 parts of liquid epoxy resin, 28-32 parts of polyamide curing agent, 4-6 parts of wetting and leveling agent, 7-9 parts of viscosity modifier, and 3-7 parts of nano thermally conductive filler.

[0013] Preferably, the polyamide curing agent is selected from at least one of type 650 and type 651 epoxy polyamide curing agents; the wetting and leveling agent is selected from any one of organosilicon leveling agents BYK-333, BYK-358, and DIG 450; the viscosity modifier is selected from at least one of fumed silica, hydrogenated castor oil, and polyamide wax thixotropic agent; and the nano thermally conductive filler comprises, by weight, nano aluminum nitride: fumed silica = 4:1.

[0014] Preferably, in S4, the modified phenolic composite adhesive comprises, by weight, 100 parts of modified phenolic resin, 8-12 parts of wood powder, 5-8 parts of light calcium carbonate, 3-5 parts of resin toughening agent, and 2-5 parts of nano-thermal conductive filler.

[0015] The nano-thermal conductive filler in the epoxy resin primer and modified phenolic resin composite components is the same material with a powder particle size of 20-80nm. It has high dispersion and good insulation properties, and can build a uniform micro-thermal conductive network in the resin system to quickly dissipate grinding heat and effectively avoid workpiece polishing burns and high-temperature aging and desanding of the adhesive layer.

[0016] Preferably, the modified phenolic resin is prepared by introducing acrylonitrile rubber flexible segments into the phenolic condensation stage of thermosetting phenolic resin, and the mass ratio of thermosetting phenolic resin to acrylonitrile rubber is 100:10. Through modification, the rigidity and brittleness of pure phenolic resin are weakened, and the bending toughness, peel strength and abrasive encapsulation and anchoring ability of the adhesive layer are greatly improved, making it suitable for repeated bending conditions of flexible coated abrasives.

[0017] Preferably, the wood powder is made from degreased poplar or pine wood chips through crushing, sieving, and impurity removal, with a mesh size of 180-300 mesh, a moisture content of ≤2%, an ash content of ≤3%, and no hard sand particles or coarse fibers. It is used to adjust the porosity of the adhesive layer, reduce the shrinkage rate of the adhesive layer, and improve the flexibility and bending resistance of the coated abrasive, while effectively controlling production costs. The resin toughening agent is selected from at least one of liquid nitrile rubber, epoxidized soybean oil, and polyurethane toughening agent, which can effectively improve the defects of high brittleness and easy cracking after curing of modified phenolic resin, and improve the impact resistance and bending fatigue resistance of the adhesive layer.

[0018] Preferably, in step S5, the negative pressure vacuum pre-curing is performed at a negative pressure of -0.06 to -0.09 MPa, a temperature of 60 to 70°C, and a holding time of 20 to 30 minutes to remove tiny air bubbles from the adhesive solution.

[0019] Preferably, in S5, the three-stage stepped heating and curing process is as follows: First stage pre-baking: Keep warm at 70-80℃ for 30-40 minutes; Second stage of medium-temperature crosslinking: heat treatment at 105-115℃ for 50-70 min; The third stage is high-temperature curing: holding at 140-150℃ for 80-100 minutes; The heating rate is 3-5℃ / min, and after curing, it should be allowed to cool naturally to room temperature.

[0020] Preferably, in S6, the functional super coating is sequentially coated with a zinc stearate dry powder anti-clogging coating and a water-based polytetrafluoroethylene lubricating coating.

[0021] The beneficial effects of the above-described technical solution of the present invention are as follows: 1. Multi-level surface modification solves abrasive interface bonding defects and significantly improves product durability; 2. The ternary gradient abrasive system is suitable for all particle size conditions, balancing grinding efficiency and polishing precision. 3. Nano-thermal conductive modified adhesive layer to construct internal heat dissipation channels and eliminate workpiece thermal burn defects; 4. The vacuum pre-curing + stepped heating composite process eliminates pores and internal stress, resulting in stronger process stability. Detailed Implementation

[0022] The following embodiments are provided to better understand the present invention and are not limited to the preferred embodiments described. They do not constitute a limitation on the content and scope of protection of the present invention. Any product that is the same as or similar to the present invention, derived by any person under the guidance of the present invention or by combining the features of the present invention with other prior art, falls within the protection scope of the present invention.

[0023] For experiments not specifically described in the examples, the procedures or conditions should be followed according to the conventional experimental procedures described in the literature in this field. Reagents or instruments whose manufacturers are not specified are all commercially available conventional reagent products. Example 1

[0024] A method for making coated abrasives using black corundum includes the following steps: S1. Select P-grade black corundum, immerse it in a 4% sodium hydroxide aqueous solution at room temperature for 10 min, rinse with pure water, dry at 100-110℃, and perform alkaline washing to remove impurities; then immerse it in a 0.3% ferrous sulfate aqueous solution for passivation and sealing, immerse it at room temperature for 25 min to form a dense passivation film in the iron oxide micropores, and dry it again (100-110℃); finally, mix the passivated and sealed black corundum with a composite coupling agent, dry stir and coat it for 15 min, and then cure and dry it at 130℃.

[0025] The composite coupling agent is selected from KH-550 silane coupling agent and KR-TTS titanate coupling agent in a mass ratio of 2:1, and the amount of composite coupling agent added is 0.8% of the mass of black corundum.

[0026] S2. Modified black corundum, calcined brown corundum, and single-crystal corundum are compounded at a mass ratio of 60:35:5 to obtain composite abrasive.

[0027] S3. Select fabric-based, paper-based, or non-woven fabric-based substrates, and pre-treat the substrates by degreasing, napping, and dehumidification. Then, apply 20~30μm epoxy resin base coat, and use high-voltage electrostatic vertical sand planting process to implant the composite abrasive in S2. Pre-bake and shape it so that the abrasive grains are initially fixed to the base coat layer. The epoxy resin primer, by weight, consists of 100 parts liquid epoxy resin, 28 parts type 650 epoxy polyamide curing agent, 4 parts BYK-333 leveling agent, 7 parts fumed silica, and 3 parts nano thermally conductive filler (nano aluminum nitride: fumed silica = 4:1).

[0028] S4. Apply modified phenolic resin evenly to the surface of the shaped abrasive layer to completely cover the root of the abrasive grains and fill the gaps between the abrasive grains, and then compact and level the resin layer.

[0029] The modified phenolic composite adhesive, by weight, consists of 100 parts modified phenolic resin, 8 parts wood powder (poplar, 200 mesh), 5 parts light calcium carbonate, 3 parts liquid nitrile rubber, and 3 parts nano thermally conductive filler. The modified phenolic resin is prepared by introducing acrylonitrile rubber flexible segments into the phenolic condensation stage of thermosetting phenolic resin. The amount of acrylonitrile rubber is 10% of the mass of thermosetting phenolic resin. The remaining parameters and steps in the modification process are as commonly used in the field or laboratory.

[0030] S5. After leveling the adhesive layer, first keep it at a negative pressure of -0.07 MPa and a temperature of 60-70℃ for 20 minutes to pre-cur and remove the tiny air bubbles inside the adhesive. Then, cure it in three stages: the first stage is to keep it at 70-80℃ for 30 minutes for pre-baking, the second stage is to keep it at 70-80℃ for 30 minutes for medium-temperature cross-linking, and the third stage is to keep it at 140-150℃ for 80 minutes for high-temperature curing.

[0031] The heating rate for the three-stage stepped heating curing process is 3℃ / min, and the product is allowed to cool naturally to room temperature after curing.

[0032] S6. After curing, zinc stearate dry powder anti-clogging coating and water-based polytetrafluoroethylene lubricating coating are sequentially applied to the surface of the abrasive layer of the substrate. Then, after aging and curing, and cutting into strips, finished sandpaper, abrasive cloth, or closed-loop abrasive belt are obtained. Example 2

[0033] A method for making coated abrasives using black corundum, employing the method described in Example 1, specifically includes the following steps: S1. Soak P-grade black corundum in a 5% sodium hydroxide aqueous solution at room temperature for 15 min, rinse with pure water, dry at 100-110℃, and perform alkaline washing to remove impurities; then immerse in a 0.5% ferrous sulfate aqueous solution for passivation and sealing, soak at room temperature for 30 min to form a dense passivation film in the iron oxide micropores, and dry again; finally, mix the passivated and sealed black corundum with a composite coupling agent, dry stir and coat for 20 min, and then cure and dry at 130℃.

[0034] The composite coupling agent is selected from KH-550 silane coupling agent and KR-TTS titanate coupling agent in a mass ratio of 2:1, and the amount of composite coupling agent added is 1.2% of the mass of black corundum.

[0035] S2. Modified black corundum, calcined brown corundum, and single-crystal corundum are compounded at a mass ratio of 70:25:5 to obtain composite abrasive.

[0036] S3. Select fabric-based, paper-based, or non-woven fabric-based substrates, and pre-treat the substrates by degreasing, napping, and dehumidification. Then, apply 20~30μm epoxy resin base coat, and use high-voltage electrostatic vertical sand planting process to implant the composite abrasive in S2. Pre-bake and shape it so that the abrasive grains are initially fixed to the base coat layer. The epoxy resin primer, by weight, consists of 100 parts liquid epoxy resin, 30 parts type 651 epoxy polyamide curing agent, 5 parts BYK-358 leveling agent, 8 parts hydrogenated castor oil, and 5 parts nano thermally conductive filler (nano aluminum nitride: fumed silica = 4:1).

[0037] S4. Apply modified phenolic resin evenly to the surface of the shaped abrasive layer to completely cover the root of the abrasive grains and fill the gaps between the abrasive grains, and then compact and level the resin layer.

[0038] The modified phenolic composite adhesive, by weight, consists of 100 parts modified phenolic resin, 10 parts wood powder (poplar, 200 mesh), 7 parts light calcium carbonate, 4 parts epoxidized soybean oil, and 4 parts nano thermally conductive filler. The modified phenolic resin is prepared by introducing acrylonitrile rubber flexible segments into the phenolic condensation stage of thermosetting phenolic resin. The amount of acrylonitrile rubber flexible segments is 10% of the mass of thermosetting phenolic resin. The remaining parameters and steps in the modification process are as per commonly used standards in the field or laboratory.

[0039] S5. After leveling the adhesive layer, first keep it at a negative pressure of -0.08 MPa and a temperature of 60-70℃ for 25 minutes to pre-cur and remove the tiny air bubbles inside the adhesive; then cure it in three stages of stepped temperature increase: the first stage is pre-baking at 70-80℃ for 35 minutes, the second stage is medium-temperature cross-linking at 70-80℃ for 35 minutes, and the third stage is high-temperature curing at 140-150℃ for 90 minutes.

[0040] The heating rate for the three-stage stepped heating curing process is 3℃ / min, and the product is allowed to cool naturally to room temperature after curing.

[0041] S6. After curing, zinc stearate dry powder anti-clogging coating and water-based polytetrafluoroethylene lubricating coating are sequentially applied to the surface of the abrasive layer of the substrate. Then, after aging and curing, and cutting into strips, finished sandpaper, abrasive cloth, or closed-loop abrasive belt are obtained. Example 3

[0042] A method for making coated abrasives using black corundum, employing the method described in Example 1, specifically includes the following steps: S1. Soak P-grade black corundum in a 6% sodium hydroxide aqueous solution at room temperature for 20 min, rinse with pure water, dry at 100-110℃, and perform alkaline washing to remove impurities; then immerse in a 0.8% ferrous sulfate aqueous solution for passivation and sealing, soak at room temperature for 35 min to form a dense passivation film in the iron oxide micropores, and dry again; finally, mix the passivated and sealed black corundum with a composite coupling agent, dry stir and coat for 25 min, and then cure and dry at 130℃.

[0043] The composite coupling agent is selected from KH-550 silane coupling agent and KR-TTS titanate coupling agent in a mass ratio of 2:1, and the amount of composite coupling agent added is 1.5% of the mass of black corundum.

[0044] S2. Modified black corundum, calcined brown corundum, and single-crystal corundum are compounded at a mass ratio of 80:17:3 to obtain composite abrasive.

[0045] S3. Select fabric-based, paper-based, or non-woven fabric-based substrates, and pre-treat the substrates by degreasing, napping, and dehumidification. Then, apply 20~30μm epoxy resin base coat, and use high-voltage electrostatic vertical sand planting process to implant the composite abrasive in S2. Pre-bake and shape it so that the abrasive grains are initially fixed to the base coat layer. The epoxy resin primer, by weight, consists of 100 parts liquid epoxy resin, 32 parts type 650 epoxy polyamide curing agent, 6 parts of Tigo 450 leveling agent, 9 parts polyamide wax thixotropic agent, and 7 parts of nano thermally conductive filler (nano aluminum nitride: fumed silica = 4:1).

[0046] S4. Apply modified phenolic resin evenly to the surface of the shaped abrasive layer to completely cover the root of the abrasive grains and fill the gaps between the abrasive grains, and then compact and level the resin layer.

[0047] The modified phenolic composite adhesive, by weight, consists of 100 parts modified phenolic resin, 12 parts wood powder (poplar, 200 mesh), 8 parts light calcium carbonate, 5 parts liquid nitrile rubber, and 5 parts nano thermally conductive filler. The modified phenolic resin is prepared by introducing acrylonitrile rubber flexible segments into the phenolic condensation stage of thermosetting phenolic resin. The amount of acrylonitrile rubber flexible segments is 10% of the mass of thermosetting phenolic resin. The remaining parameters and steps in the modification process are as per commonly used standards in the field or laboratory.

[0048] S5. After leveling the adhesive layer, first keep it at a negative pressure of -0.09 MPa and a temperature of 60-70℃ for 30 minutes to pre-cur and remove the tiny air bubbles inside the adhesive. Then, cure it in three stages: the first stage is to keep it at 70-80℃ for 40 minutes for pre-baking, the second stage is to keep it at 70-80℃ for 40 minutes for medium-temperature cross-linking, and the third stage is to keep it at 140-150℃ for 100 minutes for high-temperature curing.

[0049] The heating rate for the three-stage stepped heating curing process is 5℃ / min, and the product is allowed to cool naturally to room temperature after curing.

[0050] S6. After curing, zinc stearate dry powder anti-clogging coating and water-based polytetrafluoroethylene lubricating coating are sequentially applied to the surface of the abrasive layer of the substrate. Then, after aging and curing, and cutting into strips, finished sandpaper, abrasive cloth, or closed-loop abrasive belt are obtained.

[0051] To comprehensively and rigorously verify the inventiveness, practicality, and product advantages of the six core technologies of this invention—multi-stage passivation modification, composite coupling agent coating, ternary gradient abrasive, nano-thermal conductive adhesive layer, vacuum pre-curing, and double-layer anti-clogging lubricating coating—three sets of process comparative examples (single-variable missing control groups) were set up. Except for differences in a single variable, all self-made comparative examples and embodiments were completely unified in terms of raw materials, proportions, equipment, environment, and process flow, and were tested according to unified standards, ensuring absolute comparability of the data. Comparative Example 1

[0052] The difference between it and Example 1 is that: After the black corundum is alkali washed and ferrous salt passivated and sealed, it is not coated with a composite coupling agent in a double layer. Instead, it is modified by dry coating with an equal amount of single KH-550 silane coupling agent without titanate ester auxiliary coating. The rest of the abrasive ratio, adhesive system, curing process and coating process are completely consistent with those in Example 1. Comparative Example 2

[0053] The difference between it and Example 2 is that: Using the existing mainstream patented binary abrasive formula, the single-crystal corundum component was removed, and only modified black corundum and calcined brown corundum were physically mixed in a ratio of 70 parts modified black corundum and 30 parts calcined brown corundum. The multi-stage modification of the abrasive, the nano thermally conductive adhesive layer, the vacuum curing, and the double-layer coating process were completely consistent with those in Example 2. Comparative Example 3

[0054] The difference between it and Example 3 is that: The base adhesive and top adhesive systems completely removed nano-aluminum nitride / fumed silica nano-thermal conductive fillers, and only added conventional light calcium carbonate and wood powder as filler additives; the remaining resin system, toughening system, abrasive modification, and sand planting curing process were completely consistent with Example 3.

[0055] The above Examples 1-3 and Comparative Examples 1-3 were tested, wherein: Tensile strength and elongation at break were tested according to GB / T 15305.39-2020; tear strength was tested according to the pendulum tear method in GB / T 3917.1-2009; the abrasive layer shedding rate was calculated by collecting and weighing the detached debris using a belt grinding machine under 2.5 kg pressure; the rotational breakage rate was calculated according to GB / T 24939-2023 using a rotary testing machine with a Φ100 mm abrasive disc rotating at 3000 r / min for 120 s; grinding efficiency and wear ratio were calculated according to JB / T 10155-2012; polishing roughness was measured using a roughness meter. The test results are shown in the table below:

[0056] The results show that the overall performance of Examples 1-3 of the present invention is significantly better than that of Comparative Examples 1-3. The tear strength of the examples is not less than 89%, the sand layer shedding rate is not more than 2.3%, and the thermal stability temperature is not less than 288℃. This fully demonstrates the technical advantages of the present invention. In particular, in terms of polishing roughness, the examples are far superior to the comparative examples. It can be seen that the lack of thermally conductive filler has a great impact on the polishing performance of the product.

[0057] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Any other modifications or equivalent substitutions made by those skilled in the art to the technical solutions of the present invention, as long as they do not depart from the spirit and scope of the technical solutions of the present invention, should be covered within the scope of the claims of the present invention.

Claims

1. A method for making coated abrasives using black corundum, characterized in that, Includes the following steps: S1. Black corundum is subjected to alkali washing to remove impurities, ferrous salt passivation and sealing, and double-layer coating with composite coupling agent to obtain modified black corundum. S2. Modified black corundum is combined with calcined brown corundum and single-crystal corundum to obtain composite abrasive; S3. Apply epoxy resin primer to the pretreated substrate surface, and implant composite abrasive using high-voltage electrostatic vertical sand planting process. After sand planting is completed, pre-bake and shape it so that the abrasive particles are initially fixed to the primer layer. S4. Apply modified phenolic resin evenly to the surface of the shaped abrasive layer to completely wrap the root of the abrasive grains and fill the gaps between the abrasive grains, and then compact and level the resin layer. S5. First, perform negative pressure vacuum pre-curing to remove air bubbles from the adhesive layer, and then perform three-stage stepped temperature curing to eliminate internal stress in the resin. S6. Two functional super coating layers are sequentially applied to the surface of the abrasive layer. After aging and curing, and cutting into strips, finished abrasive cloth, sandpaper, or closed-loop abrasive belt are obtained.

2. The method for making coated abrasives using black corundum according to claim 1, characterized in that, The passivation sealing method described in S1 is as follows: after alkali washing and impurity removal, black corundum is immersed in a 0.3% to 0.8% ferrous sulfate aqueous solution and immersed at room temperature for 25 to 35 minutes to generate a dense passivation film in the micropores of iron oxide, and then dried.

3. The method for making coated abrasives using black corundum according to claim 2, characterized in that, The composite coupling agent described in S1, by weight ratio, includes KH-550 silane coupling agent: KR-TTS titanate coupling agent = 2:1, and the total amount of composite coupling agent added is 0.8% to 1.5% of the black corundum mass. It is dry-stirred and coated for 15 to 25 minutes, and then cured and dried at 115 to 130°C.

4. The method for making coated abrasives using black corundum according to claim 1, characterized in that, In S2, the compounding ratio of modified black corundum, calcined brown corundum, and single-crystal corundum, by weight, includes any one of the following: Coarsely ground P60~P120: 55~65 parts modified black corundum, 30~40 parts calcined brown corundum, and 3~8 parts single crystal corundum; Medium-milled P150~P220: 65~75 parts modified black corundum, 20~30 parts calcined brown corundum, and 2~6 parts single crystal corundum; Fine polishing P240~P600: 75~85 parts modified black corundum, 10~20 parts calcined brown corundum, and 1~5 parts monocrystalline corundum.

5. The method for making coated abrasives using black corundum according to claim 1, characterized in that, In S3, the epoxy resin primer comprises, by weight, 100 parts of liquid epoxy resin, 28-32 parts of polyamide curing agent, 4-6 parts of wetting and leveling agent, 7-9 parts of viscosity modifier, and 3-7 parts of nano thermally conductive filler; the nano thermally conductive filler comprises, by weight, nano aluminum nitride: fumed silica = 4:

1.

6. The method for making coated abrasives using black corundum according to claim 5, characterized in that, The polyamide curing agent is selected from at least one of type 650 and type 651 epoxy polyamide curing agents; the wetting and leveling agent is selected from any one of organosilicon leveling agents BYK-333, BYK-358, and DIG 450; the viscosity modifier is selected from at least one of fumed silica, hydrogenated castor oil, and polyamide wax thixotropic agent.

7. The method for making coated abrasives using black corundum according to claim 5, characterized in that, In S4, the modified phenolic composite adhesive, by weight, comprises 100 parts of modified phenolic resin, 8-12 parts of wood powder, 5-8 parts of light calcium carbonate, 3-5 parts of resin toughening agent, and 2-5 parts of nano thermally conductive filler.

8. The method for making coated abrasives using black corundum according to claim 1, characterized in that, The modified phenolic resin is prepared by introducing a nitrile rubber flexible segment into the phenolic condensation stage of thermosetting phenolic resin, wherein the mass ratio of the thermosetting phenolic resin to the nitrile rubber is 100:10; the wood powder is degreased poplar or pine wood sawdust powder with a mesh size of 180-300 mesh, a moisture content of ≤2%, and an ash content of ≤3%; the resin toughening agent is selected from at least one of liquid nitrile rubber, epoxidized soybean oil, and polyurethane toughening agent.

9. The method for making coated abrasives using black corundum according to claim 1, characterized in that, In S5, the negative pressure vacuum pre-curing is performed at a negative pressure of -0.06 to -0.09 MPa, a temperature of 60 to 70°C, and a holding time of 20 to 30 minutes to remove tiny air bubbles inside the adhesive. The three-stage stepped heating and curing process is as follows: First stage pre-baking: Keep warm at 70-80℃ for 30-40 minutes; Second stage of medium-temperature crosslinking: heat treatment at 105-115℃ for 50-70 min; The third stage is high-temperature curing: holding at 140-150℃ for 80-100 minutes; The heating rate is 3-5℃ / min, and after curing, it is allowed to cool naturally to room temperature.