A method for preparing and transferring a profiled texture module

By combining PC+PMMA sheet pretreatment, UV transfer adhesive lamination, and high-pressure molding, the problems of low texture accuracy and complex surface adaptation of silicone molds have been solved, realizing an efficient, low-cost, and environmentally friendly texture transfer method.

CN123104097APending Publication Date: 2026-11-17HUIZHOU WEIBO HARDWARE PROD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611333719.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-31
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies for silicone mold texture processing suffer from low precision, long processing time, high cost, and inability to adapt to complex curved surfaces.

Method used

The texture module is prepared by a combination of processes including PC+PMMA sheet pretreatment, UV transfer adhesive coating, composite texture sheet, vertical static leveling, LED pre-curing, high-pressure molding, and mercury lamp complete curing; then the texture module is transferred to a liquid silicone mold.

Benefits of technology

It achieves 1:1 accurate replication of 0.5μm fine textures with a texture fidelity of ≥99%, adapts to any complex curved surface, shortens the development cycle by 70%, reduces costs by 60%, is environmentally friendly and pollution-free, and has good batch consistency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123104097A_ABST
    Figure CN123104097A_ABST
Patent Text Reader

Abstract

The application relates to a preparation and transfer printing method of a profile texture module, and belongs to the technical field of mold manufacturing. The method comprises the following steps: a first stage of preparing a profile texture module: providing a PC+PMMA co-extruded sheet, spraying a UV transfer printing glue on the PC+PMMA co-extruded sheet, and then combining a PET texture sheet, vertical static flow leveling, LED pre-curing, high-pressure gas forming, mercury lamp complete curing, and obtaining a texture PC+PMMA transfer printing carrier consistent with the shape of a target curved surface; and a second stage of transferring the texture to a liquid silicone mold: positioning the profile texture module on a back mold core, injecting liquid silicone, and separating after curing, and the texture is reversely transferred to the surface of the silicone mold core. The application takes "preparation of a module and transfer printing" as the core, solves the problem that a traditional process cannot process high-precision textures on complex curved surfaces, the texture reduction degree is greater than or equal to 99%, the development cycle is shortened by more than 70%, the cost is reduced by 60%, the environment is protected without pollution, batch consistency is good, and the application is suitable for mold texture preparation in the fields of consumer electronics, automotive interiors, micro-fluidic chips and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to the field of mold manufacturing technology, and more specifically, to a method for preparing and transferring a contoured texture module. Background Technology

[0002] Liquid silicone molds are widely used in product molding for consumer electronics, automotive interiors, and medical devices. The texture of the mold cavity surface directly determines the appearance, texture, and feel of the final product. Currently, the texturing of silicone molds mainly employs the following traditional methods: Chemical etching: relies on manual film application and chemical etching, resulting in severe pollution and low texture processing accuracy (usually ≥50μm). It is prone to problems such as texture breaks and uneven depth on complex curved surfaces, and cannot achieve three-dimensional textures. The development cycle is as long as 15-20 days.

[0003] Laser engraving: This method involves directly etching the silicone surface, which can easily cause thermal deformation and carbonized burrs, resulting in blurred edges of fine textures. It is also difficult to process deep grooves and corners, and the consistency is poor during mass production.

[0004] CNC machining: The equipment and processing costs are high, the efficiency is low, and it is almost impossible to effectively process micron-level textures and complex curved surfaces.

[0005] Existing transfer methods: These methods often involve directly transferring the texture to the silicone surface. However, when dealing with complex curved surfaces, there are problems such as incomplete texture transfer, poor adhesion, and easy peeling.

[0006] Therefore, there is an urgent need to develop a new method for preparing texture modules to overcome the shortcomings of the existing technologies, such as low accuracy, long cycle time, high cost, high pollution, and inability to adapt well to complex curved surfaces. Summary of the Invention

[0007] The purpose of this invention is to provide a method for preparing and transferring a contoured texture module, so as to solve the problems of low precision, long cycle, high cost, and inability to adapt to complex curved surfaces in the prior art for processing textures in silicone molds.

[0008] To achieve the above objectives, the present invention provides the following technical solution: A method for preparing and transferring a contoured texture module includes the following two stages: Phase 1: Pre-made contour texture module (1) Pretreatment of PC+PMMA sheet: Provide a PC+PMMA sheet for cleaning and dust removal; (2) Applying UV transfer adhesive: Applying UV transfer adhesive to the PMMA interface of the PC+PMMA sheet; (3) Composite texture sheet: Vacuum-bonded PET texture sheet with target texture to the surface of UV transfer adhesive layer; (4) Vertical static leveling: Place the composite sheet vertically and perform static leveling; (5) LED pre-curing: The composite sheet is pre-cured by irradiation with a UV-LED lamp; (6) High pressure forming: The pre-cured composite sheet is placed in a high pressure gas forming machine and held under pressure under heating and pressurization conditions to form the composite sheet into the target curved surface shape; (7) Mercury lamp complete curing: The composite sheet after high pressure molding is completely cured by a high-pressure mercury lamp to obtain the contour texture module; Phase Two: Transferring the texture from the contouring texture module to the liquid silicone mold. (8) Position the contour texture module on the rear core of the liquid silicone mold, inject liquid silicone, and cure it. (9) After the mold is opened, the texture module is separated from the cured silicone core, so that the texture is transferred to the surface of the silicone core.

[0009] Furthermore, the thickness of the PC+PMMA sheet in step (1) is 0.35-0.40 mm, preferably 0.38 mm, and the flatness is ≤0.05 mm.

[0010] Furthermore, the UV transfer adhesive mentioned in step (2) is a high-leveling, high-adhesion acrylic UV adhesive with a viscosity of 1500-2500cps (25℃), a coating thickness of 0.05-0.10mm, and a light transmittance of ≥92% after curing.

[0011] Furthermore, the thickness of the PET texture sheet in step (3) is 0.18-0.20 mm, preferably 0.188 mm, and the target texture depth on its surface is 0.5-50 μm.

[0012] Furthermore, the static leveling time in step (4) is 25-35 minutes, preferably 30 minutes, with an ambient temperature of 22-26°C and a humidity of 45%-55%.

[0013] Further, the energy of LED pre-curing in step (5) is 280-320mJ / cm², preferably 300mJ / cm²; the energy of mercury lamp complete curing in step (7) is 1200-1500mJ / cm², preferably 1300mJ / cm², and the pencil hardness of the UV transfer adhesive after complete curing is ≥2H.

[0014] Furthermore, the conditions for high-pressure molding in step (6) are: temperature 120-140℃, pressure 0.6-0.8MPa, and holding time 5-10 seconds.

[0015] Furthermore, in step (8), the injection mold temperature of the liquid silicone is 120-130℃, the injection pressure is 20-60MPa, the curing time is 240-290 seconds, the Shore hardness of the liquid silicone is 60-70A, and the shrinkage rate is ≤0.1%.

[0016] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects: Ultra-high texture fidelity: Through a combination of processes including "high-precision planar transfer, high-pressure curved surface forming, and reverse transfer", it can achieve 1:1 accurate replication of fine textures at the 0.5μm level, with a fidelity of ≥99%, and the texture is full, without pinholes or deformation.

[0017] Perfectly adaptable to any complex curved surface: First, high-precision texture transfer is completed on a flat surface, and then high-pressure gas is used to make the composite sheet evenly adhered to a complex curved surface with any curvature, solving the problem that traditional processes cannot process uniform textures in deep grooves and corners.

[0018] Significantly shorten the development cycle: The mold texture development cycle can be shortened from the traditional 15-20 days to 3-5 days, a reduction of more than 70%, enabling a rapid response to market demands.

[0019] Significantly reduces production costs: No expensive laser engraving and CNC machining equipment are required, reducing production costs by more than 60% compared to traditional processes. Furthermore, the process parameters are standardized, making it suitable for mass production, with a yield rate of over 95%.

[0020] Green and environmentally friendly: The entire process uses physical and photochemical processes, replacing the highly polluting chemical etching method, with no wastewater or exhaust gas emissions.

[0021] Good batch consistency: Standardized process parameters ensure that the texture deviation of the same batch of molds is ≤±2%, resulting in high product appearance consistency. Attached Figure Description

[0022] Figure 1 This is a schematic diagram of the process of the present invention. Detailed Implementation

[0023] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. It is understood that the specific embodiments described herein are only for explaining this application and not for limiting it. Furthermore, it should be noted that, for ease of description, only the parts related to this application are shown in the accompanying drawings, not all structures. All other embodiments obtained by those skilled in the art based on the embodiments of this application without creative effort are within the scope of protection of this application.

[0024] In the description of this application, it should be noted that, unless otherwise expressly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection, an electrical connection, or a connection that allows communication between them; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal communication between two components or the interaction between two components. Those skilled in the art can understand the specific meaning of the above terms in this application according to the specific circumstances.

[0025] Example 1: This example prepares a contour texture module and transfer for a liquid silicone mold for a mobile phone frame. The target texture is a CD texture with a depth of 8μm, and the target curved surface is a complex shape with a 2.5D arc edge.

[0026] Phase 1: Pre-made contour texture module Step 1: Preprocessing of PC+PMMA wafers Select a 0.38mm thick high-transmittance optical-grade PC+PMMA sheet (transmittance ≥90%). Wipe the surface with a lint-free cloth dampened with isopropyl alcohol, then place it in an ultrasonic cleaner and clean for 5 minutes with anhydrous ethanol as the medium. Rinse with deionized water for 2 minutes, and finally dry in a clean oven at 50℃ for 15 minutes. Check flatness: Use a laser flatness measuring instrument; the flatness should be ≤0.05mm. If it exceeds this limit, the PC sheet must be replaced. Precautions: The surface of the PC+PMMA sheet must be free of fingerprints, oil, dust, or scratches; otherwise, it will lead to reduced adhesion of the subsequent UV adhesive or imperfections in the texture. A Class 10,000 cleanroom is recommended for operation.

[0027] Step 2: Apply UV transfer adhesive A precision microporous coating machine is used to uniformly coat a layer of acrylic UV transfer adhesive onto the surface of a PC+PMMA sheet. The adhesive viscosity is controlled at 2000±100cps at 25℃, and the coating thickness is set at 0.08mm (allowable tolerance ±0.01mm). The coating speed is controlled at 50mm / s to ensure the adhesive layer is free of streaks and bubbles. Precautions: Before use, the adhesive should be left to stand in a 25℃ constant temperature water bath for 30 minutes to eliminate internal air bubbles; after coating, let it stand for 2 minutes to allow the adhesive layer to level naturally.

[0028] Step 3: Composite Texture Patch Take a 0.188mm thick PET textured sheet with an 8μm deep CD pattern on its surface (made by electroforming or photolithography). Place the PET textured sheet on the lower platform of the vacuum laminator, textured side up; align it with the PC sheet coated with UV adhesive (adhesive side down). Evacuate to -0.1MPa, then apply a lamination pressure of 0.2MPa and hold for 10 seconds. Note: Lamination should proceed gradually from the center to the edges to prevent air bubbles. If air bubbles appear, increase the holding time to 15 seconds or increase the pressure to 0.25MPa, but be careful to prevent adhesive overflow. Post-lamination inspection: Visually inspect under 1000Lux light; there should be no air bubbles larger than 0.2mm in diameter.

[0029] Step 4: Erect static leveling Place the laminated sheet vertically in a constant temperature and humidity chamber at 24±1℃ and 50±5% relative humidity for 30 minutes. Explanation: When vertically positioned, the UV adhesive undergoes a downward micro-flow under gravity, fully filling the micron-level grooves on the PET textured sheet while expelling tiny air bubbles upwards. Precautions: The settling time should not be too short (<25 minutes) or the filling will be insufficient; it should also not be too long (>40 minutes) or the adhesive may flow to the edges, resulting in uneven thickness. Low humidity (<40%) can easily cause static electricity and dust attraction; high humidity (>60%) may cause the UV adhesive to absorb moisture and turn white.

[0030] Step 5: LED pre-curing A 365nm UV-LED surface light source was used, 50mm from the composite sheet surface, with an irradiation energy of 300mJ / cm² (calibrated using a radiometer). After pre-curing, the UV adhesive transformed into a gel state, with a slightly tacky surface, but remained flexible without cracking. Precautions: Excessive energy will cause premature hardening, loss of flexibility, and easy cracking during subsequent high-pressure molding; insufficient energy will prevent proper shaping, damaging the texture when the PET texture sheet is removed. The key to this step is to achieve a "semi-cured" adhesive layer, retaining a certain degree of flow and filling capacity.

[0031] Step 6: High-pressure molding Separate the pre-cured PET textured sheet from the PC+PMMA sheet; transfer the texture to the PMMA interface of the PC+PMMA, then place the textured side into a high-pressure gas molding machine (such as a dedicated high-pressure molding machine for IMD / OMD), with the cavity being the target curved surface of the mold. After mold closing, rapidly heat to 130℃ while simultaneously filling with high-pressure air to 0.7MPa, holding the pressure for 20 seconds. Operating details: Control the heating rate at 5℃ / s to avoid thermal shock causing deformation of the PC+PMMA sheet. After holding the pressure, cool to below 60℃ before releasing the pressure and opening the mold. For 3D curved surfaces with greater curvature (such as spheres or freeform surfaces), the temperature can be increased to 140℃, the pressure increased to 0.8MPa, and the holding time extended to 25 seconds. The molded composite sheet should completely fit the cavity, without warping or wrinkles, and the textured surface should remain intact.

[0032] Step 7: Mercury lamp fully cures A high-pressure mercury lamp (power density 80W / cm²) was used with a lamp spacing of 150mm, accumulating an energy of 1300mJ / cm². After curing, the UV adhesive layer achieved a pencil hardness of 2H (GB / T 6739-2006) and an adhesion (cross-cut test) grade of 0. At this point, the texture and the PC+PMMA sheet have firmly bonded together through the cured UV adhesive, forming a unified contoured texture module. This module can be directly used for the next transfer step.

[0033] Phase Two: Transferring the texture from the contouring texture module to the liquid silicone mold. Step 8: Liquid silicone injection transfer Precisely position the prepared textured module (PC+PMMA with textured sheet) onto the rear mold core of the liquid silicone mold. Positioning can be achieved by using pins on the mold and positioning holes on the module, or by temporarily fixing it with double-sided high-temperature resistant tape. Note: The textured surface should face the mold core cavity. After mold closing, inject high-transparency liquid silicone (commercially available high-transparency liquid silicone with a Shore hardness of 60A and a shrinkage rate of 0.1%) using an LSR (liquid silicone) injection molding machine. Process parameters: injection mold temperature 125℃, injection pressure 45MPa, curing time 290 seconds. Precautions: The injection pressure should not be too high, otherwise the fragile textured module may be damaged; sufficient curing time is required to ensure complete cross-linking of the silicone, otherwise it will easily stick together during demolding.

[0034] Step 9: Mold Opening and Separation After curing, the mold is opened slowly at a speed of 0.5 mm / s. Due to the inherent low adhesion (surface energy difference) between the PMMA interface of the PC+PMMA sheet and the silicone, and the high hardness of the UV adhesive layer, the two can be separated smoothly. If local adhesion occurs, a very thin layer of release agent (such as a fluorinated release agent, thickness <0.1 μm) can be sprayed onto the surface of the textured module before mold closing, but this is usually not necessary. After separation, the silicone mold core surface will have a complete CD texture. Inspection: Observation using a 3D laser microscope shows a texture depth of 7.9-8.1 μm, a reproduction rate of 99%, and no pinholes or deformation.

[0035] Example 2: This example verifies the adaptability of the present invention to different texture depths. PET texture sheets with texture depths of 0.5μm (precision raster texture) and 50μm (coarse leather texture) were used respectively, with other parameters the same as in Example 1. The results show that for the 0.5μm texture, the coating thickness needs to be reduced to 0.05mm and the standing time extended to 35 minutes to ensure perfect filling of the microstructure; for the 50μm texture, the coating thickness needs to be increased to 0.10mm and the standing time shortened to 25 minutes to prevent over-filling of the adhesive and blurring of texture details. After curing, a contoured texture module with a texture reproduction accuracy of ≥99% can be obtained.

[0036] Example 3: The PC+PMMA sheet was replaced with a PET sheet (0.38mm) of the same thickness, or a PMMA sheet and a PC sheet, while keeping other conditions unchanged. Results showed that the PET sheet had significant springback after high-pressure molding, making it difficult to maintain complex curved surfaces; the PMMA sheet was prone to microcracks during high-pressure molding. The PC sheet had a low hardness (<HB) after UV coating. Therefore, the preferred substrate was the PC+PMMA sheet, which offered the best overall performance. However, if the target curved surface is a simple bend (such as a single-curvature arc), the PET sheet can also be used at a lower cost.

[0037] The contouring texture module and transfer method prepared in Examples 1-3 of this invention were used to test 50 batches of molds, and the results are as follows: Average texture fidelity: 99.3%, lowest value: 98.7%; A single module can be reused for transfer printing 3-5 times (after which the UV adhesive layer will wear slightly, and replacement is recommended). Mold development cycle: From obtaining texture samples to producing qualified molds, it takes an average of 4 days (15 days for traditional etching methods). Cost Comparison: Based on 10 sets of molds, the total cost of this invention is approximately 35% of that of the traditional laser engraving method; Environmentally friendly: No waste liquid or exhaust gas emissions, and complies with RoHS standards.

[0038] It should be noted that; All operations that come into contact with the textured surface must be performed in a Class 10,000 cleanroom to prevent dust from causing texture defects.

[0039] Acrylic UV adhesives should be stored away from light and refrigerated (4-8℃). Before use, they should be warmed to 25℃.

[0040] For PC+PMMA sheets of different thicknesses (e.g., 0.3mm or 0.4mm), the temperature (±5℃) and pressure (±0.1MPa) should be adjusted accordingly. Use low temperature and low pressure for thin sheets, and high temperature and high pressure for thick sheets.

[0041] After one transfer, a trace amount of silicone oil may remain on the surface of the texture module. This can be gently wiped off with anhydrous ethanol before reuse. However, after three uses, it is recommended to replace the module to ensure texture accuracy.

[0042] The embodiments described above are merely preferred embodiments of the present invention, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can make various modifications, improvements, and substitutions without departing from the concept of the present invention, and these all fall within the scope of protection of the present invention. Therefore, the scope of protection of this patent should be determined by the appended claims.

Claims

1. A method of making and transferring a profiled texture module, characterized in that, Includes the following stages: Phase 1: Pre-made contour texture module (1) Pretreatment of PC+PMMA sheet: Provide a PC+PMMA sheet for cleaning and dust removal; (2) Applying UV transfer adhesive: Applying UV transfer adhesive to the PMMA interface of the PC+PMMA sheet; (3) Composite texture sheet: Vacuum-bonded PET texture sheet with target texture to the surface of UV transfer adhesive layer; (4) Vertical static leveling: Place the composite sheet vertically and perform static leveling; (5) LED pre-curing: The composite sheet is pre-cured by irradiation with a UV-LED lamp; (6) High pressure forming: The pre-cured composite sheet is placed in a high pressure gas forming machine and held under pressure under heating and pressurization conditions to form the composite sheet into the target curved surface shape; (7) Mercury lamp complete curing: The composite sheet after high pressure molding is completely cured by a high-pressure mercury lamp to obtain the contour texture module; Phase Two: Transferring the texture from the contouring texture module to the liquid silicone mold. (8) Position the contour texture module on the rear core of the liquid silicone mold, inject liquid silicone, and cure it. (9) After the mold is opened, the texture module is separated from the cured silicone core, so that the texture is transferred to the surface of the silicone core.

2. The method of claim 1, wherein, The thickness of the PC sheet mentioned in step (1) is 0.35-0.40 mm, and the flatness is ≤0.05 mm.

3. The method of claim 1, wherein, The UV transfer adhesive mentioned in step (2) is an acrylic UV adhesive with a viscosity of 1500-2500 cps and a coating thickness of 0.05-0.10 mm; the pencil hardness of the UV transfer adhesive after complete curing in step (7) is ≥2H.

4. The method of claim 1, wherein, The thickness of the PET texture sheet mentioned in step (3) is 0.18-0.20 mm, and the target texture depth on its surface is 0.5-50 μm.

5. The method of claim 1, wherein, The static leveling time in step (4) is 25-35 minutes, the ambient temperature is 22-26℃, and the humidity is 45%-55%.

6. The method of claim 1, wherein, The energy of LED pre-curing in step (5) is 280-320 mJ / cm²; the energy of mercury lamp complete curing in step (7) is 1200-1500 mJ / cm².

7. The method of claim 1, wherein, The conditions for high-pressure molding in step (6) are: temperature 120-140℃, pressure 0.6-0.8MPa, and holding time 5-10 seconds.

8. The method of claim 1, wherein, The temperature of the injection mold for the liquid silicone in step (8) is 120-130℃, the injection pressure is 20-60MPa, the curing time is 240-290 seconds, the Shore hardness of the liquid silicone is 60-70A, and the shrinkage rate is ≤0.1%.