A method for preparing polyurethane composite material for mobile phone battery cover
By using asymmetric partitioning impregnation with low-scattering photosensitive impregnating solution A and high-thermal-conductivity photosensitive impregnating solution B, and controlling with multi-physics fields, the spatial decoupling problem between thermal conductivity and dielectric properties was solved, achieving high thermal conductivity and low dielectric properties in ultrathin composite materials, and avoiding warping deformation and stress concentration.
Patent Information
- Application Number
- CN202611149742.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-31
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies cannot achieve spatial decoupling of thermal conductivity and dielectric properties within a single ultrathin composite substrate. Furthermore, the introduction of high-load thermally conductive fillers leads to UV deep curing defects and warping deformation, making it difficult to meet the requirements of ultrathin design and frequent thermal shock.
An asymmetric partitioned impregnation method using low-scattering photosensitive impregnating liquid A and high-thermal-conductivity photosensitive impregnating liquid B, combined with gradient interface fiber preforms and multi-physics field control, forms a low-filler layer on the outer surface and a thermally conductive filler-rich layer on the inner heat source side. The uniform distribution and curing of the resin are achieved through online surface density feedback and adhesive control mechanism.
It reduces ultraviolet light scattering and surface curing defects in the thickness direction, improves thermal conductivity, reduces dielectric loss, avoids stress concentration, and satisfies both heat dissipation and communication performance.
Smart Images

Figure CN123104115A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the technical field of polyurethane composite materials for mobile phones, and specifically to a method for preparing a polyurethane composite material for a mobile phone battery cover. Background Technology
[0002] With the evolution of mobile communication technology towards 5G and future higher frequency bands, smart terminal devices are placing stringent comprehensive requirements on shell materials, demanding "ultra-thinness, high thermal conductivity, and low dielectric loss." Continuous fiber reinforced polyurethane composites, with their excellent mechanical properties and design flexibility, have become an important material for manufacturing ultra-thin mobile phone back panels. To address the heat accumulation problem in high-performance chips, it is typically necessary to introduce high-load inorganic thermally conductive fillers such as boron nitride and alumina into the resin matrix. However, improving thermal conductivity often comes at the cost of sacrificing signal transmittance and material molding quality. Current technologies typically employ physical lamination or uniform impregnation methods to prepare these composites.
[0003] CN111469518A discloses a composite organic ceramic material and its mobile phone back panel. This structure achieves a balance between thermal conductivity and signal strength by macroscopically stacking a thermosetting resin layer, a fiber braided layer, and an organic ceramic layer. However, this macroscopic multilayer physical stacking method results in significant abrupt changes in physical properties along the thickness direction. Under ultra-thin designs and frequent thermal shocks, stress concentration easily occurs at the interlayer interfaces, leading to peeling and cracking. Furthermore, since each functional layer is distributed in-plane, it is impossible to optimize the dielectric properties of the antenna area inside the mobile phone locally. On the other hand, regarding the optical / wave transmittance properties of composite materials, CN113681935A discloses a manufacturing process for transparent 3D glass fiber sheets, which involves coating glass fibers with transparent resin to form a prepreg and then UV curing it. While this solution ensures excellent light and wave transmittance, it completely lacks thermal conductivity. If high-load thermally conductive fillers are introduced into this process system, the strong scattering of ultraviolet light by the fillers will block the transmission of light energy to the deeper layers of the material, resulting in a severe defect of "over-curing of the surface layer and under-curing of the deep layer" in the composite material. More challenging is that existing curing processes often use fixed-parameter program control, lacking real-time online feedback on the cross-linking shrinkage state of the resin. This easily leads to warping and deformation of ultra-thin sheets after curing and demolding, making it difficult to meet the requirements of precision assembly.
[0004] In summary, existing technologies have been unable to overcome the physical conflict between the high scattering properties of thermally conductive fillers and deep UV curing, nor have they been able to achieve spatial decoupling of thermal conductivity and dielectric properties within a single ultrathin composite substrate. Summary of the Invention
[0005] Therefore, the purpose of this invention is to provide a method for preparing polyurethane composite material for mobile phone battery covers, which can form a precise functional gradient in the in-plane and thickness directions, and overcome the curing shrinkage and warping of high filler systems.
[0006] To achieve the above objectives, the present invention provides the following technical solution:
[0007] A method for preparing a polyurethane composite material for a mobile phone battery cover includes the following steps:
[0008] S1: Glass fiber and basalt fiber are mixed and woven to form a fiber preform. After cleaning, drying and plasma activation, the fiber preform is immersed in a grafting solution containing silane coupling agent, acrylate monomer and photoinitiator. After ultraviolet irradiation and heat treatment, a gradient interface layer containing plasma-activated polar groups, silane anchoring structure and co-curable grafting structure containing acrylate double bond is formed on the fiber surface to obtain a gradient interface fiber preform.
[0009] S2: Prepare low-scattering photosensitive impregnation solution A and high-thermal-conductivity photosensitive impregnation solution B respectively; the low-scattering photosensitive impregnation solution A comprises a bio-based polyurethane acrylate prepolymer with acrylate end groups, a reactive diluent, and a compound photoinitiator; the high-thermal-conductivity photosensitive impregnation solution B comprises a bio-based polyurethane acrylate prepolymer with acrylate end groups, a reactive diluent, a compound photoinitiator, a fluorosilicone modifier containing acrylate double bonds, and a surface-modified boron nitride nanosheet and spherical alumina compound filler; wherein, the content of the compound filler in the low-scattering photosensitive impregnation solution A is 0~5wt%, the content of the compound filler in the high-thermal-conductivity photosensitive impregnation solution B is 20~30wt%, and the amount of fluorosilicone modifier added is 1.5~2.5wt% of the total mass of the high-thermal-conductivity photosensitive impregnation solution B;
[0010] S3: A dual-cavity, multi-channel slit mold is used to asymmetrically apply low-scattering photosensitive impregnating solution A and high-thermal-conductivity photosensitive impregnating solution B to the gradient interface fiber preform. Low-scattering photosensitive impregnating solution A is applied to the outer surface side and the position corresponding to the mobile phone antenna clearance area, while high-thermal-conductivity photosensitive impregnating solution B is applied to the position near the internal heat source side of the mobile phone. Subsequently, the coated gradient interface fiber preform is continuously passed through a tapered impregnation channel with an inlet-to-outlet cross-sectional area ratio of 2.0~3.0:1. Impregnation and degreasing are performed in conjunction with a linear vacuum gradient field, online surface density feedback, and a glue control mechanism. The resulting prepreg has a resin content of 40~45wt%, and forms a low filler layer on the outer surface side, a thermally conductive filler enrichment layer on the internal heat source side, a low dielectric region corresponding to the mobile phone antenna clearance area, and a transition region between the high thermal conductivity region and the low dielectric region in the prepreg.
[0011] S4: Place the prepreg between UV-transmitting plates for constraint curing, and then irradiate it with 365nm first-band UV light and 395nm second-band UV light in sequence;
[0012] During the first-band ultraviolet irradiation, a dual-channel near-infrared spectrometer was used to monitor the C=C overtone absorption peak of acrylate in the 1610~1640nm band in real time, and the conversion rates of the upper surface R_top and the lower surface R_bottom of the prepreg were calculated.
[0013] The switching from the first band to the second band is triggered based on the conversion rate R_top of the upper surface and the difference in conversion rates ΔR between the upper and lower surfaces;
[0014] The constraint pressure was simultaneously released in a stepped manner during the second-band ultraviolet irradiation.
[0015] After the second-band ultraviolet light irradiation is completed, infrared post-curing is performed, and the infrared power and infrared action time are adjusted according to the temperature difference ΔT in the thickness direction of the material to obtain a polyurethane composite material for the battery cover of the mobile phone body.
[0016] The present invention is further configured such that: in step S1, the mass ratio of glass fiber to basalt fiber is 7.0~8.0:2.0~3.0; the fiber preform is a plain weave fabric with a thickness of 0.20~0.40mm and a surface density of 190~210g / m², and the monofilament diameter of the glass fiber and basalt fiber is 7~9μm.
[0017] The present invention is further configured such that: in step S1, plasma activation uses a mixture of Ar and O2 gas, with a volume ratio of Ar to O2 of 93~97:3~7, a processing power of 130~150W, a processing speed of 1.5~2.0m / min, and a vertical distance of 2.5~3.5mm between the plasma nozzle and the surface of the fiber preform; after plasma activation, the O / C atomic ratio on the fiber surface is 0.25~0.35.
[0018] The present invention is further configured such that: in step S1, the silane coupling agent is γ-methacryloxypropyltrimethoxysilane, and the acrylate monomer includes trimethylolpropane triacrylate and 1,6-hexanediol diacrylate.
[0019] The heat treatment employs a gradient process of holding at 75℃ for 8-12 minutes, holding at 95℃ for 4-6 minutes, and holding at 75℃ for 8-12 minutes, resulting in a gradient interface layer thickness of 80-120 nm.
[0020] The present invention is further configured such that: in step S2, the bio-based content of the bio-based polyurethane acrylate prepolymer containing acrylate end groups is 30-40%, the weight-average molecular weight is 5000-8000, and the viscosity at 25°C is 4000-5000 mPa·s.
[0021] The reactive diluent is isoborneol acrylate, added at a rate of 5-10 wt%.
[0022] The composite photoinitiator is composed of TPO-L and 1173 in a mass ratio of 1.5:1, with an addition amount of 0.8~1.2wt%.
[0023] The present invention is further configured such that: in step S2, the boron nitride nanosheets are subjected to oxygen plasma treatment or dopamine-assisted coating treatment before silanization;
[0024] The boron nitride nanosheets have a D50 diameter of 1~3μm and a thickness of 20~50nm, while the spherical alumina has a D50 particle size of 1~5μm. The mass ratio of boron nitride nanosheets to spherical alumina is 1.0~1.5:1.
[0025] Surface modification uses a silane coupling agent containing double bonds to give the surface of the composite filler double bond groups that can participate in the photocuring reaction.
[0026] The present invention is further configured such that: in step S2, the high thermal conductivity photosensitive impregnation solution B also contains 0.2~0.5wt% fumed silica, and the thixotropic index of the high thermal conductivity photosensitive impregnation solution B is 2.4~2.8;
[0027] Fluorosilicone modifiers containing acrylate double bonds are matched according to the amount of compound filler added:
[0028] When the amount of compound filler added is 20~23wt%, the amount of fluorosilicone modifier added is 2.0~2.5wt%.
[0029] When the amount of compound filler added is 24~30wt%, the amount of fluorosilicone modifier added is 1.5~2.0wt%.
[0030] The present invention is further configured such that: in step S3, the dual-cavity multi-channel slit mold head includes mutually independent channels, which are respectively used to transport low-scattering photosensitive impregnation liquid A and high-thermal-conductivity photosensitive impregnation liquid B;
[0031] The low-scattering photosensitive impregnating solution A is applied by switching the position of the corresponding mobile phone antenna clearance area via a solenoid valve.
[0032] The width of the transition zone is 3~8mm, and the content of the composite filler in the transition zone gradually decreases from the high thermal conductivity zone to the low dielectric zone.
[0033] The present invention is further configured such that: the ultraviolet-transmitting pressure plate in step S4 is a quartz glass pressure plate; the intensity of ultraviolet light irradiation in the first band is 150~250mW / cm², and the intensity of ultraviolet light irradiation in the second band is 300~500mW / cm²;
[0034] The first wave of ultraviolet irradiation ends when R_top reaches 55-65%. If ΔR ≤ 15%, the second wave of ultraviolet irradiation is then executed.
[0035] If ΔR > 15%, then reduce the initial irradiation intensity of the second band and extend the irradiation time of the second band until ΔR drops to below 15%.
[0036] The constraint pressure is released in stages by reducing the initial pressure from 0.30 to 0.40 MPa to 0.15 to 0.25 MPa.
[0037] The thickness-direction temperature difference ΔT is estimated by the top infrared temperature measurement value, the bottom heat flow value, and the calibrated thickness-direction heat conduction model. When ΔT > 8℃, the infrared power is 0.4~0.6W / cm²; when 3℃ < ΔT ≤ 8℃, the infrared power is 0.6~0.8W / cm²; when ΔT ≤ 3℃ and lasts for 30~60s, the infrared curing ends, and the material surface temperature does not exceed 75℃ during the infrared curing process.
[0038] Compared with the shortcomings of the prior art, the beneficial effects of the present invention are as follows:
[0039] This invention utilizes a low-scattering photosensitive impregnating solution A and a high-thermal-conductivity photosensitive impregnating solution B, employing an asymmetric partitioned impregnation method, to create a composite material with a low-filler layer on the outer surface and a thermally conductive filler-rich layer on the inner heat source side in the thickness direction. The low-filler layer on the outer surface reduces ultraviolet light scattering and surface curing defects, while the thermally conductive filler-rich layer on the inner heat source side improves the thermal conductivity near heat sources such as batteries and motherboards, thereby alleviating the conflict between the high thermal conductivity filler load and ultraviolet curing penetration. Only or primarily low-scattering photosensitive impregnating solution A is applied to the corresponding mobile phone antenna clearance area, creating a low-dielectric region in that area. Simultaneously, a transition zone with gradually changing filler content is set between the high thermal conductivity and low dielectric regions. This reduces dielectric loss in the antenna area and avoids stress concentration caused by excessive stiffness or shrinkage differences between the high-filler and low-filler regions, thus balancing heat dissipation and communication performance.
[0040] This invention sequentially forms plasma-activated polar groups, silane anchoring structures, and co-curable graft structures containing acrylate double bonds on the surface of a glass fiber and basalt fiber hybrid preform, enabling the fiber surface to co-cur and bond with the polyurethane acrylate matrix during subsequent UV curing. This improves the interfacial bond strength between the fiber reinforcement layer and the resin matrix, reducing the risk of interlayer delamination, whitening, and crack propagation in the backsheet under bending, dropping, or humid and hot environments. Attached Figure Description
[0041] Figure 1 This is a schematic diagram of the control terminal of the present invention;
[0042] Figure 2 This is a schematic diagram of the structure of step 3 of the present invention;
[0043] Figure 3 This is a top view of the functional partitions on the back panel of the mobile phone according to the present invention.
[0044] Figure 4 This is a cross-sectional view of the three-layer co-directional stacked micro-gradient structure of the present invention.
[0045] Figure 5 This is a multiphysics response curve of the composite material closed-loop control state provided in an embodiment of the present invention; wherein, Figure 5 a represents the closed-loop curve of NIR real-time monitoring conversion kinetics. Figure 5 b is the linkage curve between the curing process and the stepwise release of constraint pressure. Figure 5 c represents the infrared thermal equilibrium dynamic compensation curve based on thickness temperature difference grading. Detailed Implementation
[0046] Reference Figures 1 to 5 The embodiments of the present invention will be further described below.
[0047] Example 1:
[0048] Step S1: First, a fiber preform is selected, consisting of three layers of plain weave fabric with a single-layer density of 190 g / m² and a single-layer thickness of 0.067 mm, resulting in a total thickness of 0.20 mm. The plain weave fabric is made of high-strength glass fiber with a single filament diameter of 7 μm and basalt fiber in a mass ratio of 7.0:3.0. To remove residual sizing agent and organic contaminants from the fiber surface, the fabric is placed in an ultrasonic cleaning tank (frequency 40 kHz, power density 0.3 W / cm²), treated in an acetone bath at 40°C for 20 min, followed by three cycles of deionized water rinsing, and finally dried in an oven at 80°C and a vacuum degree ≤100 Pa for 4 h. The moisture content is measured to be below 0.05% using a Karl Fischer moisture analyzer.
[0049] Next, the dried preform underwent plasma surface activation treatment. Atmospheric pressure plasma treatment equipment was used, with the vertical distance between the plasma nozzle and the fabric surface controlled at 2.5 mm. A mixture of Ar and O2 with a volume ratio of 93:7 was used as the working gas, and the total gas flow rate was set to 25 SLM (standard liters / minute). At a processing power of 130 W, the preform was passed through the treatment head at a uniform speed of 1.5 m / min. After this treatment, X-ray photoelectron spectroscopy determined that the oxygen-to-carbon ratio (O / C) on the fiber surface increased to 0.25.
[0050] Subsequently, the silane grafting solution was prepared by adding the silane coupling agent γ-(methacryloyloxy)propyltrimethoxysilane (KH-570) to a mixed solvent of isopropanol and water (volume ratio 9:1). The pH of the system was adjusted to 4.0 using glacial acetic acid, and the mixture was hydrolyzed at a constant temperature of 30±2℃ for 3.5 h. Then, 7.5 wt% of a TMPTA and HDDA complex monomer (mass ratio 1:1) and 0.4 wt% of photoinitiator 1173 were added to the system. After thorough mixing, isopropanol and water were removed by film evaporation at 40±2℃ and a vacuum of -0.090 to -0.092 MPa until the solid content of the system was ≥85 wt%. After the slurry cooled to 25±2℃, 0.4 wt% of photoinitiator 1173 was added, and the mixture was dispersed at a low speed of 300 rpm for 5 min in a dark environment to obtain a grafting solution with a viscosity of 18 mPa·s (25℃).
[0051] Finally, the activated preform was immersed in the grafting solution for 3 minutes, then removed and irradiated with 365 nm ultraviolet light at an energy of 600 mJ / cm² to induce initial cross-linking of the double bonds. A gradient heat treatment process of 75℃ (8 min) → 95℃ (4 min) → 75℃ (8 min) was then performed. The thickness of the resulting gradient interface layer was initially measured using an ellipsometry on a polished single-crystal silicon reference sample treated with the same process, and calibrated using XPS argon ion etching depth profiling of the fiber sample. The total thickness of the interface layer was 80 nm.
[0052] Step S2: In the preparation stage of the photosensitive impregnation solution, the thermally conductive filler is first subjected to surface functionalization treatment. Boron nitride nanosheets are treated with oxygen plasma (power 100W, time 5min, O2 flow rate 50sccm) to introduce surface hydroxyl groups, and then mixed with spherical alumina at a mass ratio of 1.0:1. The mixture is then placed in an ethanol solution containing 1.5wt% silane coupling agent (KH-570) for high-speed shear dispersion. A chemical coating layer is constructed on the filler surface by reflux reaction at 70±2℃ for 4h. After centrifugation, washing, and vacuum drying at 80℃ for 2h, a surface-modified composite filler is obtained. The boron nitride nanosheets have a D50 particle size of 1μm and a thickness of 20nm, and the spherical alumina has a D50 particle size of 1μm.
[0053] Next, low-scattering photosensitive impregnation solution (A-resin) and high-thermal-conductivity photosensitive impregnation solution (B-resin) were prepared. Aliphatic bio-based polyurethane acrylate was selected as the core prepolymer, with a bio-based content of 30%, a weight-average molecular weight (M_w) of 5000, and an initial viscosity of 4000 mPa·s at 25°C. When preparing A-resin, 5 wt% of isobornyl acrylate (IBOA) was added to the above prepolymer as an reactive diluent, the content of the compound filler was controlled at 0 wt%, and 0.8 wt% of a compound photoinitiator (TPO-L and 1173 mixed at a mass ratio of 1.5:1) was added. The mixture was stirred in the dark at ≤25°C until the viscosity of the system reached 500 mPa·s.
[0054] When preparing the B-type adhesive, the amount of compound filler added was 20 wt%, and the amount of fluorosilicone modifier (molecular weight 2000, fluorine content 15%) added was set at 2.5 wt%. Simultaneously, 0.2 wt% fumed silica (specific surface area 200 m² / g) was additionally introduced into the system to construct a weak gel thixotropic network. The mixed slurry was circulated and milled three times using a three-roll mill with a roller gap of 10 μm, and finally degassed under a vacuum of -0.095 MPa for 15 min to obtain a high thermal conductivity photosensitive impregnating solution with a thixotropic index of 2.4 and a rotational viscosity of 3000 mPa·s at 25℃ and 20 rpm shear.
[0055] Step S3: A customized dual-cavity, multi-channel slit-type die is used to simultaneously apply the two adhesive solutions prepared in S2 to both sides of the preform. The die's interior uses high-precision machined isolation gaskets to completely isolate the flow channels. The upper chamber 21 connects to the upper lip, with an outlet slit width set to 0.10±0.02mm, used for applying adhesive A to the upper surface of preform 1; the lower chamber 22 connects to the lower lip, with an outlet slit width set to 0.15mm, used for applying adhesive B to the lower surface of preform 1. To prevent the A and B adhesive solutions from mixing at the outlet meniscus, the upper and lower lips are designed with isolation steps with a vertical misalignment height of 0.3mm, allowing the two adhesive solutions to adhere to the upper and lower surfaces of the preform as independent streams. For the antenna clearance area of the mobile phone back panel, a high-speed solenoid valve assembly linked to the die is used. For the antenna clearance area of the mobile phone back panel, a local switching process is implemented through a high-speed solenoid valve group (response time ≤ 5ms) linked with the mold head. The solenoid valve switching signal is set with advance based on the production line speed and the volume of the mold head flow channel, so that the A / B glue switching boundary error is controlled within ±0.5mm. A transition zone with a width of 3~8mm is formed between the high thermal conductivity zone and the low dielectric zone. The content of compound filler in the transition zone decreases along the in-plane direction. This area is only wetted by A glue.
[0056] Subsequently, the preform coated with an asymmetric adhesive layer, under the constraint of the tension control system, is immediately introduced into the roller impregnation zone composed of an upper flexible pressure roller 6 and a lower rigid metering roller 7. Upstream of the roller impregnation zone, a linearly tapering guide channel 3 is configured, with a total length of 32 mm and an inlet-to-outlet cross-sectional area ratio of 2.5:1. As the cross-sectional area linearly decreases, the adhesive liquid generates hydrodynamic pressure, which, in conjunction with the roller extrusion pressure, forces the high-viscosity B adhesive to overcome the penetration resistance of the fiber bundles and penetrate from bottom to top into the fiber core layer, while the surface A adhesive is kept in the near-surface region by the roller pressure flow restriction. Under the synergistic drive of the roller extrusion action and the linear vacuum gradient field below (increasingly distributed along the running direction) from -0.060 to -0.080 MPa, dense wetting of the material's interior is achieved.
[0057] An elastic lip seal 8 is installed at the outlet of the impregnation chamber to maintain a negative pressure environment within the chamber and to initially scrape off excess resin. Immediately following the lip seal is a pair of high-precision metering extrusion rollers 9, whose pressure is adjusted via a servo system to control the prepreg compression ratio at 15%. At the end of the production line, a β-ray areal density meter 4 is installed to scan and collect the total mass density data of the prepreg in real time. This monitoring system, together with the metering rollers and pump flow meter at the front end, forms a feedback loop: when an areal density deviation exceeding ±1.5% is detected, the system automatically fine-tunes the metering roller pressure and the die extrusion pressure, thereby anchoring the resin mass content of the final product at 40wt%.
[0058] After impregnation, the content of the compound filler in the 100μm thickness range near the outer surface is less than 10wt%, and the content of the compound filler in the 100μm thickness range near the internal heat source of the mobile phone is 20wt%, and the ratio of the content of the compound filler on both sides is 1.8:1.
[0059] After the continuous prepreg obtained in step S3 is cut to a fixed length or continuously wound, it is transferred to the lamination station for multi-layer assembly. The lamination process includes the following steps:
[0060] The prepregs are stacked with the low-scattering photosensitive impregnating liquid A side facing outwards and the high-thermal-conductivity photosensitive impregnating liquid B side facing each other. During stacking, mechanical blocks or a CCD vision alignment system are used to control the edge alignment deviation of each layer to ≤±0.5mm, ensuring that the in-plane functional zones (high thermal conductivity zone / low dielectric zone / transition zone) strictly coincide in the thickness direction.
[0061] After stacking, immediately apply uniform light pressure of 0.05~0.15MPa using a flexible silicone roller or plate, with the compaction time controlled between 10~30s. This pressure is only used to remove macroscopic air between layers and establish initial interfacial contact, avoiding excessive resin extrusion that could disrupt the filler gradient in the thickness direction. Preferably, a microporous vacuum adsorption platform (vacuum degree -0.02~-0.04MPa) is activated simultaneously with compaction to assist in extracting microbubbles between layers.
[0062] The lamination process should be carried out in an environment with a cleanliness level ≥ ISO 8, relative humidity ≤ 40%RH, and temperature 20±5℃. After lamination, the time interval between the laminate and the first-wavelength ultraviolet irradiation in step S4 should be ≤ 120 min (25℃ applicable period). If extended storage is required, it can be stored in a light-protected refrigerator at 4±1℃. Before use, it should be warmed at 20±5℃ for 30 min to restore the resin rheological properties.
[0063] The laminates are transferred to the curing unit via an anti-static conveyor belt or vacuum suction cup. Before entering the oven, edge positioning pins or flexible clamps are used to secure the laminates and prevent interlayer slippage during transport. The alignment deviation between the centerline of the laminate and the center of the optical path of the curing plate is ≤±1.0mm.
[0064] Step S4: After precise alignment, the laminated body is clamped between the upper and lower UV-transmitting quartz glass plates, and a precision airbag equalizing plate is configured (the airbag is located on the non-irradiated area on the back side of the quartz glass plate). Its pressure control system accuracy reaches ±0.005MPa. The initial constraint equalizing pressure is set to 0.30MPa.
[0065] Subsequently, 365nm first-band ultraviolet irradiation was initiated, with the irradiation intensity controlled at 150mW / cm². During this period, the C=C overtone absorption peaks in the 1610–1640nm band were monitored in real time using a dual-channel near-infrared (NIR) spectrometer (diffuse reflectance mode, spectral resolution 8cm²). -1 (Scanned 16 times), the conversion rate of the upper surface was calculated. Conversion rate with lower surface .
[0066] upper surface conversion rate Conversion rate with lower surface Calculate using the following formula:
[0067]
[0068] Where: A is the area of the C=C overtone absorption peak at 1610~1640nm (the peak boundary is determined by the second derivative spectroscopy method); A0 represents the reference peak area of CH that does not participate in the reaction (at approximately 1450 nm, corresponding to the methylene vibration of the polyurethane backbone); A0 represents the initial peak area before irradiation.
[0069] The peak area at irradiation time t; The peak area of the fully cured sample (heat cured at 120℃ for 2 hours).
[0070] To eliminate the scattering interference of high-filler B-type adhesive on the NIR signal, the original spectrum was preprocessed using the multivariate scattering correction (MSC) algorithm, and noise was reduced using Savitzky-Golay smoothing filter (11-point window, second-order polynomial).
[0071] The preset threshold for band switching is set to the upper surface conversion rate. Reaching 55%. When When this threshold is reached, the first band ends; if ΔR ≤ 15%, the standard second band curing procedure is executed; if ΔR > 15%, the initial light intensity of the second band is reduced and the irradiation time is extended until ΔR drops below 15%. Within a 2-second switching interval, the system automatically switches to the more penetrating 395nm second band, with the irradiation intensity correspondingly increased to 300mW / cm².
[0072] During the second-band ultraviolet irradiation, the system simultaneously executes a three-stage step-by-step pressure release procedure: first, the pressure is reduced from 0.30MPa to 0.25MPa at the beginning of the irradiation, then reduced to 0.20MPa in the middle of the irradiation, and finally maintained at 0.15MPa at the end of the irradiation.
[0073] Immediately after UV irradiation, the process proceeds to the infrared thermal equalization and post-curing stage. To obtain the temperature difference ΔT along the material thickness in real time, this process employs a strategy combining dual-channel infrared direct measurement and thermal conduction model estimation.
[0074] (1) Dual-channel direct measurement method: The surface temperature of the material is simultaneously acquired by a top infrared thermal imager (wavelength 8~14μm, spatial resolution ≤1mm) and a bottom infrared temperature probe (response time ≤100ms). With lower surface temperature ΔT = directly .
[0075] (2) Thermal conduction model estimation method: For samples with a thickness ≥0.85mm or high filler content (≥28wt%), a ΔT estimation model based on the thermal conduction equation is used in addition to the dual-channel direct measurement. This model uses a heat flow sensor (sensitivity ≥1μV / W) placed at the bottom of the curing stage and an infrared thermal imager at the top to measure the surface cooling slope monitored by matching it with a calibrated 0.6~0.9mm cross-section thermophysical parameter database, thereby deriving the real-time temperature difference ΔT between the core layer and the surface layer. The thermophysical parameter database is obtained by calibrating a calibration sample of the same thickness and formulation by embedding a miniature thermocouple (diameter ≤0.1mm).
[0076] In continuous production, the dual-channel direct measurement method is the main method. When the direct measurement ΔT fluctuation exceeds ±2℃, the model estimation method is activated for cross-validation.
[0077] Implement three-level hierarchical control based on the magnitude of ΔT:
[0078] When ΔT > 8℃, it indicates that the thermal field is severely uneven in the thickness direction. The infrared array power is set to 0.4W / cm² and applied for 25s to equalize the thermal field by slowing down the heating rate.
[0079] When 3℃<ΔT≤8℃, the thermal field is basically balanced but there is a local temperature difference. The power is compensated to 0.7W / cm² and applied for 18s to enhance the final crosslinking density.
[0080] When ΔT≤3℃ and lasts for 30~60s, it indicates that the material has reached a thermally stable state and is cured after the infrared radiation ends.
[0081] The entire process is combined with hot air circulation at 60±5℃ from the top to keep the upper limit of the material surface temperature below 75℃, ultimately producing a 0.6mm thick polyurethane composite material for the mobile phone back panel.
[0082] The aforementioned partitioned adhesive application process creates a low-dielectric-performance window in the antenna clearance area. Vector network analyzer testing, using the resonant cavity perturbation method (YD / T2583.1-2013), shows that the dielectric constant ε_r in the low-dielectric region is 3.2~3.6 in the 28GHz band, and the dielectric loss tangent tanδ≤0.008; while in the 5GHz band, tanδ≤0.012.
[0083] Example 2:
[0084] Step S1: First, a fiber preform was selected, consisting of two layers of plain weave fabric with a single-layer density of 210 g / m² and a single-layer thickness of 0.20 mm, resulting in a total thickness of 0.40 mm. The plain weave fabric was made by blending high-strength glass fiber with a single filament diameter of 9 μm and basalt fiber at a mass ratio of 8.0:2.0. The cleaning and drying process was the same as in Example 1. Plasma activation was performed using an Ar / O2 mixture with a volume ratio of 97:3, a processing power of 150 W, a processing speed of 2.0 m / min, and a nozzle distance of 3.5 mm. XPS measurements showed that the O / C ratio on the fiber surface increased to 0.35.
[0085] In the preparation of the grafting solution, the concentrations of KH-570, TMPTA / HDDA composite monomers, and photoinitiator were the same as in Example 1. The ultraviolet irradiation energy was increased to 800 mJ / cm², and the gradient heat treatment program was 75℃ (12 min) → 95℃ (6 min) → 75℃ (12 min). The total thickness of the interface layer was measured to be 120 nm.
[0086] Step S2: Boron nitride nanosheets, after being treated with oxygen plasma, are mixed with spherical alumina at a mass ratio of 1.5:1. The amount of silane coupling agent added is 2.0 wt%. The D50 particle size of the boron nitride nanosheets is 3 μm and the thickness is 50 nm, while the D50 particle size of the spherical alumina is 5 μm.
[0087] The matrix prepolymer has a bio-based content of 40%, a weight-average molecular weight (M_w) of 8000, and an initial viscosity of 5000 mPa·s. In adhesive A, the amount of IBOA added is 10 wt%, the content of compound fillers is 5 wt%, the amount of compound photoinitiator added is 1.2 wt%, and the system viscosity reaches 800 mPa·s.
[0088] The filler loading of the B-type compound was increased to 30 wt%. To address the viscosity surge caused by high filler content, the fluorosilicone modifier (molecular weight 3500, fluorine content 20%) was inversely reduced to 1.5 wt%, and the amount of fumed silica added was increased to 0.5 wt%. After three-roll milling (roller gap 30 μm, 3 cycles) and vacuum degassing, the viscosity of the B-type compound system was 6000 mPa·s, and the thixotropic index was 2.8.
[0089] Step S3: Other implementations are the same as in Example 1. The pressure is adjusted through a closed-loop servo system to control the compression ratio of the preform at 25%, anchoring the resin content of the final product to 42.5 wt%. The content of the compound filler in the 100 μm thickness range near the internal heat source of the mobile phone is 35 wt%, and the ratio of the compound filler content on both sides is 4.0:1. The obtained prepreg is stacked in three layers in the same direction (with the low-scattering photosensitive impregnating liquid A side facing outwards). The wet thickness after stacking is approximately 0.75 mm, and then proceeds to step S4 for constrained curing.
[0090] Step S4: Initial pressure is 0.40 MPa, irradiance of the first band (365 nm) is increased to 250 mW / cm², NIR monitoring logic is the same as in Example 1, and the switching threshold is set to R_top reach 65%. Irradiance of the second band (395 nm) is increased to 500 mW / cm², with a switching interval of 4 s.
[0091] Pressure step release procedure: 0.40MPa→0.30MPa→0.25MPa→0.20MPa.
[0092] Infrared post-curing graded control: When ΔT > 8℃, apply power of 0.6W / cm² for 25s; when 3℃ < ΔT ≤ 8℃, apply power of 0.8W / cm² for 18s; when ΔT ≤ 3℃ and continues for 30~60s, the curing process ends. The surface temperature throughout the process is ≤ 75℃.
[0093] A polyurethane composite material with a thickness of 0.9 mm was finally obtained. In the low dielectric region at 28 GHz, the dielectric constant ε_r is 3.6 and tanδ≤0.008.
[0094] Example 3:
[0095] Step S1: First, a fiber preform was selected, consisting of three layers of plain weave fabric with a single-layer density of 200 g / m² and a single-layer thickness of 0.10 mm, resulting in a total thickness of 0.30 mm. The plain weave fabric was made by blending high-strength glass fiber with a single filament diameter of 8 μm and basalt fiber at a mass ratio of 7.5:2.5. Plasma activation was performed using a 95:5 Ar / O2 mixed gas (140 W, 1.8 m / min, distance 3.0 mm). The grafting solution preparation and UV grafting process were the same as in Example 1, with a 365 nm irradiation energy of 700 mJ / cm². The gradient heat treatment program was 75℃ (10 min) → 95℃ (5 min) → 75℃ (10 min). The interface layer thickness was measured to be 100 nm, and the O / C ratio on the fiber surface was 0.30.
[0096] Step S2: Boron nitride nanosheets and spherical alumina are mixed at a ratio of 1.2:1, with 1.8 wt% silane coupling agent added. The BN nanosheets have a D50 diameter of 2 μm and a thickness of 35 nm, while the spherical alumina has a D50 particle size of 3 μm.
[0097] The matrix prepolymer has a bio-based content of 35%, Mw 6500, and a viscosity of 4500 mPa·s. In adhesive A, the IBOA content is 7.5 wt%, the compound filler content is 2.5 wt%, the compound photoinitiator content is 1.0 wt%, and the system viscosity is 650 mPa·s.
[0098] Glue B contains 25 wt% filler, 2.0 wt% fluorosilicone modifier (molecular weight 2750, fluorine content 17.5%), and 0.3 wt% fumed silica. After three-roll milling (roller gap 20 μm) and vacuum degassing, glue B has a viscosity of 4500 mPa·s and a thixotropic index of 2.6.
[0099] Step S3: Other implementations are the same as in Example 1. The pressure is adjusted through a closed-loop servo system to control the compression rate of the preform at 20%, anchoring the resin content of the final product to 45wt%. The content of the compound filler in the 100μm thickness range near the internal heat source of the mobile phone is 27.5wt%, and the ratio of the compound filler content on both sides is 2.9:1. The obtained prepreg is stacked in three layers in the same direction (with the low-scattering photosensitive impregnating liquid A side facing outwards). The wet thickness after stacking is approximately 0.78mm, and then proceeds to step S4 for constrained curing.
[0100] Step S4: Initial pressure equalization 0.35 MPa. 365 nm irradiance 200 mW / cm², 395 nm irradiance 400 mW / cm². R_top switching threshold 60%. When ΔR ≤ 15%, execute the standard procedure; when ΔR > 15%, reduce light intensity and extend irradiation time. Switching interval 3 seconds.
[0101] Pressure step release: 0.35MPa→0.28MPa→0.23MPa→0.18MPa.
[0102] Infrared post-curing: When ΔT > 8℃, power 0.5W / cm² for 23s; when 3℃ < ΔT ≤ 8℃, power 0.75W / cm² for 15s; when ΔT ≤ 3℃, continue for 45s and then stop.
[0103] A polyurethane composite material with a thickness of 0.75 mm was finally obtained, with a dielectric constant ε_r of 3.4 and tanδ≤0.008 in the low dielectric region at 28 GHz.
[0104] Comparative Example 1: To verify the necessity of the filler gradient in the thickness direction and the in-plane partitioned adhesive supply, this comparative example uses the matrix formulation and curing process of Example 3, but cancels the dual-cavity die head partitioned pre-coating and asymmetric impregnation, and instead premixes A and B adhesives in proportion to form a uniform impregnation solution (total filler content 25wt%), and cures it after conventional single-cavity impregnation and vacuum degassing.
[0105] The specific process is as follows: a single-cavity slit die is used to uniformly coat both sides of the preform with the impregnation solution, and then the preform is impregnated in a conventional impregnation tank (without a tapered channel or roller extrusion), with a constant vacuum of -0.070 MPa and a resin content controlled at 42.5 wt%. The curing process is the same as in Example 3.
[0106] Comparative Example 2: To verify the synergistic effect of closed-loop control of dual-surface conversion rate difference and pressure step release, this comparative example used all the raw materials and impregnation process of Example 3. In the curing stage, the near-infrared dual-probe differential monitoring was cancelled and replaced with fixed-time trigger band switching (365nm irradiation for 20s followed by direct switching to 395nm). A constant flat pressure of 0.35MPa was maintained throughout the UV curing period, and infrared post-curing was only performed after the UV curing was completed.
[0107] Comparative Example 3: To verify the effect of pressure step release in reducing residual stress and warpage, this comparative example uses the formulation and impregnation process of Example 3. During the curing stage, the dual-channel NIR monitoring and band switching logic are retained, but a constant pressure of 0.35 MPa is maintained during the second band of ultraviolet irradiation. No step release is performed. The pressure is only released to normal pressure after the UV irradiation ends and infrared post-curing is performed.
[0108] To verify the comprehensive performance of the polyurethane composite material for mobile phone back panels prepared by this invention, the following industry standards and equipment were used to test the samples obtained in each embodiment and comparative example:
[0109] Thickness test: Using a high-precision digital micrometer, 10 test points were evenly selected on the prepared sample and the average value was taken.
[0110] Dielectric properties (εr and tanδ): According to the YD / T2583.1-2013 communication industry standard, Keysight N5242B vector network analyzer with resonant cavity perturbation method was used to sample and test the antenna clearance area in the 28 GHz band, with an ambient temperature of 23±2℃ and a relative humidity of 50±5%.
[0111] Thermal conductivity in the thickness direction: According to ASTM E1461 standard, the thermal diffusivity of the sample in the heat source area was measured at 25°C using a NETZSCH LFA467 laser flare instrument, and the thermal conductivity in the thickness direction (Z-axis) was calculated by combining specific heat capacity and density.
[0112] Interlaminar shear strength (ILSS): According to GB / T30969-2014 or ISO14130 short beam shear test standards, the material was cut into 20*10 strips. An Instron 5969 universal testing machine was used, with the span set to 5 times the plate thickness and the indenter loading rate set to 1.0 mm / min. Five parallel samples were taken from each group, and the average value was calculated.
[0113] Warpage test: The composite material was cut into a standard mobile phone back panel size sample of 150*75*mm. After being placed in an environment of 25℃ and 50%RH for 24 hours, the surface of the sample was scanned using a 3D laser optical profilometer. The distance between the parallel planes where the highest point and the lowest point are located was taken as the warpage.
[0114] As shown in Table 1:
[0115]
[0116] Comparative Example 1 uses a traditional uniform impregnation process, resulting in a high-frequency dielectric loss of 0.028, which fails to meet the wave transmission requirements of 5G antennas. Furthermore, a large amount of filler is distributed at the interlayer bonding surface, causing the interlayer shear strength to drop to 11.8 MPa. Example 3, however, employs a dual-cavity mold head with partitioning and gradient impregnation, ensuring the antenna area remains purely A-resin-impregnated (tanδ reduced to 0.007), while achieving high thermal conductivity (1.55 W / m·K) in the central region. In addition, the gradient distribution avoids excessive disruption of the resin matrix continuity by the thermally conductive filler at the interface, allowing the material to maintain an excellent interlayer bonding strength of 15.6 MPa even at a thickness of 0.75 mm.
[0117] Comparative Example 2 eliminated NIR closed-loop feedback and used fixed-time irradiation. Under the masking of high-concentration B adhesive, the deeper layers were in an under-cured state, resulting in the lowest interlayer shear strength of 10.8 MPa across the entire field. Furthermore, due to inconsistent curing shrinkage in the thickness direction, the warpage was out of control, reaching as high as 0.85 mm. Example 3 relied on real-time NIR measurement of the conversion rate difference between the upper and lower surfaces to precisely trigger 395 nm transmitted light compensation, ensuring the uniformity of the crosslinked network in the thickness direction and stabilizing the mechanical strength from a chemical perspective.
[0118] Although Comparative Example 3 was fully cured, it maintained constant pressure during UV irradiation and failed to release volume shrinkage stress, resulting in a warpage of 0.58 mm after demolding, which could not meet the precision assembly requirements of mobile phones. Example 3 innovatively anchored the pressure step release and closed-loop conversion rate node, which enabled the polyurethane network to obtain an excellent stress relaxation window in the gel state, ultimately suppressing the warpage to 0.15 mm, and achieving a unity of mechanical properties and dimensional stability of ultra-thin sheets.
[0119] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any ordinary changes and substitutions made by those skilled in the art within the scope of the technical solutions of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing a polyurethane composite material for a mobile phone battery cover, characterized in that, Includes the following steps: S1: Glass fiber and basalt fiber are mixed and woven to form a fiber preform. After cleaning, drying and plasma activation, the fiber preform is immersed in a grafting solution containing silane coupling agent, acrylate monomer and photoinitiator. After ultraviolet irradiation and heat treatment, a gradient interface layer containing plasma-activated polar groups, silane anchoring structure and co-curable grafting structure containing acrylate double bond is formed on the fiber surface to obtain a gradient interface fiber preform. S2: Prepare low-scattering photosensitive impregnation solution A and high-thermal-conductivity photosensitive impregnation solution B respectively; the low-scattering photosensitive impregnation solution A comprises a bio-based polyurethane acrylate prepolymer with acrylate end groups, a reactive diluent, and a compound photoinitiator; the high-thermal-conductivity photosensitive impregnation solution B comprises a bio-based polyurethane acrylate prepolymer with acrylate end groups, a reactive diluent, a compound photoinitiator, a fluorosilicone modifier containing acrylate double bonds, and a surface-modified boron nitride nanosheet and spherical alumina compound filler; wherein, the content of the compound filler in the low-scattering photosensitive impregnation solution A is 0~5wt%, the content of the compound filler in the high-thermal-conductivity photosensitive impregnation solution B is 20~30wt%, and the amount of fluorosilicone modifier added is 1.5~2.5wt% of the total mass of the high-thermal-conductivity photosensitive impregnation solution B; S3: A dual-cavity, multi-channel slit mold is used to asymmetrically apply low-scattering photosensitive impregnating solution A and high-thermal-conductivity photosensitive impregnating solution B to the gradient interface fiber preform. Low-scattering photosensitive impregnating solution A is applied to the outer surface side and the position corresponding to the mobile phone antenna clearance area, while high-thermal-conductivity photosensitive impregnating solution B is applied to the position near the internal heat source side of the mobile phone. Subsequently, the coated gradient interface fiber preform is continuously passed through a tapered impregnation channel with an inlet-to-outlet cross-sectional area ratio of 2.0~3.0:
1. Impregnation and degreasing are performed in conjunction with a linear vacuum gradient field, online surface density feedback, and a glue control mechanism. The resulting prepreg has a resin content of 40~45wt%, and forms a low filler layer on the outer surface side, a thermally conductive filler enrichment layer on the internal heat source side, a low dielectric region corresponding to the mobile phone antenna clearance area, and a transition region between the high thermal conductivity region and the low dielectric region in the prepreg. S4: Place the prepreg between UV-transmitting plates for constraint curing, and then irradiate it with 365nm first-band UV light and 395nm second-band UV light in sequence; During the first-band ultraviolet irradiation, a dual-channel near-infrared spectrometer was used to monitor the C=C overtone absorption peak of acrylate in the 1610~1640nm band in real time, and the conversion rates of the upper surface R_top and the lower surface R_bottom of the prepreg were calculated. The switching from the first band to the second band is triggered based on the conversion rate R_top of the upper surface and the difference in conversion rates ΔR between the upper and lower surfaces; The constraint pressure was simultaneously released in a stepped manner during the second-band ultraviolet irradiation. After the second-band ultraviolet light irradiation is completed, infrared post-curing is performed, and the infrared power and infrared action time are adjusted according to the temperature difference ΔT in the thickness direction of the material to obtain a polyurethane composite material for the battery cover of the mobile phone body.
2. The method for preparing a polyurethane composite material for a mobile phone battery cover according to claim 1, characterized in that, In step S1, the mass ratio of glass fiber to basalt fiber is 7.0~8.0:2.0~3.0; the fiber preform is a plain weave fabric with a thickness of 0.20~0.40mm and a surface density of 190~210g / m², and the monofilament diameter of glass fiber and basalt fiber is 7~9μm.
3. The method for preparing a polyurethane composite material for a mobile phone battery cover according to claim 2, characterized in that, In step S1, plasma activation uses a mixture of Ar and O2 gas with a volume ratio of Ar to O2 of 93~97:3~7, a processing power of 130~150W, a processing speed of 1.5~2.0m / min, and a vertical distance of 2.5~3.5mm between the plasma nozzle and the surface of the fiber preform. After plasma activation, the O / C atomic ratio on the fiber surface is 0.25~0.
35.
4. The method for preparing a polyurethane composite material for a mobile phone battery cover according to claim 3, characterized in that, In step S1, the silane coupling agent is γ-methacryloxypropyltrimethoxysilane, and the acrylate monomers include trimethylolpropane triacrylate and 1,6-hexanediol diacrylate. The heat treatment employs a gradient process of holding at 75℃ for 8-12 minutes, holding at 95℃ for 4-6 minutes, and holding at 75℃ for 8-12 minutes, resulting in a gradient interface layer thickness of 80-120 nm.
5. The method for preparing a polyurethane composite material for a mobile phone battery cover according to claim 1, characterized in that, In step S2, the bio-based content of the bio-based polyurethane acrylate prepolymer with acrylate end groups is 30-40%, the weight-average molecular weight is 5000-8000, and the viscosity at 25°C is 4000-5000 mPa·s. The reactive diluent is isoborneol acrylate, added at a rate of 5-10 wt%. The composite photoinitiator is composed of TPO-L and 1173 in a mass ratio of 1.5:1, with an addition amount of 0.8~1.2wt%.
6. The method for preparing a polyurethane composite material for a mobile phone battery cover according to claim 1, characterized in that, In step S2, the boron nitride nanosheets are treated with oxygen plasma or dopamine-assisted coating before silanization. The boron nitride nanosheets have a D50 diameter of 1~3μm and a thickness of 20~50nm, while the spherical alumina has a D50 particle size of 1~5μm. The mass ratio of boron nitride nanosheets to spherical alumina is 1.0~1.5:
1. Surface modification uses a silane coupling agent containing double bonds to give the surface of the composite filler double bond groups that can participate in the photocuring reaction.
7. The method for preparing a polyurethane composite material for a mobile phone battery cover according to claim 1, characterized in that, In step S2, the high thermal conductivity photosensitive impregnation solution B also contains 0.2~0.5wt% fumed silica, and the thixotropic index of the high thermal conductivity photosensitive impregnation solution B is 2.4~2.
8. Fluorosilicone modifiers containing acrylate double bonds are matched according to the amount of compound filler added: When the amount of compound filler added is 20~23wt%, the amount of fluorosilicone modifier added is 2.0~2.5wt%. When the amount of compound filler added is 24~30wt%, the amount of fluorosilicone modifier added is 1.5~2.0wt%.
8. The method for preparing a polyurethane composite material for a mobile phone battery cover according to claim 1, characterized in that, In step S3, the dual-cavity multi-channel slit mold head includes independent channels, which are used to transport low-scattering photosensitive impregnation solution A and high-thermal-conductivity photosensitive impregnation solution B, respectively. The position corresponding to the mobile phone antenna clearance area is switched by a solenoid valve to apply only low-scattering photosensitive impregnating solution A; The width of the transition zone is 3~8mm, and the content of the composite filler in the transition zone gradually decreases from the high thermal conductivity zone to the low dielectric zone.
9. A method for preparing a polyurethane composite material for a mobile phone battery cover according to claim 4, characterized in that, In step S4, the ultraviolet-transmitting pressure plate is a quartz glass pressure plate; the intensity of ultraviolet light irradiation in the first band is 150~250mW / cm², and the intensity of ultraviolet light irradiation in the second band is 300~500mW / cm². The first wave of ultraviolet irradiation ends when R_top reaches 55-65%. If ΔR ≤ 15%, the second wave of ultraviolet irradiation is then executed. If ΔR > 15%, then reduce the initial irradiation intensity of the second band and extend the irradiation time of the second band until ΔR drops to below 15%. The constraint pressure is released in stages by reducing the initial pressure from 0.30 to 0.40 MPa to 0.15 to 0.25 MPa. The thickness-direction temperature difference ΔT is estimated by the top infrared temperature measurement value, the bottom heat flow value, and the calibrated thickness-direction heat conduction model. When ΔT > 8℃, the infrared power is 0.4~0.6W / cm²; when 3℃ < ΔT ≤ 8℃, the infrared power is 0.6~0.8W / cm²; when ΔT ≤ 3℃ and lasts for 30~60s, the infrared curing ends, and the material surface temperature does not exceed 75℃ during the infrared curing process.
Citation Information
Patent Citations
Composite organic ceramic material, mobile phone backboard and preparation method
CN111469518A
Production process and application of transparent 3D glass fiber board with textures
CN113681935A