Carbon fiber preforms, their preparation methods and applications

By setting needled carbon fibers with bent angles in the carbon fiber preform to form non-linear heat conduction channels, the problems of heat dissipation and thermal expansion resistance of brake discs are solved, and better heat dissipation and pressure resistance are achieved.

CN123104170APending Publication Date: 2026-11-17BYD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510621949.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Brake materials formed by traditional three-dimensional needle-punched fiber preforms exhibit significant strength anisotropy, making it difficult to improve the heat dissipation and thermal expansion resistance of the outer ring of the brake disc.

Method used

A carbon fiber preform is designed to form a non-linear heat conduction channel by setting a bending angle in the needled carbon fiber in the outer region, which counteracts the expansion displacement during thermal expansion and enhances the compressive strength.

Benefits of technology

It effectively improves the heat dissipation and pressure resistance of the brake disc edge, reducing the risk of cracking due to temperature changes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123104170A_ABST
    Figure CN123104170A_ABST
Patent Text Reader

Abstract

This invention provides a carbon fiber preform, its preparation method, and its applications. The carbon fiber preform includes at least one preform unit, which comprises multiple layers of composite carbon fiber stacked together. The preform unit includes an outer region and a middle region. The preform unit has needle-punched carbon fibers extending along a first direction, which is the stacking direction of the multiple composite carbon fiber layers. At least a portion of the needle-punched carbon fibers in the outer region have a bending angle in the first direction. The needle-punched carbon fibers have non-linear heat-conducting channels in the first direction, which can effectively suppress the uniformity of heat flow direction and reduce local hot spots. When used in brake discs, this can effectively improve heat dissipation at the edge of the brake disc. Furthermore, when the bent needle-punched carbon fibers expand due to heat, they can offset part of the expansion displacement of the carbon fiber preform, reducing the risk of brake disc edge expansion and cracking caused by temperature changes, thereby improving the compressive strength of the edge region of the carbon fiber preform.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of materials technology, specifically to carbon fiber preforms, their preparation methods and applications, and more specifically to carbon fiber preforms and their preparation methods, carbon fiber reinforced matrix composites and their preparation methods, brake discs and vehicles. Background Technology

[0002] Carbon fiber reinforced polymer (CFRP) is a functional material made with needle-punched carbon fiber preforms as reinforcement and resin-based, ceramic-based, or metal-based matrices as the matrix. CFRP has advantages such as low density, high strength, and fatigue resistance, making it suitable for use in brake components in the automotive and aerospace industries. The needle-punched carbon fiber preform, as the reinforcement in CFRP composites, is traditionally formed by repeatedly laying 0° unidirectional carbon fiber fabric, a mesh layer, and 90° unidirectional carbon fiber fabric, followed by needle punching. This results in brake materials with significant anisotropy in strength.

[0003] However, during high-speed braking, the inner and outer rings of the brake disc have different linear velocities, and the outer ring receives more heat, requiring better heat dissipation and resistance to thermal expansion. However, the strength anisotropy of the brake material formed by the current traditional three-dimensional needle-punched fiber preform is obvious, making it difficult to improve the heat dissipation of the outer ring of the brake disc. Summary of the Invention

[0004] This invention aims to at least partially solve one of the technical problems in the related art. Therefore, one object of this invention is to provide a carbon fiber preform with good heat dissipation at its edges, effectively improving the heat dissipation problem at the edges of brake discs.

[0005] In one aspect of the invention, a carbon fiber preform is provided. According to an embodiment of the invention, the carbon fiber preform includes at least one preform unit, the preform unit comprising multiple layers of composite carbon fiber stacked together, the preform unit including an outer region and an intermediate region surrounded by the outer region, the preform unit having needle-punched carbon fibers extending along a first direction, the first direction being the stacking direction of the multiple layers of composite carbon fiber, wherein at least a portion of the needle-punched carbon fibers located in the outer region have a bending angle in the first direction. Thus, the needle-punched carbon fibers located in the outer region of the preform unit have a bending angle in the first direction, that is, the needle-punched carbon fibers in the outer region of the carbon fiber preform are bent in the first direction. This results in a non-linear heat conduction channel in the needle-punched carbon fibers in the first direction, which can effectively suppress the uniformity of heat flow direction and reduce local hot spots. When this carbon fiber preform is used in a brake disc, it can effectively improve the heat dissipation at the edge of the brake disc; moreover, when the bent needle-punched carbon fibers expand due to heat, they can offset part of the expansion displacement of the carbon fiber preform, reducing the risk of brake disc edge expansion and cracking due to temperature changes, thereby improving the compressive strength of the edge region of the carbon fiber preform.

[0006] According to an embodiment of the present invention, in a second direction, in the direction from the edge of the preform unit toward the center, the bending angle of the needled carbon fiber gradually decreases, and the second direction intersects the first direction.

[0007] According to an embodiment of the present invention, the maximum value of the bending angle is 2° to 30°.

[0008] According to an embodiment of the present invention, the preform unit satisfies one of the following conditions: the preform unit includes 20 to 24 layers of the composite carbon fiber stacked together, and the maximum value of the bending angle is 2° to 10°; the preform unit includes 25 to 29 layers of the composite carbon fiber stacked together, and the maximum value of the bending angle is 11° to 20°; the preform unit includes 30 to 35 layers of the composite carbon fiber stacked together, and the maximum value of the bending angle is 21° to 30°.

[0009] According to an embodiment of the present invention, the preform unit includes a top surface and a bottom surface disposed opposite to each other in the first direction, the top surface being the side where needle punching is performed during the preparation of the preform unit, wherein the carbon fiber preform includes two preform units stacked together with the same number of composite carbon fiber layers, and the top surfaces of the two preform units are attached to each other and stacked.

[0010] According to an embodiment of the present invention, the composite carbon fiber layer includes a first composite carbon fiber layer and a second composite carbon fiber layer, wherein the first composite carbon fiber layer and the second composite carbon fiber layer are alternately stacked, wherein the first composite carbon fiber layer includes a 0° unidirectional carbon fiber fabric and a carbon fiber mesh layer stacked, and the second composite carbon fiber layer includes a 90° unidirectional carbon fiber fabric and the carbon fiber mesh layer stacked.

[0011] In another aspect of the present invention, a method for preparing the aforementioned carbon fiber preform is provided. According to an embodiment of the present invention, the method for preparing the carbon fiber preform includes a method for preparing at least one preform unit, the method of preparing the preform unit comprising: placing at least one annular composite carbon fiber layer in a limiting groove of a rotating table; and needle-punching the composite carbon fiber layer during rotation to obtain the preform unit. Thus, the preform unit prepared by the above method has needle-punched carbon fibers located in the outer region of the preform unit having a bending angle in a first direction, i.e., the needle-punched carbon fibers in the outer region of the carbon fiber preform are bent in the first direction. This results in a non-linear heat-conducting channel in the needle-punched carbon fibers in the first direction, which can effectively suppress the uniformity of heat flow direction and reduce local hot spots. When this carbon fiber preform is used in a brake disc, it can effectively improve the heat dissipation at the edge of the brake disc. Moreover, when the bent needle-punched carbon fibers expand due to heat, they can offset part of the expansion displacement of the carbon fiber preform, reducing the risk of brake disc edge expansion and cracking due to temperature changes, thereby improving the compressive strength of the edge region of the carbon fiber preform.

[0012] According to an embodiment of the present invention, the sidewall of the circular limiting groove is elastic.

[0013] According to an embodiment of the present invention, two preform units are prepared. The method for preparing the carbon fiber preform further includes: immersing the two preform units in a resin solution; and bonding the needle-punched sides of the two preform units together by hot pressing to obtain the carbon fiber preform.

[0014] According to an embodiment of the present invention, the resin in the resin solution includes one or more of phenolic resin, furan resin, polyimide, and asphalt; the hot-pressing bonding time is 60-180 min, the temperature is 130-200°C, and the pressure is 0.5-3 MPa.

[0015] In another aspect, the present invention provides a carbon fiber reinforced matrix composite material. According to an embodiment of the invention, the carbon fiber reinforced matrix composite material comprises the aforementioned carbon fiber preform. Thus, the carbon fiber reinforced matrix composite material exhibits good edge heat dissipation and compressive strength. Those skilled in the art will understand that the carbon fiber reinforced matrix composite material possesses all the features and advantages of the aforementioned carbon fiber preform, which will not be elaborated further here.

[0016] In another aspect, the present invention provides a method for preparing a carbon fiber reinforced matrix composite material. According to an embodiment of the present invention, the method for preparing the carbon fiber reinforced matrix composite material includes: subjecting the carbon fiber preform to chemical vapor infiltration treatment to obtain a carbon / carbon composite material; and subjecting the carbon / carbon composite material to silicon infiltration treatment to obtain the carbon fiber preform.

[0017] In another aspect, the present invention provides a brake disc. According to an embodiment of the invention, the brake disc comprises the aforementioned carbon fiber preform or the aforementioned carbon fiber reinforced matrix composite material. Thus, the brake disc has good edge heat dissipation and compressive strength. Those skilled in the art will understand that the brake disc possesses all the features and advantages of the aforementioned carbon fiber preform, which will not be elaborated further here.

[0018] In another aspect, the present invention provides a vehicle. According to an embodiment of the invention, the vehicle includes the aforementioned brake disc. Thus, the brake disc of the vehicle has good edge heat dissipation and pressure resistance.

[0019] Additional aspects and advantages of the invention will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of the invention. Attached Figure Description

[0020] The above and / or additional aspects and advantages of the present invention will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which:

[0021] Figure 1 This is a schematic diagram of the structure of a prefabricated unit in one embodiment of the present invention;

[0022] Figure 2 yes Figure 1 A magnified view of a portion of the image;

[0023] Figure 3 This is a top view of a prefabricated unit in another embodiment of the present invention;

[0024] Figure 4 This is a flowchart illustrating the preparation process of the carbon fiber preform in another embodiment of the present invention;

[0025] Figure 5This is a schematic diagram of the composite carbon fiber stack in another embodiment of the present invention;

[0026] Figure 6 This is a schematic diagram of the preparation of the preform unit in another embodiment of the present invention;

[0027] Figure 7 This is a schematic diagram of the preparation of the preform unit in another embodiment of the present invention;

[0028] Figure 8 This is a schematic diagram of the preparation of the preform unit in Comparative Example 1;

[0029] Figure 9 This is a schematic diagram of the cut sample strips of carbon fiber reinforced matrix composite material in the examples and comparative examples;

[0030] Figure 10 This is a scanning electron microscope image of a cross-section of a prefabricated unit in Example 1;

[0031] Figure 11 This is a scanning electron microscope image of a cross-section of a prefabricated unit in Example 2;

[0032] Figure 12 This is a scanning electron microscope image of a cross section of the carbon fiber preform in Comparative Example 1. Detailed Implementation

[0033] The present invention will be explained below with reference to embodiments. Those skilled in the art will understand that the following embodiments are for illustrative purposes only and should not be considered as limiting the scope of the invention. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be obtained commercially.

[0034] The present invention will now be described with reference to specific embodiments. It should be noted that these embodiments are merely descriptive and do not limit the present invention in any way.

[0035] In one aspect of the invention, a carbon fiber preform is provided. According to an embodiment of the invention, referring to... Figure 1 , Figure 2 and Figure 3 ( Figure 2 for Figure 1(Enlarged view of the partial structure within the dashed box) The carbon fiber preform includes at least one preform unit 10. The preform unit 10 includes multiple layers of composite carbon fiber 20 stacked together. The preform unit 10 includes an outer region S1 and an inner region S2 surrounded by the outer region S1. The preform unit 10 has needled carbon fibers 30 extending along a first direction Y, which is the stacking direction of the multiple layers of composite carbon fiber 20. At least a portion of the needled carbon fibers 30 located in the outer region S1 has a bending angle in the first direction Y. Therefore, the needled carbon fiber 30 located in the outer region S1 of the preform unit 10 has a bending angle α in the first direction, that is, the needled carbon fiber in the outer region of the carbon fiber preform bends in the first direction. Thus, the needled carbon fiber 30 has a non-linear heat conduction channel in the first direction, which can effectively suppress the uniformity of heat flow direction and reduce local hot spots. When this carbon fiber preform is used in a brake disc, it can effectively improve the heat dissipation at the edge of the brake disc. Moreover, when the bent needled carbon fiber 30 expands due to heat, it can offset part of the expansion displacement of the carbon fiber preform, reduce the risk of the brake disc edge expanding and cracking due to temperature changes, and thus improve the compressive strength of the edge region of the carbon fiber preform.

[0036] When preparing carbon fiber preforms using needle punching, some carbon fibers in the composite carbon fiber layer are guided by the needle from the second direction X to the first direction Y during the needle punching process, forming a three-dimensional carbon fiber structure. At least a portion of the carbon fibers in the first direction Y located in the outer region S1 are the aforementioned bent needle-punched carbon fibers.

[0037] In an embodiment of the present invention, the aforementioned bending angle refers to the angle between the straight line connecting the two ends of the needle-pierced carbon fiber and the first direction Y, i.e., as shown below. Figure 2 The bending angle α is shown (the angles α1, α2, and α3 are marked at different positions).

[0038] It needs to be further explained that, Figures 1 to 3 This is merely an illustrative example illustrating the bending angle of the needled carbon fiber 30 and the basic structure of the carbon fiber preform. The number of needled carbon fibers in the outer and middle regions is merely an example and not a limitation on the number of needled carbon fibers in the carbon fiber preform. Furthermore, in some embodiments of the present invention, the lengths of the needled carbon fibers 30 in the carbon fiber preform vary, and the number of composite carbon fiber layers 20 they penetrate also differs. Figure 1 As shown.

[0039] In some embodiments of the present invention, the carbon fiber preform can be annular in shape, such as... Figure 1 and 3 As shown (with a ring-shaped hole in the middle), it can also be circular.

[0040] According to an embodiment of the present invention, referring to Figure 1 and Figure 2 As shown, in the second direction X (where the second direction X intersects the first direction Y), the bending angle α of the needle-punched carbon fiber 30 gradually decreases from the edge of the preform unit 10 towards the center (i.e., from the outer region S1 towards the middle region S2, i.e., directions X1 and X2). Thus, the bending angle of the needle-punched carbon fiber at the outermost edge of the carbon fiber preform (or preform unit) is the largest. Therefore, the closer to the outer edge, the larger the bending angle of the needle-punched carbon fiber. The larger the bending angle, the better the heat conduction channel formed by the needle-punched carbon fiber, which can improve heat dissipation, avoid a single direction of heat transfer, effectively reduce local hot spots, and more effectively offset some of the expansion displacement of the carbon fiber preform, further reducing the risk of brake disc edge expansion and cracking.

[0041] In some specific embodiments, the first direction and the second direction can be substantially perpendicular to each other. In some specific embodiments, such as... Figure 1 and Figure 2 As shown, the needled carbon fiber 30 located in the middle region S2 can have no bending angle, that is, its length extension direction is basically consistent with the first direction Y.

[0042] According to some embodiments of the present invention, the maximum bending angle is 2° to 30°, such as 2°, 5°, 8°, 10°, 12°, 15°, 18°, 20°, 23°, 25°, 28°, 30°, etc. Bending angles within the above range can effectively improve the heat dissipation and compressive strength of the carbon fiber preform and the edge of the brake disc; moreover, angles within the above range are relatively easy to achieve during manufacturing.

[0043] According to some embodiments of the present invention, a preform unit includes multiple needled carbon fibers, and the bending angles of the multiple different needled carbon fibers can be the same or different. In actual processes, since the state of the needled material, including the needled process itself, cannot be exactly the same each time, the bending angles of the multiple needled carbon fibers in the same preform unit will not be exactly the same.

[0044] According to some embodiments of the present invention, the bending angle of the needled carbon fiber 30 in the preform unit is related to the number of composite carbon fiber layers 20. The more layers there are, the greater the maximum bending angle of the needled carbon fiber 30 in the preform unit. This better improves the problem of poor heat dissipation at the edge of the thicker carbon fiber preform. Moreover, during the needled process, since the composite carbon fiber layers are gradually added layer by layer as the needled process proceeds, the more layers added, the more needled times there are. In the more needled processes, the more times the composite carbon fiber layer is squeezed by the needles, thus producing a larger bending angle. Conversely, the fewer layers there are, the fewer needled times there are, and the fewer times the composite carbon fiber layer is squeezed by the needles, thus producing a relatively smaller bending angle. If a preform unit with fewer composite carbon fiber layers is needled more times, a larger bending angle can be obtained. However, more needled processes may damage the composite carbon fiber layers. Therefore, the more composite carbon fiber layers in the preform unit, the larger the bending angle is, and vice versa. Specifically as follows:

[0045] In some embodiments, the prefabricated unit 10 includes 20 to 24 layers of composite carbon fiber 20 stacked together, with a maximum bending angle of 2° to 10°. In other embodiments, the prefabricated unit 10 includes 25 to 29 layers of composite carbon fiber 20 stacked together, with a maximum bending angle of 11° to 20°. In still other embodiments, the prefabricated unit 10 includes 30 to 35 layers of composite carbon fiber 20 stacked together, with a maximum bending angle of 21° to 30°. This effectively improves the heat dissipation and compressive strength of prefabricated units of different thicknesses.

[0046] According to some embodiments of the present invention, referencing Figure 4 The preform unit 10 includes a top surface 11 and a bottom surface 12 disposed opposite to each other in the first direction Y. The top surface 11 is the side where needle punching is performed during the preparation of the preform unit 10. The carbon fiber preform 100 includes two preform units 10 stacked together with the same number of composite carbon fiber layers 20, and the top surfaces 11 of the two preform units 10 are bonded and stacked together. Thus, in the two bonded preform units, the bending angles of the needled carbon fibers at the same position are basically close or the same, and the needled carbon fibers at the two locations are like needled carbon fibers on the same curve. This can provide a better heat conduction channel and improve heat dissipation.

[0047] In some embodiments, the two prefabricated units can be bonded together with an adhesive, such as resin. Specifically, the resin can be one or more of phenolic resin, furan resin, polyimide, and bitumen.

[0048] According to some embodiments of the present invention, with reference to Figure 5 The composite carbon fiber layer 20 includes a first composite carbon fiber layer 21 and a second composite carbon fiber layer 22, which are alternately stacked. The first composite carbon fiber layer 21 includes a 0° unidirectional carbon fiber fabric 211 and a carbon fiber mesh layer 212 stacked together, and the second composite carbon fiber layer 22 includes a 90° unidirectional carbon fiber fabric 221 and a carbon fiber mesh layer 222 stacked together. Therefore, in the preform unit, the alternating arrangement of the three carbon fiber layers—0° unidirectional carbon fiber fabric 211 and carbon fiber mesh layer 212 (or 222), and 90° unidirectional carbon fiber fabric 221—can help improve the overall mechanical properties of the preform unit.

[0049] Among them, 0° carbon fiber unidirectional fabric refers to the fiber length direction being consistent with the main stress direction of the carbon fiber preform, which can provide the maximum longitudinal tensile strength and modulus, effectively withstand tensile and compressive loads along the fiber direction, and play a key role in bearing axial force, etc.; 90° carbon fiber unidirectional fabric has the fiber length direction perpendicular to that of 0° carbon fiber unidirectional fabric, mainly used to enhance the performance of carbon fiber preform in the transverse direction, which can improve the strength and stiffness of carbon fiber preform in the direction perpendicular to the fiber, enhance its shear and tear resistance, and help suppress deformation in this direction, making the mechanical properties of carbon fiber preform more balanced in different directions; the carbon fiber mesh layer is made of chopped carbon fiber or carbon fiber yarn interwoven, which has a certain degree of bulkiness and softness. In the carbon fiber preform, it plays a role in uniformly distributing fibers, increasing the connection points between fibers, and improving the overall toughness of carbon fiber preform. The carbon fiber mesh layer fills between 0° carbon fiber unidirectional fabric and 90° carbon fiber unidirectional fabric, which can improve the interlayer bonding performance, reduce the possibility of interlayer delamination, and also absorb impact energy to a certain extent, improving the impact resistance of the preform.

[0050] According to some embodiments of the present invention, the aforementioned carbon fiber preform may further include a carbon layer, which can be deposited by chemical vapor infiltration (CVI) into the pinholes of the preform unit and on the surface of the carbon fibers of the preform unit. By depositing the carbon layer, pores (such as pinholes) and defects in the carbon fiber preform can be filled, increasing the density of the carbon fiber preform, reducing internal porosity, and thus enhancing its mechanical and physical properties. Furthermore, the deposited carbon layer can form bridging and bonding between carbon fibers, effectively transferring loads between carbon fibers and improving interfacial strength. Additionally, the carbon layer has good thermal stability and thermal conductivity, which can further improve the heat dissipation performance of the carbon fiber preform, reduce localized thermal stress concentration, and improve its thermal expansion performance. It can also improve the chemical stability of the carbon fiber preform, such as enhancing its corrosion resistance.

[0051] According to some embodiments of the present invention, the aforementioned carbon fiber preform may further include a silicon layer, which is deposited on the surface of the carbon-deposited product by a silicon infiltration process. Thereby, silicon and carbon can react to form silicon carbide, creating a dense ceramic layer that effectively blocks oxygen diffusion into the interior, improving the preform's oxidation resistance. The generated silicon carbide can further enhance the preform's hardness, strength, and wear resistance, enabling it to withstand greater external forces. The high thermal conductivity of silicon carbide helps improve the preform's overall thermal conductivity, allowing heat to be quickly and evenly distributed within the preform, reducing localized hot spots, improving compressive strength and expansion resistance, and making the preform less prone to cracking or damage.

[0052] In another aspect, the present invention provides a method for preparing the aforementioned carbon fiber preform. According to an embodiment of the present invention, the method for preparing the carbon fiber preform includes a method for preparing at least one preform unit, referring to… Figure 6 The methods for preparing prefabricated units include:

[0053] S100: Place at least one annular composite carbon fiber layer 20 in the circular limiting groove 40 of the rotary table.

[0054] In some embodiments of the present invention, the size of the aforementioned limiting groove is substantially the same as the diameter of the composite carbon fiber layer, which not only allows for proper placement of the composite carbon fiber layer but also serves to limit its movement. In some specific embodiments, the ring can be a circular ring structure, and the limiting groove is an annular limiting groove. The rotating platform can rotate the circular limiting groove.

[0055] In some embodiments of the present invention, the sidewall 41 of the circular limiting groove 40 is elastic (or tough), and the material of the sidewall can be at least one of silicone, rubber, polyurethane, foam or thermoplastic elastomer (TPE).

[0056] S200: The composite carbon fiber layer 20 is needled during rotation to obtain the preform unit 10.

[0057] In some embodiments, as the needling proceeds, multiple layers of composite carbon fiber are gradually placed in a circular limiting groove. For example, one or two layers of composite carbon fiber can be added after several needlings.

[0058] According to embodiments of the present invention, a circular composite carbon fiber layer is used for needle punching. After needle punching, no further cutting is required, simplifying the process. Furthermore, directly using a circular composite carbon fiber layer for needle punching requires needle punching the entire plane of the composite carbon fiber layer, rather than a partial area, which allows for more uniform stress distribution during the needle punching process. In the above preparation process, when performing needle punching, if... Figure 7As shown, the needles compress the surrounding carbon fibers, causing them to expand outwards. The expanded carbon fibers then compress the sidewalls. Because the sidewalls are elastic, they can suppress the expansion to some extent. By using sidewalls made of different elastic materials, the expansion can be controlled. Due to the layered needle punching of the composite carbon fibers, the bottom layer has more needle punches and expands more. Therefore, the bottom end of the formed needled carbon fiber expands and moves outwards with the preform unit, while the upper end moves less, becoming a bent needled carbon fiber. The thicker the layer, the more the bottom bends, and the larger the bending angle. Furthermore, the bending of the needled carbon fiber can be controlled by selecting sidewalls with different degrees of softness. Better elasticity helps to increase the bending angle of the needled carbon fiber; poorer elasticity of the sidewall helps to obtain needled carbon fibers with smaller bending angles. Of course, the selection of sidewall materials also needs to consider their fixing and limiting function to prevent the material from detaching from the rotating table during the needle punching process, leading to process failure.

[0059] According to an embodiment of the present invention, the needled carbon fiber has a non-linear heat conduction channel in the first direction, which can effectively suppress the uniformity of heat flow direction and reduce local hot spots. When the carbon fiber preform is used in a brake disc, it can effectively improve the heat dissipation at the edge of the brake disc. Moreover, when the bent needled carbon fiber expands due to heat, it can offset part of the expansion displacement of the carbon fiber preform, reduce the risk of the brake disc edge expanding and cracking due to temperature changes, and thus improve the compressive strength of the edge area of ​​the carbon fiber preform.

[0060] According to some embodiments of the present invention, two preform units are prepared. The method for preparing the carbon fiber preform further includes S300: immersing the two preform units in a resin solution; and bonding the needle-punched sides of the two preform units together by hot pressing to obtain the carbon fiber preform. Thus, in the two bonded preform units, the bending angles of the needle-punched carbon fibers at corresponding positions are substantially close or the same, and the needle-punched carbon fibers at both locations are as if they were needle-punched carbon fibers on the same curve. This provides a better heat conduction channel and improves heat dissipation.

[0061] In some embodiments, the resin in the resin solution includes one or more of phenolic resin, furan resin, polyimide, and bitumen. The aforementioned resins have good adhesive properties, effectively bonding two precast units together and improving the stability of the composite precast structure.

[0062] In some embodiments, the hot-pressing time is 60–180 min (e.g., 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min, 130 min, 140 min, 150 min, 160 min, 170 min, 180 min, etc.), the temperature is 130–200℃ (e.g., 130℃, 140℃, 150℃, 160℃, 170℃, 180℃, 190℃, 200℃, etc.), and the pressure is 0.5–3 MPa (e.g., 0.5 MPa, 1 MPa, 1.5 MPa, 2 MPa, 2.5 MPa, 3 MPa, etc.). Therefore, under the above conditions, two prefabricated units can be quickly and effectively bonded together, and are not easily detached or separated.

[0063] In some embodiments, the mass concentration of resin in the resin solution can be 30% to 50%, which results in better bonding effect.

[0064] In another aspect, the present invention provides a carbon fiber reinforced matrix composite material. According to an embodiment of the invention, the carbon fiber reinforced matrix composite material comprises the aforementioned carbon fiber preform. Thus, the carbon fiber reinforced matrix composite material exhibits good edge heat dissipation and compressive strength. Those skilled in the art will understand that the carbon fiber reinforced matrix composite material possesses all the features and advantages of the aforementioned carbon fiber preform, which will not be elaborated further here.

[0065] In some embodiments of the present invention, the carbon fiber reinforced matrix composite material further includes silicon carbide material attached to the surface of the carbon fiber preform and the surface of the pinholes, forming a dense ceramic layer that can effectively block the diffusion of oxygen into the interior and improve the oxidation resistance of the preform. The generated silicon carbide can also further improve the mechanical properties of the preform, such as hardness, strength and wear resistance, so that it can withstand greater external forces. Silicon carbide has high thermal conductivity, which can help improve the thermal conductivity of the preform, so that heat can be quickly transferred to the interior of the preform and evenly distributed, with fewer local hot spots, improving compressive strength and expansion resistance, and making the preform less prone to cracking or damage.

[0066] In some embodiments of the present invention, the carbon fiber reinforced matrix composite material is a functional material prepared by using the carbon fiber preform of the present invention as the reinforcement and a resin matrix as the matrix.

[0067] In another aspect, the present invention provides a method for preparing a carbon fiber reinforced matrix composite material. According to an embodiment of the present invention, the method for preparing the carbon fiber reinforced matrix composite material includes: subjecting the aforementioned carbon fiber preform to chemical vapor infiltration treatment to obtain a carbon / carbon composite material; and subjecting the carbon / carbon composite material to silicon infiltration treatment to obtain the carbon fiber preform.

[0068] According to some embodiments of the present invention, a carbon layer is deposited in the needle holes of the aforementioned carbon fiber preform and on the surface of the carbon fibers of the carbon fiber preform by chemical vapor infiltration (CVI). By depositing the carbon layer, pores (such as needle holes) and defects in the carbon fiber preform can be filled, increasing the density of the carbon fiber preform, reducing internal porosity, and thus enhancing its mechanical and physical properties. Furthermore, the deposited carbon layer can form bridging and bonding between the carbon fibers, effectively transferring the load between the carbon fibers and improving interfacial strength. Additionally, the carbon layer has good thermal stability and thermal conductivity, which can further improve the heat dissipation performance of the carbon fiber preform, reduce localized thermal stress concentration, and improve its thermal expansion performance. It can also improve the chemical stability of the carbon fiber preform, such as enhancing its corrosion resistance.

[0069] According to some embodiments of the present invention, a silicon layer can be deposited by silicon infiltration treatment. Silicon and carbon can react to form silicon carbide, forming a dense ceramic layer that can effectively block the diffusion of oxygen into the interior and improve the oxidation resistance of the preform. The generated silicon carbide can also further improve the mechanical properties of the preform, such as hardness, strength, and wear resistance, so that it can withstand greater external forces. Silicon carbide has high thermal conductivity, which can help improve the thermal conductivity of the preform, so that heat can be quickly transferred to the interior of the preform and evenly distributed, with fewer local hot spots, improving compressive strength and expansion resistance, and making the preform less prone to cracking or damage.

[0070] According to some embodiments of the present invention, the temperature of chemical vapor infiltration (CVI) is 950-1300°C and the time is 100-300h. Under the above conditions, the deposition of a carbon layer can be effectively achieved. In other embodiments, the silicon infiltration temperature is 1650-1800°C and the holding time is 120-240min. Under the above conditions, the reaction between silicon and carbon can be effectively achieved to generate silicon carbide, which is strongly attached to the carbon fiber.

[0071] In another aspect, the present invention provides a brake disc. According to an embodiment of the invention, the brake disc comprises the aforementioned carbon fiber preform or the aforementioned carbon fiber reinforced matrix composite material. Thus, the brake disc has good edge heat dissipation and compressive strength. Those skilled in the art will understand that the brake disc possesses all the features and advantages of the aforementioned carbon fiber preform, which will not be elaborated further here.

[0072] In another aspect, the present invention provides a vehicle. According to an embodiment of the invention, the vehicle includes the aforementioned brake disc. Thus, the brake disc of the vehicle has good edge heat dissipation and pressure resistance.

[0073] Example

[0074] Example 1

[0075] Take 12K carbon fiber unidirectional fabrics with an areal density of 400 g / m² (0° and 90°), and a carbon fiber mesh layer with an areal density of 80 g / m², and use the following... Figure 6 The method of annular needle punching (with silicone on the sidewall of the circular limiting groove) is used to obtain two prefabricated units with 20 layers of composite carbon fiber. The maximum bending angle of the needle-punched carbon fiber in the prefabricated unit is 2°-10°. During the needle punching process, the first composite carbon fiber layer and the second composite carbon fiber layer are alternately stacked. The first composite carbon fiber layer includes a 0° carbon fiber unidirectional cloth and a carbon fiber mesh layer stacked together. The second composite carbon fiber layer includes a 90° carbon fiber unidirectional cloth and a carbon fiber mesh layer stacked together.

[0076] Two preform units were impregnated in a phenolic resin solution with a mass fraction of 40%, and then hot-pressed at a pressure of 1 MPa and a temperature of 150°C for 120 min to obtain a carbon fiber preform.

[0077] Carbon / carbon composite material was obtained by chemically vapor infiltrating carbon fiber preforms at 1150℃ for 200 hours.

[0078] Carbon / carbon composite materials were infiltrated with silicon at 1750°C for 3 hours to obtain carbon fiber reinforced matrix composite materials.

[0079] Example 2

[0080] Take 12K carbon fiber unidirectional fabrics with an areal density of 400 g / m² (0° and 90°), and a carbon fiber mesh layer with an areal density of 80 g / m², and use the following... Figure 6 The method of annular needle punching (with silicone on the sidewall of the circular limiting groove) is used to obtain two prefabricated units with 25 layers of composite carbon fiber. The maximum bending angle of the needle-punched carbon fiber in the prefabricated unit is 11°-20°. During the needle punching process, the first composite carbon fiber layer and the second composite carbon fiber layer are alternately stacked. The first composite carbon fiber layer includes a 0° carbon fiber unidirectional cloth and a carbon fiber mesh layer stacked together. The second composite carbon fiber layer includes a 90° carbon fiber unidirectional cloth and a carbon fiber mesh layer stacked together.

[0081] Two preform units were impregnated in a phenolic resin solution with a mass fraction of 40%, and then hot-pressed at a pressure of 1 MPa and a temperature of 150°C for 120 min to obtain a carbon fiber preform.

[0082] Carbon / carbon composite material was obtained by chemically vapor infiltrating carbon fiber preforms at 1150℃ for 200 hours.

[0083] Carbon / carbon composite materials were infiltrated with silicon at 1750°C for 3 hours to obtain carbon fiber reinforced matrix composite materials.

[0084] Example 3

[0085] Take 12K carbon fiber unidirectional fabrics with an areal density of 400 g / m² (0° and 90°), and a carbon fiber mesh layer with an areal density of 80 g / m², and use the following... Figure 6 The method of annular needle punching (with silicone on the sidewall of the circular limiting groove) is used to obtain two prefabricated units with 30 layers of composite carbon fiber. The maximum bending angle of the needle-punched carbon fiber in the prefabricated unit is 21°-30°. During the needle punching process, the first composite carbon fiber layer and the second composite carbon fiber layer are alternately stacked. The first composite carbon fiber layer includes a 0° carbon fiber unidirectional cloth and a carbon fiber mesh layer stacked together. The second composite carbon fiber layer includes a 90° carbon fiber unidirectional cloth and a carbon fiber mesh layer stacked together.

[0086] Two preform units were impregnated in a phenolic resin solution with a mass fraction of 40%, and then hot-pressed at a pressure of 1 MPa and a temperature of 150°C for 120 min to obtain a carbon fiber preform.

[0087] Carbon / carbon composite material was obtained by chemically vapor infiltrating carbon fiber preforms at 1150℃ for 200 hours.

[0088] Carbon / carbon composite materials were infiltrated with silicon at 1750°C for 3 hours to obtain carbon fiber reinforced matrix composite materials.

[0089] Comparative Example 1

[0090] Take 12K carbon fiber unidirectional fabrics with an areal density of 400 g / m² (0° and 90°), and a carbon fiber mesh layer with an areal density of 80 g / m², and use flat needle punching (e.g.) Figure 8 The carbon fiber preform is prepared by the method shown in the figure. During needle punching, the first composite carbon fiber layer and the second composite carbon fiber layer are alternately stacked. The first composite carbon fiber layer includes a 0° carbon fiber unidirectional cloth and a carbon fiber mesh layer stacked together. The second composite carbon fiber layer includes a 90° carbon fiber unidirectional cloth and a carbon fiber mesh layer stacked together. The number of composite carbon fiber layers is 50.

[0091] The carbon fiber preform was chemically vapor-impregnated at 1100℃ for 350 hours to obtain a carbon / carbon composite material.

[0092] Carbon / carbon composite material was infiltrated with silicon at 1700°C for 3 hours, and then carbon fiber reinforced matrix composite material was obtained by cutting.

[0093] Performance testing:

[0094] The cross-section of the prefabricated unit prepared in Example 1 was observed using scanning electron microscopy, as shown below. Figure 10 As shown; the cross-section of the prefabricated unit prepared in Example 2 was observed using a scanning electron microscope, as shown. Figure 11 As shown; the cross-section of the carbon fiber preform prepared in Comparative Example 1 was observed using a scanning electron microscope, as shown. Figure 12 As shown. By comparison, it can be found that compared with the needled carbon fiber in Comparative Example 1, the needled carbon fibers in Examples 1 and 2 both bend, and the bending angle in Example 2 is larger than that in Example 1. However, the needled carbon fiber in Comparative Example 1 hardly bends.

[0095] According to such Figure 9 As shown, sample strips were cut at the edges of the carbon fiber preforms prepared in Examples 1 to 3 and Comparative Example 1. Figure 9 The black squares in the table represent the cut sample strips (eight sample strips were cut from the edge of each carbon fiber preform). The sample strips were tested for compressive strength and coefficient of thermal expansion. The coefficient of thermal expansion was tested according to ASTM E228, the compressive strength according to ASTM D2344 / D2344M-13, and the thermal conductivity according to ASTM E1461. The silica-infiltrated carbon fiber reinforced matrix composite (or disc) was cut into test slices and tested at 400°C. The test results are shown in Table 1.

[0096] Table 1

[0097]

[0098] As can be seen from the data comparison in Table 1, compared with Comparative Example 1, the outer region of the carbon fiber preform in this embodiment has a lower coefficient of thermal expansion, higher thermal conductivity, and higher compressive strength. This indicates that the outer region of the carbon fiber preform of this invention still has better dimensional stability at higher temperatures, reduces expansion displacement, lowers the risk of edge expansion cracking, has good heat dissipation, and has strong compressive strength. When applied to brake discs, the brake discs exhibit better product performance during high-speed braking.

[0099] Furthermore, as can be seen from Examples 1 to 3, as the bending angle increases, the coefficient of thermal expansion of the carbon fiber preform is smaller and the compressive strength is better.

[0100] The terms "first" and "second" used in this document are for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Therefore, a feature marked "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of this application, "multiple" means two or more, unless otherwise explicitly specified.

[0101] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., refer to specific features, structures, materials, or characteristics described in connection with that embodiment or example, which are included in at least one embodiment or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.

[0102] Although embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of the present invention.

Claims

1. A carbon fiber preform, characterized in that, The device includes at least one preform unit, which comprises multiple layers of composite carbon fiber stacked together. The preform unit includes an outer region and a central region surrounded by the outer region. The preform unit has needle-punched carbon fibers extending along a first direction, which is the stacking direction of the multiple layers of composite carbon fiber. Wherein, at least a portion of the needled carbon fibers located in the outer region have a bending angle in the first direction.

2. The carbon fiber preform according to claim 1, characterized in that, In the second direction, which is the direction from the edge of the preform unit toward the center, the bending angle of the needled carbon fiber gradually decreases, and the second direction intersects the first direction.

3. The carbon fiber preform according to claim 1 or 2, characterized in that, The maximum value of the bending angle is 2° to 30°.

4. The carbon fiber preform according to claim 3, characterized in that, The prefabricated unit satisfies one of the following conditions: The prefabricated unit includes 20 to 24 layers of the composite carbon fiber layer, and the maximum value of the bending angle is 2° to 10°. The prefabricated unit includes 25 to 29 layers of the composite carbon fiber layer, and the maximum bending angle is 11° to 20°. The prefabricated unit includes 30 to 35 layers of the composite carbon fiber stacked together, and the maximum bending angle is 21° to 30°.

5. The carbon fiber preform according to any one of claims 1 to 4, characterized in that, The preform unit includes a top surface and a bottom surface disposed opposite to each other in the first direction. The top surface is the side where needle punching is performed when preparing the preform unit. The carbon fiber preform includes two preform units that are stacked and have the same number of composite carbon fiber layers, and the top surfaces of the two preform units are attached to each other and stacked.

6. The carbon fiber preform according to any one of claims 1 to 5, characterized in that, The composite carbon fiber layer includes a first composite carbon fiber layer and a second composite carbon fiber layer, which are alternately stacked. The first composite carbon fiber layer includes a 0° unidirectional carbon fiber fabric and a carbon fiber mesh layer stacked together, and the second composite carbon fiber layer includes a 90° unidirectional carbon fiber fabric and the carbon fiber mesh layer stacked together.

7. A method for preparing a carbon fiber preform according to any one of claims 1 to 6, characterized in that, The method includes a method for preparing at least one preform unit, the method of preparing the preform unit comprising: At least one annular layer of composite carbon fiber is placed in the limiting groove of the rotary table; During rotation, the composite carbon fiber layer is needle-punched to obtain a preform unit.

8. The method according to claim 7, characterized in that, The sidewalls of the limiting groove are elastic.

9. The method according to claim 7 or 8, characterized in that, The method for preparing the carbon fiber preform further includes: preparing two preform units. The two preform units are immersed in a resin solution; The carbon fiber preform is obtained by bonding the two preform units together by needle-punching the sides using a hot-pressing method.

10. The method according to claim 9, characterized in that, The resin in the resin solution includes one or more of phenolic resin, furan resin, polyimide, and asphalt; The hot-pressing bonding time is 60–180 min, the temperature is 130–200 °C, and the pressure is 0.5–3 MPa.

11. A carbon fiber reinforced matrix composite material, characterized in that, Includes the carbon fiber preform according to any one of claims 1 to 6.

12. A method for preparing the carbon fiber reinforced matrix composite material according to claim 11, characterized in that, include: Chemical vapor infiltration treatment is performed on the carbon fiber preform according to any one of claims 1 to 6 to obtain a carbon / carbon composite material; The carbon / carbon composite material is subjected to silicon infiltration treatment to obtain the carbon fiber reinforced matrix composite material.

13. A brake disc, characterized in that, Includes the carbon fiber preform according to any one of claims 1 to 6 or the carbon fiber reinforced matrix composite material according to claim 11.

14. A vehicle, characterized in that, Includes the brake disc as described in claim 13.