A composite reinforced base and its application in impermeable boards
By designing a composite reinforced base, utilizing a fiber mesh structure and hydrolysis-resistant treatment, the problem of poor interfacial bonding between the polymer membrane and the modified asphalt coating material was solved, thereby improving the impermeability and mechanical properties under high-temperature construction and long-term water immersion environments.
Patent Information
- Application Number
- CN202611368060.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-04
- Publication Date
- 2026-11-17
AI Technical Summary
In existing technologies, the interfacial bonding between polymer films and modified bitumen coatings is poor, making them unable to withstand high-temperature construction. Furthermore, they are prone to interlayer slippage under long-term water immersion conditions, failing to meet the stringent environmental requirements of building waterproofing and water conservancy projects.
The composite reinforced base consists of an upper geotextile layer, a polymer membrane layer, and a lower geotextile layer. Through fiber mesh structure and hydrolysis-resistant treatment, an integrated composite structure of modified asphalt coating layer/upper geotextile layer/polymer membrane layer/lower geotextile layer is formed, ensuring good bonding interface and durability.
It achieves non-deformation of composite reinforced base under high-temperature construction, possesses excellent seepage prevention and mechanical properties, and is suitable for long-term durability requirements such as pumped storage power stations, solving the problem of poor bonding between polymer membrane and modified asphalt coating.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This application belongs to the field of seepage-proof materials technology, and in particular relates to a composite reinforced base and its application in seepage-proof boards. Background Technology
[0002] In the field of geotechnical seepage prevention, the composite structure of "two fabrics and one membrane" consisting of geotextile / polymer membrane / geotextile membrane is mainly used for isolation, reverse seepage and surface seepage prevention in dams and landfills. The application of this structure in the geotechnical field is to lay it independently (geomembrane + geotextile are laid separately or pre-composite and directly used as seepage prevention layer), and it has never been used as a reinforcing base in modified bitumen waterproof membranes. Summary of the Invention
[0003] To address the aforementioned technical problems, this application provides a composite reinforced substrate and its application in a seepage-proof board, aiming to at least partially solve the above-mentioned technical problems. The technical solution provided by this application is as follows.
[0004] As a first aspect of this application, a composite reinforced substrate is provided, comprising an upper geotextile layer, a polymer membrane layer, and a lower geotextile layer; wherein the upper geotextile layer and the lower geotextile layer have a fiber mesh structure.
[0005] As a second aspect of this application, the application of composite reinforced substrate in impermeable boards is provided.
[0006] Based on the above technical solution, the composite reinforced base provided in this application and its application in the impermeable board have at least one of the following beneficial effects:
[0007] (1) In this application, a composite reinforced base with a two-layer geotextile / one-layer membrane structure is provided, which is formed by an upper geotextile layer / polymer membrane layer / lower geotextile layer. Utilizing the fiber mesh structure in the geotextile layer, which can be impregnated and anchored by the modified asphalt coating applied to its surface, an integrated composite structure of modified asphalt coating layer / upper geotextile layer / polymer membrane layer / lower geotextile layer / modified asphalt coating layer is formed, solving the technical problem of poor interfacial bonding between a single-layer polymer membrane and modified asphalt coating. By utilizing the composite structure formed by the upper geotextile layer / polymer membrane layer / lower geotextile layer, excellent seepage prevention performance is ensured while maintaining support and mechanical properties. By optimizing the weight ratio of the geotextile layer and the thickness ratio of the polymer membrane layer, a balance between mechanical properties and construction conformability is achieved, while also enabling the composite reinforced base to withstand the high temperature (160-190℃) of the modified asphalt coating and long-term durability.
[0008] (2) In this application, a composite reinforced base with a two-layer fabric and one-layer membrane structure is applied to the impermeable board, so that the impermeable board has excellent mechanical properties, impermeability, puncture resistance or water impact resistance, water pressure stratification resistance, buoyancy resistance and long-term water immersion durability. Detailed Implementation
[0009] Polymer membranes are widely used as seepage prevention materials due to their excellent seepage prevention and mechanical properties. However, they cannot be directly used as seepage prevention layers on asphalt concrete dam surfaces because of their poor compatibility with asphalt concrete, their inability to withstand the high temperatures during the construction of modified asphalt concrete, their lower density than water, and their tendency to float.
[0010] A single-layer polymer membrane is used as the base layer and combined with modified bitumen coating to form a single-layer modified bitumen waterproof membrane, mainly for the building waterproofing field. However, the polymer membrane has low surface energy, weak polarity, and poor wettability with modified bitumen. It is prone to interlayer slippage under long-term water immersion, making it unsuitable for hydraulic engineering, especially in harsh environments such as high water pressure (above 1.5MPa), high frequency (4-6 times / day) water level changes, long-term water immersion, alternating wet and dry conditions, and freeze-thaw cycles.
[0011] The two-layer geotextile and one-layer membrane structure is common in the field of geotechnical seepage prevention, mainly used for isolation, filtration and seepage prevention in dams and landfills. However, this application uses a polymer membrane as the middle layer of modified bitumen waterproof membrane or seepage prevention board, and sets geotextile with fiber mesh structure on both sides to form a composite reinforced base with a two-layer geotextile and one-layer membrane structure. It has the high seepage prevention and high strength of polymer membrane, and can withstand the high temperature (160-190℃) during the construction of modified bitumen coating material, meeting the requirements of long-term durability, seepage prevention and high strength of pumped storage power station.
[0012] Table 1 below provides a detailed comparative analysis of the differences between the geomembrane with a two-layer fabric and one-layer membrane structure in the prior art and the composite reinforced geomembrane with a two-layer fabric and one-layer membrane structure in this application.
[0013] Table 1
[0014]
[0015] As a first aspect of this application, a composite reinforced base is provided, which consists of an upper geotextile layer, a polymer membrane layer and a lower geotextile layer; wherein the upper geotextile layer and the lower geotextile layer have a fiber mesh structure.
[0016] In this application, a composite reinforced base formed by an upper geotextile layer, a polymer membrane layer, and a lower geotextile layer is suitable as a base layer for modified bitumen waterproof membranes or geomembranes. The lower geotextile layers have a fiber mesh structure, which can be fully impregnated with the modified bitumen coating, forming a physically anchored "integrated composite structure of modified bitumen coating layer / upper geotextile layer / polymer membrane layer / lower geotextile layer / modified bitumen coating layer," providing a good bonding interface with the modified bitumen coating layer and solving the technical problem of poor interfacial bonding between a single-layer polymer membrane and the modified bitumen coating. Simultaneously, the flexibility of the upper and lower geotextile layers compensates for the relatively hard texture of the polymer membrane layer, improving the overall conformability of the modified bitumen waterproof membrane or geomembrane. The intermediate polymer membrane has excellent tensile strength (up to 30-60 kN / m) and impermeability (impermeability coefficient <10). -11 (cm / s) is the core contributing layer that gives the composite reinforced base excellent mechanical properties and impermeability.
[0017] In some implementations, the upper and lower geotextile layers require hydrolysis-resistant treatment to ensure that the mechanical properties are retained at 85% or higher after long-term water immersion. The hydrolysis-resistant treatment methods include using a monoepoxy polyester end-capping hydrolysis-resistant agent to treat the upper and lower geotextile layers. The mechanism can be understood as follows: the monoepoxy end-capping agent reacts with the carboxyl groups (-COOH) at the ends of the polyethylene terephthalate (PET) molecular chains, sealing the active end groups and thus inhibiting the hydrolytic breakage of the molecular chains under hot water and acid / alkali environments, ensuring that the strength retention rate of the upper and lower geotextile layers is ≥85% after immersion in hot water at 40°C for 90 days.
[0018] The specific anti-hydrolysis treatment process includes the following steps:
[0019] 1. Impregnation: Add 0.8-1.2wt% of anti-hydrolysis agent and 25%-30% of liquid carry-over rate during rolling. The purpose is to ensure that the end-sealing agent is evenly adhered to the fiber surface.
[0020] 2. Pre-drying: 120℃ for 3 minutes to fully evaporate the solvent.
[0021] 3. Curing and setting at 185-195℃ for 20-30 seconds allows the sealing agent to react with the carboxyl groups at the PET ends for sealing.
[0022] 4. Natural cooling and winding completes the hydrolysis resistance modification.
[0023] In some implementations, the basis weight of the upper geotextile layer and the lower geotextile layer are each independently 50-200 g / m². 2 For example, it can be 50g / m 2 80g / m 2 100g / m 2120g / m 2 150g / m 2 180g / m 2 200g / m 2 etc., or any value within this range, preferably 150-200 g / m 2 The thickness of the polymer membrane layer is 0.3-1.0 mm, for example, it can be 0.3 mm, 0.5 mm, 0.7 mm, 0.8 mm, 1.0 mm, etc., or any value within this range, preferably 0.5 mm-1.0 mm. By optimizing the ratio of the geotextile layer's basis weight to the polymer membrane layer's thickness, a balance between mechanical properties and construction conformability is achieved, while also enabling the composite reinforced base to withstand the high temperatures (160-190℃) of modified asphalt coating and to maintain long-term durability.
[0024] In some implementations, the peel strength between the upper and lower geotextile layers and the polymer film layer is ≥3.0 N / cm, thereby ensuring that the composite reinforced base does not exhibit internal delamination under high water pressure (≥1.5 MPa).
[0025] In some embodiments, the temperature of the modified bitumen coating material in the modified bitumen waterproof membrane or seepage barrier is as high as 160-190℃. The intermediate polymer film layer is required to remain stable at this temperature (i.e., not curling or peeling at the edges). Therefore, the Vicat softening temperature of the polymer film layer is ≥120℃ (GB / T 1633-2025), and the heat shrinkage rate at 190℃ is ≤2.0wt% (GB / T 12027-2004). The polymer film layer that meets the above requirements will not undergo significant heat shrinkage or deformation during the application of the modified bitumen coating material, ensuring the flatness and dimensional stability of the substrate.
[0026] In some embodiments, the composite quality of the reinforced base material directly affects its anti-delamination ability. The upper and / or lower geotextile layers are bonded to the polymer membrane layer via thermal bonding or adhesive bonding, with thermal bonding being preferred. By optimizing the thermal bonding process parameters, the interfacial bonding strength between the upper and lower geotextile layers and the polymer membrane layer is ensured. Therefore, the thermal bonding temperature in this application is 140-180℃, and the thermal bonding pressure is 0.3-0.8 MPa. If the thermal bonding temperature is too low (e.g., <140℃), the surface of the polymer membrane layer will not soften sufficiently, resulting in insufficient bonding strength with the geotextile layer; if the thermal bonding temperature is too high (e.g., >180℃), it will cause thermal shrinkage or degradation of the polymer membrane layer, which is detrimental to adhesion and impermeability. Furthermore, appropriate thermal bonding pressure facilitates the embedding of fibers from the geotextile layer into the polymer membrane, forming a certain mechanical anchoring effect, and can also improve interfacial bonding strength, preventing delamination.
[0027] In some embodiments, the material of the polymer membrane layer is selected from at least one of high-density polyethylene (HDPE) and polyvinyl chloride (PVC), preferably HDPE membrane. The aforementioned polymer membrane layer material has excellent impermeability, mechanical properties, and hydrolysis resistance.
[0028] In some embodiments, the upper geotextile layer and / or the lower geotextile layer are polyester geotextiles woven from core-sheath composite fibers, including a sheath layer and a core layer. The sheath layer is a light rare earth element-modified copolyester, which is a copolymer of sodium isophthalate sulfonate (SIPA) and polyester. The core layer comprises nano-montmorillonite-modified polyester, which may be polyethylene terephthalate (PET).
[0029] In this application, SIPA is copolymerized with polyester to form a copolyester. The light rare earth elements are anchored by the network structure of the copolyester and the chemical bonding between the light rare earth elements and the ester groups in the copolyester, thus obtaining a light rare earth element-modified copolyester (i.e., the sheath of the core-sheath composite fiber). Furthermore, the light rare earth elements, acting as coordination centers, can form coordination bonds with polar groups such as carboxyl groups (-COOH) and hydroxyl groups (-OH) in the modified asphalt coating, enhancing the interfacial bonding between the matrix asphalt and the sheath. They can also coordinate with the ester groups in the sheath, thus achieving chemical bonding between the modified asphalt coating and the core-sheath composite fiber through the coordination effect of the light rare earth elements. This forms a molecular bridge between the modified asphalt coating and the core-sheath composite fiber, significantly enhancing the interfacial bonding between the modified asphalt coating and the composite reinforcing base. Simultaneously, it can inhibit the migration and overflow of asphalt components during long-term use, ensuring the long-term stability of the seepage prevention performance of the modified asphalt waterproof membrane or geomembrane. Furthermore, light rare earth elements can absorb ultraviolet light and quench free radicals, giving the base layer excellent anti-aging properties. In the core layer, the layered structure of nano-montmorillonite is utilized to uniformly peel and disperse the layered nano-montmorillonite in the polyester, forming a nanoscale interpenetrating network structure. This enhances the strength and modulus of the core-sheath composite fiber, while the labyrinth effect of the nano-montmorillonite layered structure blocks water molecule penetration, enhancing the impermeability of the geotextile. Through the combined action of the sheath and core layers, the polyester geotextile woven with core-sheath composite fibers exhibits significantly improved fatigue resistance, elasticity, toughness, anti-aging properties, and water immersion resistance.
[0030] Furthermore, the outer layer is a copolyester formed by the copolymerization of SIPA and polyester. Its molecular chain contains high-density polar functional groups (sulfonic acid groups and ester groups), which form stable coordination chemical bonds / ionic bonds with light rare earth elements. This anchors the light rare earth elements in situ within the copolyester network, preventing their loss during processing and service. Although the core layer contains ester groups, it is only ordinary PET and lacks strong coordination groups such as sulfonic acid groups. Its binding force to rare earth ions is weak, and it cannot adsorb light rare earth elements. Therefore, the light rare earth element components are stably enriched in the outer layer, achieving enhanced interfacial bonding with the modified bitumen. In addition, the interface between the outer layer and the core layer is dense, and the light rare earth elements are locked in the outer layer by chemical coordination / ionic bonds, with no molecular diffusion channels, enabling it to function effectively for a long time.
[0031] In some implementations, the weight ratio of the cortex to the core is 5-10:95-90, for example, it can be 5:95, 8:92, 10:90, or any value within this range.
[0032] In some embodiments, based on copolyester, the addition amount of light rare earth element complex is 0.5-1.0 wt%, for example, 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%, 0.9 wt%, 1.0 wt%, or any value within this range. A small amount of light rare earth element complex can achieve coordination and anti-aging effects. During the preparation of the skin layer, the feed material in the system is the light rare earth element complex, and the final effective anchoring component is the light rare earth element. Specifically, the light rare earth element complex is composed of 20% La2O3, 45% CeO2, and 5% Pr6O3. 11 The mixture was synthesized with an elemental ratio of 30% Nd₂O₃, based on a copolyester, with the addition of light rare earth element complexes at a rate of 0.5-1.0 wt%. During the blending process, light rare earth element ions react with sulfonic acid groups (-SO₃) on the copolyester molecular chain. - It forms coordination / ionic bonds with ester groups (-COO-), and is chemically anchored in situ in the skin layer, thus remaining stable and not migrating or being lost during subsequent high-temperature spinning to form core-sheath composite fibers, thermal bonding, asphalt coating and other subsequent processing and long-term service.
[0033] In some embodiments, the interlayer spacing of nano-montmorillonite is ≥3.0 nm, and the amount of nano-montmorillonite added is 0.3-0.8 wt% based on polyester, for example, it can be 0.3 wt%, 0.4 wt%, 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt% or any value within this range.
[0034] In some embodiments, the core layer further includes: 0.1-0.2 wt% flowability improver and / or 1.0-2.0 wt% compatibilizer, wherein the compatibilizer is polyester-grafted maleic anhydride, that is, maleic anhydride is grafted onto polyester segments. The introduced maleic anhydride (MAH) groups can form chemical bonds with the hydroxyl groups on the surface of nano-montmorillonite, thereby improving the compatibility between nano-montmorillonite and polyester. The flowability improver can be rheology modifier RC-610, used to inhibit intermolecular hydrogen bonding, reduce apparent viscosity, and thus improve the flowability of the core layer melt and reduce the spinning breakage rate.
[0035] In some embodiments, the preparation method of the above-mentioned core-sheath composite fiber includes: steps 1-3.
[0036] Step 1: The light rare earth element complex and the copolyester are fed into a twin-screw extruder for melt mixing, and then extruded and granulated to obtain the skin-modified material (i.e., light rare earth element modified copolyester).
[0037] Step 2: The polyester and nano-montmorillonite are fed into a twin-screw extruder for melt mixing, and then extruded and granulated to obtain the core layer modified material.
[0038] Step 3: Feed the modified sheath material and the modified core material into the sheath-core composite spinning assembly, and after extrusion, stretching, and heat setting, obtain the sheath-core composite fiber.
[0039] In this application, during the preparation of the skin layer, the feed material in the system is a light rare earth element complex, and the final effective anchoring component is a light rare earth element.
[0040] In some embodiments, the temperature of the melt mixing in the twin-screw extruder in steps 1-2 is 260-280°C, the rotation speed of the twin screw is 200-400 rpm, and the residence time is 1-3 min.
[0041] In some embodiments, the core-sheath composite fiber is woven using a core-sheath composite spinning process in step 3. During the spinning process, the modified sheath material and the modified core material are fed into the core-sheath composite spinning assembly respectively, and the spinning temperature is controlled at 275-285℃, the stretch ratio is controlled at 3.5-4.5 times, and the heat setting temperature is set at 180-200℃. The resulting core-sheath composite fiber has excellent mechanical properties.
[0042] As a second aspect of this application, the application of composite reinforced substrate in seepage barrier boards is provided, particularly the application of seepage barrier boards in the field of water conservancy engineering.
[0043] In some embodiments, the asphalt impermeable board includes the aforementioned composite reinforced base and a modified asphalt coating applied to the upper and lower surfaces of the composite reinforced base, which, after curing, forms a modified asphalt coating layer.
[0044] In some embodiments, the geomembrane or modified bitumen waterproof membrane made from the composite reinforced substrate provided in this application can be used for industrial applications in fields such as seepage prevention of rockfill concrete-faced dams in pumped storage power stations, seepage prevention of roller-compacted concrete dams, lining of water conveyance tunnels, or seepage prevention of sluice gate bottom slabs. The composite reinforced substrate and geomembrane containing it provided in this application have a relatively simple process and widely available raw materials, and can be mass-produced using existing geomembrane composite production lines.
[0045] In some implementations, to ensure that the impermeable sheet or modified bitumen waterproof membrane can meet the requirements of pumped storage power stations under long-term water immersion, thermal aging, water pressure cycle fatigue, wet-dry alternation, and freeze-thaw cycles, the following durability design is required:
[0046] 1) Hydrolysis-resistant design: HDPE membrane has excellent hydrolysis resistance and will be used as the middle polymer membrane layer. At the same time, the polyester geotextile is treated with hydrolysis resistance to ensure that the mechanical properties are retained at ≥85% under long-term water immersion.
[0047] 2) Thermal aging stability: HDPE film has excellent thermal stability, and its tensile strength retention rate is ≥90% after thermal aging at 80℃ for 168h.
[0048] 3) Chemical corrosion resistance: HDPE membrane is resistant to acid, alkali and salt corrosion, and is suitable for various water quality environments.
[0049] 4) Resistance to biological attack: HDPE membranes are not easily attacked by microorganisms and algae, ensuring long-term service stability.
[0050] 5) Resistance to water pressure cycle fatigue: The integrated composite structure of modified asphalt coating layer / upper geotextile layer / polymer film layer / lower geotextile layer / modified asphalt coating layer ensures interface stability under high frequency water pressure fluctuations.
[0051] The following detailed description, in conjunction with specific embodiments, illustrates the composite reinforced substrate of this application and its application in impermeable boards.
[0052] The raw materials used in the embodiments and comparative examples of this application, as well as their specifications, sources, and parameters, are shown in Table 2 below.
[0053] The test samples and test items in the embodiments and comparative examples of this application are shown in Table 3 below.
[0054] The test methods for the composite reinforced base material in the embodiments and comparative examples of this application are shown in Table 4 below.
[0055] Table 2
[0056]
[0057] Table 3
[0058]
[0059] Table 4
[0060]
[0061] Example 1
[0062] A method for preparing a composite reinforced base includes steps A1-A4.
[0063] Step A1, Material Preparation: 1) The upper and lower geotextile layers are subjected to anti-hydrolysis treatment, namely, through impregnation, pre-drying, curing and shaping, cooling and winding. During impregnation, the amount of single epoxy polyester end-capping anti-hydrolysis agent added is 0.8-1.2wt%, and the liquid-holding rate during rolling is 25%-30%, so that the single epoxy polyester end-capping anti-hydrolysis agent is evenly adhered to the fiber surface of the geotextile layer. Pre-dry at 120℃ for 3 minutes. Then, at 185-195℃, wait for 20-30 seconds for curing and shaping, so that the single epoxy polyester end-capping anti-hydrolysis agent reacts with the PET end carboxyl groups to seal the ends. Finally, naturally cool and wind up to obtain the anti-hydrolysis treated upper and lower geotextile layers, and wind them up for later use. 2) The intermediate polymer film layer is corona treated to achieve a moisture surface tension ≥38dyn / cm to improve the adhesion performance with the geotextile layer.
[0064] Step A2, thermal bonding: The upper geotextile layer, the middle polymer film layer, and the lower geotextile layer are stacked in sequence and thermally bonded by heated roller pressing.
[0065] Step A3, Cooling and Shaping: The thermally laminated base is cooled to room temperature by cooling rollers, shaped and wound up to obtain a composite reinforced base with a two-layer fabric and one-layer film structure.
[0066] Step A4, performance testing: The finished composite reinforced base is subjected to peel strength test (peel strength between geotextile and polymer film layer ≥3.0N / cm) and heat shrinkage test (≤2.0% at 190℃). Qualified products are put into storage.
[0067] The parameters of the above-mentioned composite reinforced base are as follows: the upper geotextile layer is polyester geotextile (conventional), with a basis weight of 200 g / m. 2 The polymer membrane is an HDPE membrane with a thickness of 0.3 mm; the underlying geotextile is a polyester geotextile with a basis weight of 200 g / m². 2 The thermal bonding temperature is 160℃, the thermal bonding pressure is 0.5MPa, and the thermal bonding speed is 10m / min.
[0068] Example 2
[0069] The composite reinforced base was prepared using the same method and parameters as in Example 1, except that the basis weight of the upper and lower geotextiles was 150 g / m².2 .
[0070] Example 3
[0071] The composite reinforced base was prepared using the same method and parameters as in Example 1, except that the basis weight of the upper and lower geotextiles was 100 g / m². 2 .
[0072] Example 4
[0073] The composite reinforced base was prepared using the same method and parameters as in Example 1, except that the basis weight of the upper and lower geotextiles was 50 g / m². 2 .
[0074] Example 5
[0075] The composite reinforced base was prepared using the same method and parameters as in Example 2, except that the thickness of the HDPE film was 0.5 mm.
[0076] Example 6
[0077] The composite reinforced base was prepared using the same method and parameters as in Example 2, except that the thickness of the HDPE film was 1.0 mm.
[0078] Comparative Example 1: Single-layer HDPE membrane without geotextile layer
[0079] The difference from Example 2 is that there is no upper geotextile layer and lower geotextile layer. Only a single layer of HDPE film (0.3 mm thick) is used as the base layer to verify the necessity of the geotextile layer.
[0080] Comparative Example 2: Geotextile basis weight too low (30g / m²) 2 )
[0081] The difference from Example 2 is that the geotextile layer has a basis weight of 30 g / m. 2 Everything else is the same.
[0082] Comparative Example 3: Geotextile weight too high (250g / m²) 2 )
[0083] The difference from Example 2 is that the geotextile weight is 250 g / m². 2 Everything else is the same.
[0084] Comparative Example 4: HDPE film thickness is too low (0.2mm)
[0085] The difference from Example 2 is that the HDPE thickness is 0.2 mm, but everything else is the same.
[0086] Comparative Example 5: HDPE film thickness is too high (1.5mm)
[0087] The difference from Example 2 is that the HDPE thickness is 1.5mm, but everything else is the same.
[0088] Comparative Example 6: No heat-stabilized HDPE film was used.
[0089] The difference from Example 2 is that a regular HDPE film (3.5% heat shrinkage rate at 190°C) was used, while everything else was the same, to verify the necessity of a heat-stable HDPE film.
[0090] The performance of the tire bases in Examples 1-6 and Comparative Examples 1-6 were tested using the test methods in Table 3 above. The specific test results are shown in Table 5.
[0091] The modified asphalt formulation is as follows (by mass fraction): 82% 70# asphalt (penetration 60-80, 0.1mm), 4.5% styrene-butadiene-styrene block copolymer (SBS, star-shaped, molecular weight 100,000-150,000), 3% rubber powder (60 mesh, activated waste tire rubber powder), 2.5% tackifying resin (C5 petroleum resin (softening point 100-120℃)), 1% anti-aging agent 1010 (Irganox 1010), 1% compatibilizer (maleic anhydride-grafted styrene-butadiene-styrene block copolymer (MAH-g-SBS, grafting rate 1.0%)), and 6% filler (800 mesh stone powder). Before testing, the modified asphalt is coated onto the surface of the tire base and cured before testing.
[0092] Table 5
[0093]
[0094] As shown in Table 5, the effect of geotextile basis weight on the performance of the composite reinforced substrate was first investigated. The test results show that Example 2 exhibited the highest peel strength of 4.3 N / cm, indicating that the modified asphalt at this basis weight provided the most thorough impregnation of both the upper and lower geotextile layers. If the geotextile basis weight is too low, insufficient anchoring will occur; if the geotextile basis weight is too high, insufficient impregnation of the modified asphalt will result in a decrease in peel strength.
[0095] Furthermore, the change in HDPE film thickness (from 0.3 mm to 1.0 mm) mainly affects mechanical strength and impermeability, but has little impact on the peel strength of the composite reinforced base, and its peel strength meets the requirements.
[0096] Example 7: Geotextile woven from core-sheath composite fibers
[0097] Example 7 uses the same method as in Example 1 to prepare the composite reinforced base, except that the upper and lower geotextile layers are polyester geotextiles woven from core-sheath composite fibers, with a basis weight of 150 g / m². 2 The intermediate polymer film is an HDPE film with a thickness of 0.5 mm; the thermal bonding temperature is 160℃, the thermal bonding pressure is 0.5 MPa, and the thermal bonding speed is 10 m / min.
[0098] A method for weaving polyester geotextile with core-sheath composite fibers includes steps B1-B4.
[0099] Step B1, preparation of the skin material: The copolyester formed by copolymerizing SIPA and PET is blended with a light rare earth element complex and then fed into a twin-screw extruder for extrusion granulation to obtain skin granules. The blending temperature is 270℃, the screw speed is 300rpm, and the residence time is 2min. The amount of light rare earth element complex added is 0.8wt% based on the copolyester.
[0100] Step B2, preparation of core layer granules: PET, 0.5wt% nano montmorillonite, 1.5wt% PET-g-MAH, and 0.15wt% flowability improver are blended and fed into a twin-screw extruder for extrusion granulation to obtain core layer granules. The blending temperature is 270℃, the screw speed is 300rpm, and the residence time is 2min.
[0101] Step B3, core-sheath composite spinning: The sheath granules and core granules are fed into the core-sheath composite fiber assembly at a weight ratio of 8:92 for spinning. After stretching and heat setting, core-sheath composite fibers are obtained. The spinning temperature is 280℃, the draw ratio is 4.0 times, and the heat setting temperature is 190℃.
[0102] Step B4, Geotextile Weaving: The obtained core-sheath composite fibers are woven into polyester geotextile with a basis weight of 150 g / m². 2 .
[0103] Example 8
[0104] Example 8 uses the same method as in Example 7 to prepare a composite reinforced base, except that the intermediate polymer film is an HDPE film with a thickness of 1.0 mm.
[0105] The performance of the composite reinforced tire base prepared by the core-sheath composite fiber in Examples 7-8 above was tested, and the specific test results are shown in Table 6 below.
[0106] Table 6
[0107]
[0108] After replacing the conventional polyester geotextile layer with a polyester geotextile woven from a core-sheath composite fiber, the overall performance of the resulting composite reinforced base is significantly improved in the following aspects.
[0109] (1) Tensile strength of geotextile: increased from 52kN / m to 70kN / m, which is 35% higher than that of conventional geotextile (52kN / m), proving the mechanical reinforcement effect of core-sheath composite fiber.
[0110] (2) Peel strength between geotextile and modified asphalt: increased to 5.2 N / mm, which is 49% higher than that of conventional geotextile (3.5 N / mm), proving that the coordination chemical bonding between light rare earth elements in the skin layer and modified asphalt significantly enhances the interfacial bonding force between the geotextile layer and modified asphalt.
[0111] (3) Interlayer peel strength: increased to 4.5 N / cm, which is 29% higher than that of conventional geotextile (3.5 N / cm), proving that the composite interface between the core-sheath composite fiber and the HDPE membrane is more firmly bonded.
[0112] (4) UV aging performance: The tensile strength retention rate after 300h was 86%, which is 65% higher than that of conventional geotextile (52%), proving that the UV absorption function of light rare earth elements is effective.
[0113] (5) Hot water aging performance: The tensile strength retention rate after 28 days was 78%, which is 42% higher than that of conventional geotextile (55%), proving that the maze effect of the core layer montmorillonite effectively blocks the penetration of water molecules.
[0114] Furthermore, the composite reinforced base prepared using conventional polyester geotextile in Example 5 (HDPE film thickness of 0.5 mm, geotextile layer basis weight of 150 g / m²) was further analyzed. 2 Taking as an example, the long-term durability performance of was tested, and the specific test results are shown in Table 7.
[0115] Table 7
[0116]
[0117] As shown in Table 7, the composite reinforced substrate in Example 5 of this application, after heat aging at 80℃ for 168 hours, exhibits a tensile strength retention rate of up to 92% and a peel strength retention rate of up to 91%, meeting the heat aging requirements of pumped storage power stations. After immersion in hot water at 40℃ for 90 days, the tensile strength retention rate is 90% and the peel strength retention rate is 89%, demonstrating excellent hydrolysis resistance. After immersion in alkali or acid for 30 days, the retention rates of all properties are above 90%, proving the stability of the composite reinforced substrate under various water quality environments. After UV aging for 500 hours, the performance retention rate still reaches above 85%, demonstrating good weather resistance.
[0118] In addition, the durability of the composite reinforced base composed of polyester geotextile layers woven from core-sheath composite fibers was tested, and the specific test results are shown in Table 8.
[0119] Table 8
[0120]
[0121] As shown in Table 8, compared with the composite reinforced base prepared by conventional polyester geotextile, the composite reinforced base composed of geotextile layers woven with sheath-core composite fibers showed an improvement of 2-5 percentage points in the retention rate of various aging parameters, further verifying the synergistic enhancement effect of the coordination bonding of light rare earth elements in the sheath layer and the maze effect of montmorillonite in the core layer on the durability of the composite reinforced base.
[0122] Furthermore, the composite reinforced tire base of this application has the following advantages compared to existing conventional tire bases:
[0123] 1. Compared with traditional polyester single-layer base
[0124] Traditional polyester geotextile bases are single-layer polyester geotextile structures, whose impermeability relies entirely on the surface-coated asphalt layer and lacks structural-level impermeability. This application employs a composite reinforced base consisting of a three-layer composite structure of "geotextile-HDPE membrane-geotextile," with the intermediate HDPE membrane having an impermeability coefficient <10. -11 cm / s, it has excellent seepage prevention performance from the structural level.
[0125] Secondly, traditional polyester single-layer geotextiles rely solely on the physical bond between asphalt and polyester fabric for interlayer bonding. High water pressure exceeding 1.5 MPa can easily cause delamination and bulging due to wedging along the interface. This application addresses this by completely impregnating and anchoring the fiber mesh in both the upper and lower geotextile layers with modified asphalt, forming a multi-layer integrated composite structure with an interlayer peel strength ≥3.0 N / cm, effectively resisting water pressure delamination.
[0126] Furthermore, traditional polyester single-layer base materials are prone to heat shrinkage and deformation at asphalt coating temperatures of 160-190℃. This application uses a heat-stable HDPE film with a heat shrinkage rate of ≤2.0% at 190℃, ensuring dimensional stability of the base material during high-temperature coating. Regarding long-term durability, traditional polyester single-layer base materials age and degrade rapidly. This application, through anti-hydrolysis treatment combined with the inherent weather resistance of HDPE film, improves performance retention by over 40% after aging.
[0127] 2. Comparison with conventional fiberglass base
[0128] Conventional fiberglass-based geotextiles have smooth, chemically inert surfaces, resulting in weak mechanical bonding with modified asphalt and a tendency for interfacial slippage and delamination. The polyester geotextile described in this application features a three-dimensional fiber mesh structure, allowing for thorough impregnation and anchoring of the modified asphalt, significantly enhancing interfacial bonding. In particular, the coordination bonding between the light rare earth elements in the core-sheath composite fibers and the modified asphalt further enhances the interfacial bonding.
[0129] Secondly, fiberglass substrates are relatively brittle and prone to breakage during construction at irregularly shaped sections; the composite reinforced substrate of this application exhibits excellent flexibility, remaining crack-free even when bent 180° around a Φ50mm round bar. Furthermore, fiberglass is prone to alkali precipitation and powdering after prolonged water immersion; the polyester geotextile + HDPE system of this application is water-resistant, corrosion-resistant, and exhibits stable performance. Fiberglass cannot withstand high-frequency water pressure cycling; the integrated composite structure of this application provides stress dispersion and synergistic deformation, resulting in excellent fatigue resistance and suitability for harsh environments such as pumped storage power stations.
[0130] In summary, the fiber-mesh geotextile layer of this application can be fully impregnated with molten modified asphalt, and after curing, it is anchored through a strong mechanical interlocking effect, solving the technical problems of poor interfacial adhesion between polymer membrane and modified asphalt, inability to withstand high temperatures, and lack of long-term durability. Furthermore, this application applies a composite reinforced base with a two-layer fabric-one-membrane structure to modified asphalt waterproof membranes or impermeable boards, meeting the requirements for thermal stability (heat shrinkage rate ≤2.0% at 190℃) and long-term durability (retention rate of various aging processes ≥85%), providing technical standards and implementation basis for impermeable materials for pumped storage power stations.
[0131] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of this application. It should be understood that the above descriptions are merely specific embodiments of this application and are not intended to limit this application. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.
Claims
1. A composite reinforced tire base, characterized in that, The composite reinforced substrate consists of an upper geotextile layer, a polymer membrane layer, and a lower geotextile layer; The upper geotextile layer and the lower geotextile layer have a fiber mesh structure.
2. The composite reinforced tire base according to claim 1, characterized in that, The weight of the upper geotextile layer and the lower geotextile layer are each independently 50-200 g / m². 2 ; The thickness of the polymer film is 0.3-1.0 mm.
3. The composite reinforced tire base according to claim 2, characterized in that, The peel strength between the upper geotextile layer and the lower geotextile layer and the polymer film layer is ≥3.0 N / cm; The polymer film has a Vicat softening temperature ≥120℃ and a thermal shrinkage rate ≤2.0wt% at 190℃.
4. The composite reinforced tire base according to claim 1, characterized in that, The upper geotextile layer and / or the lower geotextile layer are bonded to the polymer film layer by thermal bonding or adhesive bonding.
5. The composite reinforced tire base according to claim 4, characterized in that, The temperature of the thermal bonding is 140-180℃, and the pressure of the thermal bonding is 0.3-0.8MPa.
6. The composite reinforced tire base according to claim 3, characterized in that, The material of the polymer film layer is selected from at least one of high-density polyethylene and polyvinyl chloride.
7. The composite reinforced tire base according to claim 3, characterized in that, The upper geotextile layer and / or the lower geotextile layer are polyester geotextiles woven from core-sheath composite fibers, including a sheath layer and a core layer. The sheath layer is a light rare earth element modified copolyester, which is a copolymer of sodium isophthalate sulfonate and polyester. The core layer includes nano-montmorillonite modified polyester. The weight ratio of the cortex to the core is 5-10:95-90.
8. The composite reinforced tire base according to claim 7, characterized in that, Based on the aforementioned copolyester, the amount of light rare earth element complex added is 0.5-1.0 wt%; Based on the polyester, the amount of nano-montmorillonite added is 0.3-0.8 wt%, and the interlayer spacing of the nano-montmorillonite is ≥3.0 nm.
9. The composite reinforced tire base according to claim 8, characterized in that, The core layer also includes: 0.1-0.2 wt% flowability improver and / or 1.0-2.0 wt% compatibilizer.
10. The application of the composite reinforced base material as described in any one of claims 1-9 in the impermeable board.