A liquid cooling film and its preparation method
By employing a two-layer structural design and roll-to-roll processing technology, the problem of low production efficiency of liquid cooling films has been solved, enabling the efficient preparation of flexible and bendable colored liquid cooling films, expanding application scenarios and reducing costs.
Patent Information
- Application Number
- CN202611240254.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-17
- Publication Date
- 2026-11-17
AI Technical Summary
Existing liquid cooling films have low production efficiency and can only be processed one piece at a time, which limits their application scenarios and cost control.
The liquid-cooled film is manufactured using a two-layer structure design, including a substrate layer and a microchannel resin layer. It is prepared by roll-to-roll processing and is compounded with NLK-UV006 main adhesive, BYK-333 leveling agent, HDDA diluent and color paste to achieve flexibility and color customization.
It has improved production efficiency, reduced costs, broadened application scenarios, enabled the production of flexible and bendable colored liquid cooling films, and enhanced sealing performance and stability.
Smart Images

Figure CN123104201A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of liquid cooling film technology, and in particular to a liquid cooling film and its preparation method. Background Technology
[0002] The full name of liquid cooling film is flexible microchannel liquid cooling film. It is a lightweight active liquid cooling heat dissipation device. It is formed by hot pressing and laminating of polymer composite film materials to form a closed microchannel, which is filled with coolant. It relies on micro pumps to drive the liquid circulation to remove heat. It is a flexible alternative to traditional VC metal cold plates and graphite heat-conducting sheets.
[0003] The mainstream structure in the liquid cooling film industry is a sandwich three-layer structure, with a microchannel core layer in the middle and surface sealing barrier layers on the top and bottom. The microchannel core layer in the middle is formed using a carving process. The middle layer is stacked with the top and bottom layers, and the surrounding area is sealed by high-temperature hot pressing to complete the liquid cooling film processing. This processing method means that liquid cooling films can only be processed piece by piece, which affects production efficiency. Summary of the Invention
[0004] The purpose of this invention is to overcome the shortcomings of the prior art and provide a liquid cooling film and its preparation method.
[0005] To achieve the above objectives, the present invention adopts the following technical solution: A liquid cooling film includes a microchannel structure layer and a surface sealing barrier layer. The microchannel structure layer includes a substrate layer and microchannel resin layers spaced apart, with the microchannel resin layers located between the substrate layer and the surface sealing barrier layer.
[0006] Furthermore, the thickness of the substrate layer is 25~200μm, the thickness of the microchannel resin layer is 50~200μm, and the thickness of the surface sealing barrier layer is 50~150μm.
[0007] Furthermore, the mass composition of the microchannel resin layer is as follows: 80-120 parts of NLK-UV006 main adhesive, 0.4-1.8 parts of BYK-333 leveling agent, 2-10 parts of HDDA diluent, and 0-2 parts of color paste.
[0008] Furthermore, the preparation method of the microchannel resin includes the following steps: Add NLK-UV006 main adhesive to the reaction apparatus, start stirring, and stir at 300 rpm for 5-10 minutes. Weigh BYK-333 leveling agent, HDDA, diluent and color paste, stir thoroughly for 10-20 minutes, and degas under vacuum for 30-50 minutes to obtain the microchannel resin. Take samples for testing, and test the solid content >90% and the viscosity 20-500 mPaS.
[0009] Furthermore, the substrate layer is selected from one of PET film, TAC film, PI film, and PC film.
[0010] A method for preparing a liquid cooling film, the method comprising the following steps: S1 metal mold preheated to 50-90℃; The shape of the metal mold can be designed and processed according to the shape of the liquid cooling film required by the customer to form the corresponding microchannel resin layer. The metal mold can be flat or roller-shaped.
[0011] S2 places the substrate on the first unwinding device for film feeding, with the coated side facing upwards, and applies UV resin to the coated side of the substrate; The substrate can be a film material such as PET film, TAC film, PI film, PC film, etc., and can be with or without the property of blocking water vapor, gas, etc. The substrate coated with UV resin is passed through a mold roller and then through a first UV lamp to pre-cur and shape the UV resin. After the UV resin is demolded from the mold roller and cured by a second UV lamp, it is then removed by an oven to obtain a microfluidic structure layer film. S4 places the sealing barrier layer on the second unwinding device with the adhesive side facing down, and it is bonded together with the microchannel structure layer film material. After being bonded and sealed by a heating roller, it is finally die-cut to obtain the finished product. Beneficial effects
[0012] 1. Compared to the traditional three-layer structure, the liquid cooling film in this invention is designed as a two-layer structure. A two-layer structure requires only one sealing barrier layer, simplifying the manufacturing process, resulting in better sealing, higher stability, and lower cost. Furthermore, existing liquid cooling films have a microchannel-formed core layer as the middle layer, with the microchannels formed by laser. Therefore, existing liquid cooling films can only be black. In contrast, the microchannel material of this invention is a resin layer, which can be colored according to customer needs by adding colorant. The resin layer can also be made flexible, resulting in higher overall bendability. Existing liquid cooling films are rigid sheets, bonded with adhesive during production, and cannot be bent, which to some extent limits the application scenarios of the liquid cooling film.
[0013] 2. The preparation method of the liquid cooling film in this invention enables roll-to-roll processing, greatly improving production efficiency and reducing production costs. The microchannel resin in this invention is formulated with NLK-UV006 as the main adhesive, BYK-333 as the leveling agent, toluene as a diluent, and colorant, exhibiting good adhesion, high flexibility, and resistance to yellowing. Furthermore, this liquid cooling film preparation method can produce colored liquid cooling films, allowing for customized color production according to customer requirements. The liquid cooling film preparation method in this invention can also produce flexible and bendable liquid cooling films, further expanding the application scenarios of liquid cooling films. Attached Figure Description
[0014] Figure 1 This is a flowchart illustrating the preparation process of the liquid cooling film in this invention. Detailed Implementation
[0015] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to specific examples. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0016] This invention provides a liquid cooling film comprising a microchannel structure layer and a surface sealing barrier layer. The microchannel structure layer includes a substrate layer and spaced-apart microchannel resin layers, with the resin layers positioned between the substrate layer and the surface sealing barrier layer. Compared to the traditional three-layer structure, the two-layer structure requires only one sealing barrier layer, resulting in a simpler manufacturing process, better sealing performance, higher stability, and lower cost.
[0017] Furthermore, the existing liquid cooling film has a microchannel-formed core layer as its middle layer, and the microchannels on the core layer are formed by laser. Therefore, the existing liquid cooling film can only be black. However, the microchannel material of the present invention is a resin layer, which can be colored according to customer needs by adding color paste. Moreover, the resin layer can be made flexible, so the overall flexibility is high. In contrast, the existing film is a rigid sheet that is glued during production and cannot be bent, which to some extent limits the application scenarios of the liquid cooling film.
[0018] In a preferred embodiment, the thickness of the substrate layer in this embodiment is 25~200μm, specifically: 25μm, 50μm, 75μm, 100μm, 125μm, 150μm, 175μm, 200μm, preferably 100μm; the thickness of the microchannel resin layer is 50~200μm, specifically: 50μm, 75μm, 100μm, 120μm, 150μm, 170μm, 200μm, preferably 100μm; the thickness of the surface sealing barrier layer is 50~150μm, specifically: 50μm, 75μm, 100μm, 125μm, 150μm, preferably 100μm.
[0019] In a preferred embodiment, the microchannel resin layer in this embodiment is composed of the following parts by weight: 80-120 parts of NLK-UV006 main adhesive, 0.4-1.8 parts of BYK-333 leveling agent, 2-10 parts of HDDA diluent, and 0-2 parts of color paste.
[0020] In a preferred embodiment, the substrate layer in this example is selected from one of PET film, TAC film, PI film, and PC film, preferably PET film. Example
[0021]
[0022] The preparation method of the microchannel resin in Examples 1 to 6 includes the following steps: Add NLK-UV006 main adhesive to the reaction apparatus, start stirring, stir at 300 rpm for 10 min, weigh BYK-333 leveling agent, HDDA, diluent and color paste, stir thoroughly for 20 min, vacuum degas for 40 min, to obtain the microchannel resin, take a sample to test the solid content of 95% and the viscosity of 100 mPaS.
[0023] like Figure 1 As shown, the method for preparing the liquid cooling film in this invention includes the following steps: S1 metal mold preheated to 80℃; The shape of the metal mold can be designed and processed according to the shape of the liquid cooling film required by the customer to form the corresponding microchannel resin layer. The metal mold can be flat or roller-shaped.
[0024] S2 places the substrate on the first unwinding device for film feeding, with the coated side facing upwards, and applies UV resin to the coated side of the substrate; The substrate coated with UV resin is passed through a mold roller and then through a first UV lamp to pre-cur and shape the UV resin. After the UV resin is demolded from the mold roller and cured by a second UV lamp, it is then removed by an oven to obtain a microfluidic structure layer film. S4 places the sealing barrier layer on the second unwinding device with the adhesive side facing down, and it is bonded together with the microchannel structure layer film material. After being bonded and sealed by a heating roller, it is finally die-cut to obtain the finished product.
[0025] The performance of the liquid cooling films prepared in each embodiment was tested, and the experimental test results were obtained.
[0026] Experimental results show that the liquid cooling film prepared by this invention meets the application requirements. The roll-to-roll process has the advantages of high production efficiency and low cost. It can also produce liquid cooling films with colored appearance to adapt to personalized customization. The thin liquid cooling film has bendable characteristics, which expands the application environment of the product.
[0027] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent claim. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.
Claims
1. A liquid cooling film, characterized in that: It includes a microchannel structure layer and a surface sealing barrier layer. The microchannel structure layer includes a substrate layer and microchannel resin layers spaced apart. The microchannel resin layers are located between the substrate layer and the surface sealing barrier layer.
2. The liquid cooling film according to claim 1, characterized in that: The thickness of the substrate layer is 25~200μm, the thickness of the microchannel resin layer is 50~200μm, and the thickness of the surface sealing barrier layer is 50~150μm.
3. The liquid cooling film according to claim 1, characterized in that: The microchannel resin layer is composed of the following components by weight: 80-120 parts of NLK-UV006 main adhesive, 0.4-1.8 parts of BYK-333 leveling agent, 2-10 parts of HDDA diluent, and 0-2 parts of color paste.
4. The liquid cooling film according to claim 3, characterized in that: The preparation method of the microfluidic resin includes the following steps: Add NLK-UV006 main adhesive to the reaction apparatus, start stirring, and stir at 300 rpm for 5-10 minutes. Weigh BYK-333 leveling agent, HDDA, diluent and color paste, stir thoroughly for 10-20 minutes, and degas under vacuum for 30-50 minutes to obtain the microchannel resin. Take samples for testing, and test the solid content >90% and the viscosity 20-500 mPaS.
5. The liquid cooling film according to claim 1, characterized in that: The substrate layer is selected from one of PET film, TAC film, PI film, and PC film.
6. A method for preparing a liquid cooling film according to any one of claims 1 to 5, characterized in that: The preparation method includes the following steps: S1 metal mold preheated to 50-90℃; S2 places the substrate on the first unwinding device for film feeding, with the coated side facing upwards, and applies UV resin to the coated side of the substrate; The substrate coated with UV resin is passed through a mold roller and then through a first UV lamp to pre-cur and shape the UV resin. After the UV resin is demolded from the mold roller and cured by a second UV lamp, it is then removed by an oven to obtain a microfluidic structure layer film. S4 places the sealing barrier layer on the second unwinding device with the adhesive side facing down, and it is bonded together with the microchannel structure layer film material. After being bonded and sealed by a heating roller, it is finally die-cut to obtain the finished product.