A novel clothing material and its preparation method
By employing a three-layer gradient composite structure consisting of a skin-friendly moisture-wicking layer, an intelligent temperature-regulating intermediate layer, and a biomimetic self-healing outer layer, the shortcomings of single-function textile materials in existing technologies are overcome, achieving multi-functional synergistic effects and enhancing the thermal and moisture comfort and protective durability of clothing.
Patent Information
- Application Number
- CN202611621563.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-20
- Publication Date
- 2026-11-17
AI Technical Summary
In existing technologies, single-function textile materials are difficult to meet complex and ever-changing usage requirements. In particular, in terms of heat and humidity management and surface protection, there are problems such as easy leakage of phase change materials, low thermal conductivity, and contradiction between self-healing efficiency and mechanical strength. There is a lack of structural designs that organically combine the three functions.
Employing a three-layer gradient composite structure consisting of a skin-friendly moisture-wicking layer, an intelligent temperature-regulating intermediate layer, and a biomimetic self-healing outer layer, this material combines polycaprolactone, carboxylated chitosan, self-healing polyurethane, and polyvinylidene fluoride-hexafluoropropylene copolymer to form a multi-layer gradient composite clothing material, achieving synergistic effects of thermal buffering, one-way moisture wicking, and surface self-healing.
It achieves rapid sweat absorption and unidirectional transport, efficient response of the intelligent temperature regulating layer, durability and hydrophobic protection of the biomimetic self-healing layer, and the overall fabric has excellent thermal and moisture comfort, protective durability and intelligent response characteristics.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of clothing fabric technology, and in particular to a novel clothing material and its preparation method. Background Technology
[0002] With the increasing demands for comfort and functionality in outdoor sports, specialized operations, and everyday wear, single-function textile materials are no longer sufficient to meet the complex and ever-changing needs. Currently, functional fabrics used in smart clothing mainly focus on two aspects: thermal and moisture management and surface protection. In terms of thermal and moisture management, existing technologies mostly use phase change materials (PCM) microcapsule coatings or fillings to give fabrics temperature-regulating functions. However, these materials generally suffer from problems such as easy leakage of the phase change core material during processing or use, low thermal conductivity leading to lag in response, and the coating structure significantly affects the fabric's moisture permeability and breathability, failing to effectively solve the problem of the damp and cold feeling caused by sweat accumulating on the skin surface.
[0003] In terms of surface protection, giving the outer layer of fabric self-healing ability is an important way to extend the service life of clothing. However, existing self-healing polymer materials often rely on the recombination of dynamic covalent or non-covalent bonds. There is a trade-off between their repair efficiency and mechanical strength. How to achieve efficient room temperature self-healing while ensuring the hydrophobic protective performance of the outer layer is a current technical challenge.
[0004] Furthermore, existing technologies lack a structural design that can organically combine the three functions of heat buffering, one-way moisture wicking, and surface self-healing into the same fabric. The interfacial compatibility and processing technology matching between the functional layers also constitute bottlenecks restricting the development of integrated fabrics. Summary of the Invention
[0005] To address the aforementioned technical problems, this invention provides a novel clothing material and its preparation method. This novel material achieves multifunctional synergistic effects through a three-layer gradient composite structure consisting of a skin-friendly moisture-wicking layer, an intelligent temperature-regulating intermediate layer, and a biomimetic self-healing outer layer.
[0006] In order to achieve the objective of this invention, the following technical solution is adopted: This invention provides a novel clothing material, comprising, in sequence: a skin-friendly and moisture-wicking layer, an intelligent temperature-regulating intermediate layer, and a biomimetic self-healing outer layer; The skin-friendly moisture-wicking layer includes polycaprolactone and carboxylated chitosan; The intelligent temperature-regulating intermediate layer is a phase change microcapsule; The biomimetic self-healing outer layer comprises a blend of self-healing polyurethane and polyvinylidene fluoride-hexafluoropropylene copolymer.
[0007] Furthermore, the intelligent temperature-regulating intermediate layer is a temperature-regulating layer formed by uniformly spreading phase change microcapsules.
[0008] Furthermore, the polycaprolactone has a number-average molecular weight of 80,000, the carboxylated chitosan has a number-average molecular weight of 15,000, and the degree of carboxylation is ≥90%. The self-healing polyurethane is prepared from polytetrahydrofuran diol, isophorone diisocyanate, 2,2'-diaminodiphenyl disulfide, and 3,3',5,5'-tetrabromobisphenol A as raw materials; the number average molecular weight of the polytetrahydrofuran diol is 2000, and the weight average molecular weight of the polyvinylidene fluoride-hexafluoropropylene copolymer is 400,000; and the molar ratio of vinylidene fluoride monomer to hexafluoropropylene monomer in the polyvinylidene fluoride-hexafluoropropylene copolymer is 88:12.
[0009] Furthermore, the phase change microcapsule is composed of a shell layer and a core layer; The core layer comprises lauric acid and myristic acid, the shell layer is a silica shell layer, the shell layer is wrapped around the surface of the core layer, and the outer surface of the silica shell layer is coated with hydroxylated multi-walled carbon nanotubes.
[0010] Furthermore, the mass ratio of polycaprolactone to carboxylated chitosan is (70:30) to (95:5). The water contact angle of the skin-friendly moisture-wicking layer is less than 30°, and the water contact angle of the biomimetic self-healing outer layer is greater than 140°.
[0011] Furthermore, the mass ratio of polycaprolactone to carboxylated chitosan is 85:15.
[0012] Furthermore, the hydroxylated multi-walled carbon nanotubes have a diameter of 10 nm-20 nm, a length of 10 μm-30 μm, and a hydroxyl content of 1 wt% to 3 wt% of the mass of the multi-walled carbon nanotubes. The amount of the silica shell is 15% to 40% of the core layer mass; The amount of multi-walled carbon nanotubes used is 0.5% to 5.0% of the core layer mass.
[0013] Furthermore, the amount of the silica shell is 25% of the core layer mass; The amount of multi-walled carbon nanotubes used is 2.0% of the core layer mass.
[0014] Furthermore, the mass ratio of lauric acid to myristic acid is (60:40) to (85:15). The molar ratio of isophorone diisocyanate to polytetrahydrofuran diol is (1.6~2.4):1; The molar ratio of 2,2'-diaminodiphenyl disulfide to 3,3',5,5'-tetrabromobisphenol A is 1:(6~2).
[0015] Furthermore, the mass ratio of lauric acid to myristic acid is 70:30; The molar ratio of isophorone diisocyanate to polytetrahydrofuran diol is 2.0:1; The molar ratio of 2,2'-diaminodiphenyl disulfide to 3,3',5,5'-tetrabromobisphenol A is 1:4.
[0016] Furthermore, the areal density of the intelligent temperature-regulating intermediate layer is 80 g / m³. 2 ~200g / m 2 .
[0017] This invention also provides a method for preparing a novel clothing material, comprising the following steps: S1. Prepare the intelligent temperature-regulating intermediate layer; S2. Prepare a skin-friendly and moisture-wicking layer; S3. Prepare a biomimetic self-healing outer layer; S4, hot-pressed composite.
[0018] Furthermore, step S1 specifically includes the following steps: S101, Prepare the core material melt; S102. Emulsify the core material melt with deionized water to form an oil-in-water emulsion; S103. The water-in-oil emulsion is used to prepare phase change microcapsules.
[0019] Furthermore, S101 specifically includes: mixing lauric acid and myristic acid, heating to 70°C and stirring until completely melted to obtain a phase change core material melt.
[0020] Furthermore, S103 specifically includes: adding tetraethyl orthosilicate and ammonia to an oil-in-water emulsion, reacting at 50°C for 4 hours, so that tetraethyl orthosilicate hydrolyzes and condenses on the surface of the phase change core material melt to form a silica shell, thereby obtaining a microcapsule primary product coated with the phase change core material. Hydroxylated multi-walled carbon nanotubes were added to the reaction system and stirred for 1 hour to allow the hydroxylated multi-walled carbon nanotubes to be composited on the outer surface of the silica shell. After centrifugation, washing and vacuum drying, phase change microcapsules were obtained.
[0021] Furthermore, S2 specifically includes: dissolving polycaprolactone and carboxylated chitosan in a mixed solvent of N,N-dimethylformamide and tetrahydrofuran to prepare a first spinning solution; and using electrospinning technology to form a first nanofiber membrane as a skin-friendly and moisture-wicking layer.
[0022] Furthermore, S3 specifically includes: reacting polytetrahydrofuran diol with isophorone diisocyanate at 80°C for 2 hours to obtain an isocyanate-terminated prepolymer; 2,2'-diaminodiphenyl disulfide and 3,3',5,5'-tetrabromobisphenol A were added to the prepolymer, and the reaction was continued at 60°C for 3 hours. A self-healing polyurethane was obtained by chain extension reaction. The self-healing polyurethane and polyvinylidene fluoride-hexafluoropropylene copolymer were dissolved in a mixed solvent of N,N-dimethylformamide and tetrahydrofuran to prepare a second spinning solution. The second spinning solution is used to form a second nanofiber membrane using electrospinning technology, which serves as a biomimetic self-healing outer layer.
[0023] Furthermore, S4 specifically includes: sequentially stacking the skin-friendly moisture-wicking layer, the phase change microcapsules prepared in S1, and the biomimetic self-healing outer layer, performing hot-pressing composite under conditions of hot-pressing temperature of 70℃~90℃ and hot-pressing pressure of 1MPa to 3MPa, and obtaining the multi-layer composite clothing fabric after cooling.
[0024] This invention also provides the application of the above-mentioned novel clothing material in the preparation of outdoor sportswear or medical protective clothing.
[0025] The present invention has the following technical effects: This application achieves multifunctional synergistic effects through a three-layer gradient composite structure consisting of a skin-friendly moisture-wicking layer, an intelligent temperature-regulating intermediate layer, and a biomimetic self-healing outer layer. The skin-friendly moisture-wicking layer rapidly absorbs and conducts sweat from the skin to the outer surface of the fabric, preventing the damp and cold discomfort caused by sweat retention. Simultaneously, the wettability gradient distribution from a superhydrophilic inner layer to a superhydrophobic outer layer provides the driving force for unidirectional sweat transport, effectively improving the wearer's feeling of dryness. In the intelligent temperature-regulating intermediate layer, the phase change core material is completely encapsulated by a silica shell, eliminating leakage problems during hot pressing and long-term use. Combined with the enhanced thermal conductivity and photothermal conversion effect of hydroxylated multi-walled carbon nanotubes composited on the shell surface, the response rate and energy storage efficiency of the phase change material are significantly improved, achieving active buffering and regulation of the body's microenvironment temperature. The surface microcracks of the biomimetic self-healing outer layer have self-repairing capabilities without sacrificing the material's mechanical strength, allowing the fabric to maintain the integrity of the outer structure and hydrophobic protective properties even after long-term use or repeated friction. The layers are bonded together by hot pressing to form a stable interface, and the overall fabric has excellent thermal and moisture comfort, protective durability and intelligent response characteristics. Detailed Implementation
[0026] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of them. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.
[0027] Example 1 The raw materials used in this embodiment are all commercially available products, and their specific specifications are as follows: Skin-friendly wicking layer raw materials: Polycaprolactone (PCL), number average molecular weight (M) 80,000, purity ≥99%; Carboxylated chitosan, with a number average molecular weight (M) of 15,000 and a degree of carboxylation ≥90%, was purchased from Zhejiang Jinke Pharmaceutical Co., Ltd. N,N-Dimethylformamide (DMF), purity ≥99.5%, anhydrous grade; Tetrahydrofuran (THF), purity ≥99.5%, anhydrous grade.
[0028] Intelligent temperature-regulating intermediate layer raw materials: Lauric acid (LA), purity ≥98%, melting point 44℃~46℃; Myristic acid (MA), purity ≥98%, melting point 52℃~54℃; Tetraethyl orthosilicate (TEOS), purity ≥99%, SiO2 content ≥28%; Ammonia solution, concentration 25%~28%, analytical grade; hydroxylated multi-walled carbon nanotubes (MWCNTs-OH), purity ≥95%, diameter 10nm to 20nm, length 10μm~30μm, hydroxyl content 1wt%~3wt% of the mass of the multi-walled carbon nanotubes; Tween-80, analytical grade.
[0029] Biomimetic self-healing outer layer materials: polytetrahydrofuran glycol (PTMG), number average molecular weight (M) of 2000; isophorone diisocyanate (IPDI), purity ≥99%; 2,2'-diaminodiphenyl disulfide (DTDA), purity ≥98%; 3,3',5,5'-tetrabromobisphenol A (TBBA), purity ≥98%; polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), weight average molecular weight (M_w) of 400,000, molar ratio of vinylidene fluoride monomer to hexafluoropropylene monomer of 88:12; DMF, purity ≥99.5%, anhydrous grade; THF, purity ≥99.5%, anhydrous grade.
[0030] S1. Preparation of intelligent temperature-regulating intermediate layer (1) Mix lauric acid and myristic acid at a mass ratio of 70:30, place them in a 70°C water bath and stir until completely melted to obtain a phase change core material melt.
[0031] (2) Mix the phase change core material melt with deionized water, add Tween-80 as an emulsifier, and emulsify for 10 minutes at a speed of 10,000 rpm to form an oil-in-water emulsion.
[0032] (3) Add tetraethyl orthosilicate and ammonia to the oil-in-water emulsion. The amount of tetraethyl orthosilicate added is 25% of the mass of the phase change core material melt, and the amount of ammonia added is 10% of the mass of tetraethyl orthosilicate. React at 50°C for 4 hours to allow tetraethyl orthosilicate to hydrolyze and condense on the surface of the phase change core material melt to form a silica shell, thereby obtaining the microcapsule primary product coated with the phase change core material.
[0033] (4) Add hydroxylated multi-walled carbon nanotubes to the reaction system. The amount added is 2.0% of the molten mass of the phase change core material. Stir for 1 hour to make the hydroxylated multi-walled carbon nanotubes composite on the outer surface of the silica shell.
[0034] (5) The reaction product was separated by centrifugation, washed three times with deionized water, and dried under vacuum at 60°C for 12 hours to obtain phase change microcapsules.
[0035] S2, Preparation of the skin-friendly moisture-wicking layer Polycaprolactone and carboxylated chitosan were co-dissolved in a mixed solvent of DMF and THF at a mass ratio of 85:15 (DMF to THF volume ratio of 1:1) to prepare a first spinning solution with a total solute mass concentration of 12%. The first spinning solution was then used to fabricate a skin-friendly, moisture-wicking layer using electrospinning technology. The electrospinning process parameters were: spinning voltage 18 kV, receiving distance 15 cm, and spinning solution flow rate 0.8 mL / h. The resulting skin-friendly, moisture-wicking layer had a water contact angle of less than 30°.
[0036] S3. Preparation of biomimetic self-healing outer layer (1) Synthesis of self-healing polyurethane (SR-PU): Polytetrahydrofuran diol and isophorone diisocyanate were fed at a molar ratio of 2.0:1 and reacted at 80°C for 2 hours to obtain an isocyanate-terminated prepolymer.
[0037] (2) Add 2,2'-diaminodiphenyl disulfide and 3,3',5,5'-tetrabromobisphenol A to the prepolymer at a molar ratio of 1:4, and continue the reaction at 60°C for 3 hours to obtain self-healing polyurethane through chain extension reaction.
[0038] (3) The self-healing polyurethane and polyvinylidene fluoride-hexafluoropropylene copolymer are co-dissolved in a mixed solvent of DMF and THF at a mass ratio of 60:40 (the volume ratio of DMF to THF is 1:1) to prepare a second spinning solution with a total solute mass concentration of 15%.
[0039] (4) The second spinning solution was used to form a second nanofiber membrane as a biomimetic self-healing outer layer by electrospinning. The electrospinning process parameters were: spinning voltage 20 kV, receiving distance 18 cm, and spinning solution flow rate 1.0 mL / h. The water contact angle of the resulting biomimetic self-healing outer layer was greater than 140°.
[0040] S4, hot-pressed composite The skin-friendly and moisture-wicking layer prepared in S2 and the phase change microcapsules prepared in S1 (evenly spread by electrostatic flocking, with an areal density of 120 g / m²) were then prepared. 2 The biomimetic self-healing outer layer obtained by S3 is stacked in sequence and hot-pressed for 5 minutes at a hot-pressing temperature of 80℃ and a hot-pressing pressure of 2.0MPa. After cooling, the multi-layer composite clothing fabric is obtained.
[0041] Example 2 The only difference between this embodiment and Embodiment 1 is the ratio of some raw materials, as detailed below: In S1, the mass ratio of lauric acid to myristic acid is 60:40; the amount of tetraethyl orthosilicate added is 15% of the molten mass of the phase change core material; and the amount of hydroxylated multi-walled carbon nanotubes added is 0.5% of the molten mass of the phase change core material.
[0042] In S2, the mass ratio of polycaprolactone to carboxylated chitosan is 95:5.
[0043] In S3, the molar ratio of isophorone diisocyanate to polytetrahydrofuran diol is 2.4:1; the molar ratio of 2,2'-diaminodiphenyl disulfide to 3,3',5,5'-tetrabromobisphenol A is 1:2; and the mass ratio of self-healing polyurethane to polyvinylidene fluoride-hexafluoropropylene copolymer is 40:60.
[0044] In S4, the areal density of the phase change microcapsules is 80 g / m³. 2 The hot pressing temperature is 70℃ and the hot pressing pressure is 1.0MPa.
[0045] The remaining steps and process parameters are the same as in Example 1.
[0046] Example 3 The only difference between this embodiment and Embodiment 1 is the ratio of some raw materials, as detailed below: In S1, the mass ratio of lauric acid to myristic acid is 85:15; the amount of tetraethyl orthosilicate added is 40% of the molten mass of the phase change core material; and the amount of hydroxylated multi-walled carbon nanotubes added is 5.0% of the molten mass of the phase change core material.
[0047] In S2, the mass ratio of polycaprolactone to carboxylated chitosan is 70:30.
[0048] In S3, the molar ratio of isophorone diisocyanate to polytetrahydrofuran diol is 1.6:1; the molar ratio of 2,2'-diaminodiphenyl disulfide to 3,3',5,5'-tetrabromobisphenol A is 1:6; and the mass ratio of self-healing polyurethane to polyvinylidene fluoride-hexafluoropropylene copolymer is 80:20.
[0049] In S4, the areal density of the phase change microcapsules is 200 g / m³. 2 The hot pressing temperature is 90℃ and the hot pressing pressure is 3.0MPa.
[0050] The remaining steps and process parameters are the same as in Example 1.
[0051] Comparative Example 1 This comparative example provides a temperature-regulating fabric prepared using a conventional phase change microcapsule coating method, the preparation method of which is as follows: (1) Preparation of phase change microcapsules: Paraffin wax (melting point 52℃~54℃) was mixed with deionized water, and an emulsifier was added. The mixture was emulsified at high speed to form an oil-in-water emulsion. Melamine resin prepolymer was slowly added dropwise to the emulsion, and the mixture was reacted at 60℃ for 2 hours to allow the melamine resin to polymerize on the surface of the paraffin wax to form a shell. After washing and drying, paraffin wax@melamine resin phase change microcapsules were obtained. No thermally conductive fillers were added to these microcapsules.
[0052] (2) Preparation of coating finishing solution: The phase change microcapsules obtained in step (1) are mixed with polyacrylate adhesive at a mass ratio of 60:40, an appropriate amount of thickener is added, and the mixture is stirred and dispersed evenly to prepare a coating finishing solution.
[0053] (3) Coating finishing: using commercially available pure cotton woven fabric (area density 150g / m²) 2 Using a base fabric, a coating finishing liquid is evenly applied to the surface of the base fabric using a scraping method, with a coating amount of 150 g / m². 2 The fabric is dried and set at 120℃ to obtain a temperature-regulating fabric.
[0054] This comparative example represents a typical phase change microcapsule coated temperature-regulating fabric in the prior art, with a phase change core material of paraffin and a shell material of melamine resin, which are bonded to the fabric through a coating process.
[0055] Comparative Example 2 This comparative example provides a coated fabric prepared using conventional self-healing polyurethane, the preparation method of which is as follows: (1) Synthesis of self-healing polyurethane: Polytetrahydrofuran diol (M=2000) and isophorone diisocyanate were fed at a molar ratio of 1.5:1 and reacted at 80°C for 2 hours to obtain a prepolymer. 2,2'-Diaminodiphenyl disulfide (DTDA) was added to the prepolymer as a chain extender (5% of the prepolymer mass), and the reaction was continued at 60°C for 3 hours to obtain self-healing polyurethane. 3,3',5,5'-Tetrabromobisphenol A (TBBA) was not added as a co-chain extender to this polyurethane.
[0056] (2) Preparation of coating finishing solution: Dissolve the self-healing polyurethane obtained in step (1) in DMF to prepare a solution with a mass concentration of 20% as the coating finishing solution.
[0057] (3) Coating and finishing: using commercially available polyester woven fabric (area density 120g / m²) 2 Using a base fabric as the base fabric, a coating finishing liquid is applied to the surface of the base fabric by dip coating method, and then dried and shaped at 100℃ to obtain a self-healing coated fabric.
[0058] This comparative example represents conventional self-healing polyurethane coated fabrics in the prior art, which only use DTDA to provide dynamic crosslinking of disulfide bonds and do not introduce the hydrogen bond synergistic crosslinking network of TBBA.
[0059] Experimental Example 1: Thermal Conductivity Test of Phase Change Microcapsules A total of 3 groups of samples were tested: Sample A: MWCNTs-OH@SiO2@LA-MA composite phase change microcapsules prepared in Example 1S1 (MWCNTs-OH addition amount 2.0%). Sample B: SiO2@LA-MA phase change microcapsules without the addition of MWCNTs-OH, with the remaining preparation conditions the same as in Example 1S1; Sample C: Paraffin@melamine resin phase change microcapsules prepared in step (1) of Comparative Example 1.
[0060] Test method: The thermal conductivity of each microcapsule sample was determined using a transient hot-wire thermal conductivity meter. Before the test, the microcapsule powder was vacuum dried at 60℃ for 12 hours. An appropriate amount of powder was placed in a special sample cell, compacted to the same density, and tested under constant temperature conditions of 25℃. Each group of samples was measured 5 times, and the average value was taken. The experimental results are shown in Table 1.
[0061] Table 1: Test Results The phase change microcapsules in Example 1 are composited with hydroxylated multi-walled carbon nanotubes on the surface of a silica shell, achieving a thermal conductivity of 0.92 W·m. -1 ·K -1Compared to sample B (0.28 W·m⁻¹) without the addition of MWCNTs-OH, -1 ·K -1 The efficiency was increased by approximately 228% compared to traditional paraffin@melamine resin microcapsules (0.21 W·m³). -1 ·K -1 The thermal conductivity of the phase change microcapsules was increased by approximately 338%. This indicates that the composite of MWCNTs-OH effectively enhances the thermal conductivity of the phase change microcapsules and can significantly improve the response rate of the phase change material.
[0062] Experiment Example 2: Testing of the Mechanical Properties and Repair Efficiency of the Self-Healing Outer Layer Three groups of samples were tested, all of which were prepared as nanofiber membranes using electrospinning: Sample D: Bionic self-healing outer nanofiber membrane prepared in Example 1S3 (SR-PU / PVDF-HFP=60:40, DTDA:TBBA=1:4). Sample E: The self-healing polyurethane used only DTDA as a chain extender and did not contain TBBA. The ratio of SR-PU to PVDF-HFP was 60:40. The other preparation conditions were the same as in Example 1S3. Sample F: Self-healing polyurethane coated fabric prepared in Comparative Example 2 (dip coating method).
[0063] Test method: (1) Tensile strength test: Refer to GB / T 1040.3—2006 "Determination of tensile properties of plastics Part 3: Test conditions for films and sheets", cut each sample into dumbbell-shaped specimens (effective size 25mm×6mm), and perform tensile test on a universal testing machine. The tensile rate is 50mm / min. Five specimens are tested for each group of samples, and the average value is taken. Record the original tensile strength (σ0).
[0064] (2) Self-healing efficiency test: A scratch with a depth of about 50% of the film thickness was made on the surface of each sample with a sharp blade. The sample was placed in a room temperature (25±2℃) environment for 24 hours. After repair, a tensile test was performed again, and the tensile strength (σ1) after repair was recorded. The self-healing efficiency (η) was calculated according to the following formula: η = (σ1 / σ0) × 100%. The test results are shown in Table 2.
[0065] Table 2: Experimental Results The biomimetic self-healing outer layer of Example 1 (sample D) achieved an initial tensile strength of 15.87 MPa, significantly higher than that of sample E (8.34 MPa) without TBBA and sample F (6.52 MPa) of Comparative Example 2 with an impregnated coating. Simultaneously, sample D achieved a self-healing efficiency of 89.8%, higher than that of samples E (86.6%) and F (77.5%). This indicates that the introduction of TBBA provides additional hydrogen bonding, forming a synergistic dynamic network with disulfide bonds, significantly improving the mechanical strength of the material without sacrificing repair efficiency, effectively resolving the contradiction between the mechanical properties and repair efficiency of self-healing materials.
[0066] Experiment Example 3: Overall One-Way Moisture-Guiding Performance Test of Fabric A total of 3 groups of samples were tested: Sample G: The three-layer composite garment fabric prepared in Example 1; Sample H: Single-layer PCL / carboxylated chitosan nanofiber membrane, with the same thickness as the skin-friendly moisture-wicking layer in Example 1, without composite intermediate and outer layers; Sample I: Phase change microcapsule coated temperature-regulating fabric (pure cotton base + coating) prepared in Comparative Example 1.
[0067] Test Method: The test was conducted according to AATCC 195—2017 "Liquid Moisture Management Performance of Textile Fabrics". Each sample was cut into 8cm × 8cm specimens and equilibrated for 24 hours under standard atmospheric conditions (20±2℃, 65±4%RH). The specimens were placed on a Liquid Moisture Management Tester (MMT), and a quantitative test solution (0.15mL, 0.9% sodium chloride solution) was added to the upper surface of the specimen (the simulated skin contact surface). The instrument automatically recorded and calculated the One-Way Moisture Transfer Index (OMMC, dimensionless; a higher value indicates better one-way moisture wicking performance) for each specimen. The test results are shown in Table 3.
[0068] Table 3: Test Results The three-layer composite fabric of Example 1 (sample G) achieved a unidirectional moisture transfer index of 0.94, exhibiting excellent unidirectional moisture wicking performance. The single-layer hydrophilic nanofiber membrane (sample H) had an OMMC value of -0.12, indicating that moisture diffuses bidirectionally within the membrane and lacks unidirectional transfer capability. The coated temperature-regulating fabric of Comparative Example 1 (sample I) had an OMMC value of only 0.08, indicating that the coating severely blocked the fabric's moisture-wicking channels. This demonstrates that the present invention achieves effective unidirectional transport of sweat through a gradient design of wettability from a skin-friendly moisture-wicking layer (superhydrophilic) to a biomimetic self-healing outer layer (superhydrophobic).
[0069] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the technical solutions of the embodiments of the present invention.
Claims
1. A new garment material, characterized in that, It includes, in sequence: a skin-friendly moisture-wicking layer, an intelligent temperature-regulating intermediate layer, and a biomimetic self-healing outer layer; The skin-friendly moisture-wicking layer includes polycaprolactone and carboxylated chitosan; The intelligent temperature-regulating intermediate layer is a phase change microcapsule; The biomimetic self-healing outer layer comprises a blend of self-healing polyurethane and polyvinylidene fluoride-hexafluoropropylene copolymer.
2. The novel garment material according to claim 1, characterized in that, The polycaprolactone has a number-average molecular weight of 80,000, the carboxylated chitosan has a number-average molecular weight of 15,000, and the degree of carboxylation is ≥90%. The self-healing polyurethane is prepared from polytetrahydrofuran diol, isophorone diisocyanate, 2,2'-diaminodiphenyl disulfide, and 3,3',5,5'-tetrabromobisphenol A as raw materials; the number average molecular weight of the polytetrahydrofuran diol is 2000, and the weight average molecular weight of the polyvinylidene fluoride-hexafluoropropylene copolymer is 400,000; and the molar ratio of vinylidene fluoride monomer to hexafluoropropylene monomer in the polyvinylidene fluoride-hexafluoropropylene copolymer is 88:
12.
3. The novel garment material according to claim 1, characterized in that, The phase change microcapsule consists of a shell and a core layer; The core layer comprises lauric acid and myristic acid, the shell layer is a silica shell layer, the shell layer is wrapped around the surface of the core layer, and the outer surface of the silica shell layer is coated with hydroxylated multi-walled carbon nanotubes.
4. The novel garment material according to claim 1, characterized in that, The mass ratio of polycaprolactone to carboxylated chitosan is (70:30) to (95:5). The water contact angle of the skin-friendly moisture-wicking layer is less than 30°, and the water contact angle of the biomimetic self-healing outer layer is greater than 140°.
5. The novel garment material according to claim 3, characterized in that, The hydroxylated multi-walled carbon nanotubes have a diameter of 10nm-20nm, a length of 10μm-30μm, and a hydroxyl content of 1wt%~3wt% of the mass of the multi-walled carbon nanotubes. The amount of the silica shell is 15% to 40% of the core layer mass; The amount of multi-walled carbon nanotubes used is 0.5% to 5.0% of the core layer mass.
6. The novel garment material according to claim 2, wherein, The mass ratio of lauric acid to myristic acid is (60:40) ~ (85:15). The molar ratio of isophorone diisocyanate to polytetrahydrofuran diol is (1.6~2.4):1; The molar ratio of 2,2'-diaminodiphenyl disulfide to 3,3',5,5'-tetrabromobisphenol A is 1:(6~2).
7. A method for producing a novel garment material as claimed in any one of claims 1 to 6, characterized in that, Includes the following steps: S1. Prepare the intelligent temperature-regulating intermediate layer; S2. Prepare a skin-friendly and moisture-wicking layer; S3. Prepare a biomimetic self-healing outer layer; S4, hot-pressed composite.
8. The method of producing a new garment material according to claim 7, characterized in that, S1 specifically includes the following steps: S101, Prepare the core material melt; S102. Emulsify the core material melt with deionized water to form an oil-in-water emulsion; S103. The water-in-oil emulsion is used to prepare phase change microcapsules.
9. The application of a novel clothing material as described in any one of claims 1 to 6 in the preparation of outdoor sportswear or medical protective clothing.