Catalyst for preparing methane by directly driving water and carbon dioxide through solar energy as well as preparation method and application of catalyst
Through Nb-doped W18O49 nanomaterial, the full spectrum absorption and photothermal conversion of solar light are achieved, solving the problems of existing photocatalysts' limited light response range and external heating source, and improving the efficiency and selectivity of CO2 conversion to methane, which is in line with Requirements for sustainable development.
Patent Information
- Application Number
- CN202411100572.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-22
AI Technical Summary
The light response range of existing photocatalysts is limited to the ultraviolet-visible area, and the utilization rate of sunlight is low, making it difficult to achieve the UV-visible-near-infrared full spectrum solar light response. Traditional reactions require external heating sources, efficiency and selectivity. insufficient.
Using Nb-doped W18O49 nanomaterial as catalyst, synthesis by solvothermal method provides higher specific surface area and photogenerated carrier separation and migration efficiency. It uses full-spectrum absorption and photothermal conversion of solar light to efficiently convert CO2 to methane. , and no external heating source is required.
The photocatalytic activity and product selectivity of the catalyst are significantly improved, and the efficient conversion of CO2 and H2O into methane is achieved, which overcomes the dependence on external heating sources in traditional technology, and has good sustainable development characteristics and application prospects.
Smart Images

Figure CN118988288A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of catalytic material preparation, and in particular relates to a catalyst for producing methane by directly driving water and carbon dioxide with solar energy, and a preparation method and application thereof. Background Art
[0003] Methane is a high-quality, safe, efficient and clean hydrocarbon resource. The catalytic conversion of CO2 into CH4 is one of the important ways to reuse CO2, which can not only solve the problem of CO2 emissions, but also synthesize new energy and realize the resource utilization of CO2.
[0004] Photocatalytic technology can directly use sunlight to convert CO2 into fuel or chemical raw materials by simulating natural photosynthesis, effectively realizing the resource utilization of CO2. The light response range of most photocatalysts reported so far is limited to the UV-visible region, and the utilization rate of sunlight is low. How to develop catalysts that respond to the full spectrum of UV-visible-near infrared (UV-vis-NIR) sunlight and improve their catalytic activity and product selectivity is a key issue in the research field of direct solar-driven water and CO2 production of hydrocarbons. Summary of the invention
[0005] The purpose of the present invention is to overcome the above-mentioned problems existing in the conventional technology and to provide a catalyst for producing methane by directly driving water and carbon dioxide with solar energy and a preparation method and application thereof.
[0006] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:
[0007] The present invention provides a catalyst for producing methane by directly driving water and carbon dioxide with solar energy. The catalyst is a Nb-doped W 18 O 49 The nanomaterial has a mass fraction of Nb element in the catalyst of 3.88-10.29wt.%.
[0008] The present invention also provides a method for preparing the above catalyst, comprising the following steps:
[0009] 1) Weigh a certain amount of tungsten-containing raw material and niobium-containing raw material respectively, add them into ethanol, and stir and dissolve them at room temperature to form a solution;
[0010] 2) The solution is transferred to a hydrothermal reactor, sealed and kept at 180-200°C for 12-24 hours; then cooled to room temperature, the precipitate is collected, washed and dried to obtain Nb-doped W 18 O 49 Nanomaterial, which is the target catalyst.
[0011] Furthermore, in step 1), the tungsten-containing raw material is a tungsten-containing soluble salt.
[0012] Furthermore, in step 1), the tungsten-containing raw material is tungsten hexachloride.
[0013] Furthermore, in step 1), the niobium-containing raw material is a soluble salt containing niobium.
[0014] Furthermore, in step 1), the niobium-containing raw material is niobium pentachloride.
[0015] Furthermore, in step 1), the concentration of tungsten in the solution is 0.013-0.025 mol / L, and the molar ratio of niobium to tungsten is 0.10-0.30:1.
[0016] The present invention also provides the use of the catalyst in directly driving water and carbon dioxide to produce methane using solar energy.
[0017] Furthermore, the carbon dioxide conversion reaction is carried out in a gas-solid reaction system.
[0018] Further, the operation is as follows: a certain amount of catalyst is weighed, dispersed in a sealed container such as a quartz glass container, a mixed gas of carbon dioxide and water vapor is introduced, and the reaction is carried out under light.
[0019] The beneficial effects of the present invention are:
[0020] 1. The catalyst of the present invention is Nb 5+ Uniformly doped with W 18 O 49 W 18 O 49 As a light-absorbing semiconductor, Nb-doped 5+ Provides more metal active sites. Nb doping causes W 18 O 49 The lattice expands and changes its morphology, significantly increasing the specific surface area of the catalyst, enhancing the adsorption capacity of CO2, and also improving the separation and migration efficiency of photogenerated carriers. 18 O 49 The surface has abundant defect sites, which is conducive to enhancing the adsorption of CO2 and H2O molecules and reaction intermediates. The doped Nb sites can promote the water oxidation half-reaction and thus increase the proton supply rate, significantly improving the reaction efficiency and selectivity of the photocatalytic reduction of CO2 to produce CH4.
[0021] 2. The catalyst of the present invention has excellent full-spectrum sunlight absorption properties and good photothermal conversion capabilities. By utilizing the synergistic effect of photothermal effect and multiple catalytic sites, CO2 can be converted into methane with high efficiency and selectivity under sunlight.
[0022] 3. The catalyst of the present invention has good photothermal conversion ability. Under the irradiation of sunlight, it mainly acts on photocatalysis and supplemented by photothermal effect to achieve efficient conversion of CO2 and H2O, overcoming the problem that traditional reactions require external heat sources, conforming to the sustainable development energy strategy, and having broad application prospects.
[0023] 4. The raw materials used in the catalyst preparation method proposed in the present invention are low in cost and easy to obtain, and do not involve the use of precious metals; the preparation process is simple, the equipment requirements are low, it is environmentally friendly, and it meets the requirements of sustainable development. It is a catalyst synthesis method that can be mass-produced; in the photocatalytic reduction of CO2 and H2O to produce methane, the amount of catalyst used is small and can be recycled, which has the characteristics of sustainable development.
[0024] 5. The catalyst of the present invention can generate methane at a rate of 20.27 μmol·g under normal pressure, simulated sunlight and without external heat source. cat -1 ·h -1 The methane product selectivity is 82.6%, and the conversion of CO2 and H2O into methane is achieved through a mild, environmentally friendly and energy-saving approach.
[0025] 6. The catalyst of the present invention can directly utilize sunlight to catalyze the conversion of CO2 and H2O into CH4 by simulating photosynthesis in nature, thereby realizing the resource utilization of carbon dioxide.
[0026] Of course, any product implementing the present invention does not necessarily need to achieve all of the above advantages at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0028] Figure 1 are XRD patterns of the catalysts prepared in Examples 1 to 4 and Comparative Example 1, respectively;
[0029] Figure 2 are SEM images of the catalysts prepared in Example 1 and Comparative Example 1, respectively;
[0030] Where (ab) is W 18 O 49 , (cf) is Nb 0.20 -W 18 O 49 ;
[0031] Figure 3 TEM, HRTEM and HAADF-STEM of the catalyst prepared in Example 1 and the corresponding element distribution diagram;
[0032] Figure 4 1 and 2 are XPS graphs of the catalysts prepared in Example 1 and Comparative Example 1, respectively.
[0033] Figure 5 are the UV-visible absorption spectra of the catalysts prepared in Examples 1 to 4 and Comparative Example 1, respectively;
[0034] Figure 6 The catalysts prepared in Examples 1 to 4 and Comparative Example 1 were respectively subjected to UV-vis (320-780nm, 0.40W·cm -2 ) Schematic diagram of the photocatalytic reaction of CO2 and H2O;
[0035] Figure 7 Schematic diagram of the results of the photocatalytic reaction of CO2 and H2O under UV-vis for the catalysts prepared in Comparative Examples 2 and 3, respectively;
[0036] Figure 8 It is a schematic diagram of the change of catalyst surface temperature over time under light of different wavelength ranges in Example 1 and the results of the photocatalytic reaction of CO2 and H2O under corresponding conditions. DETAILED DESCRIPTION
[0037] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] The present invention provides a catalyst for producing methane by directly driving water and CO2 with solar energy, and its preparation method and application. The catalyst of the present invention is a W doped with Nb element synthesized by a solvent thermal method. 18 O 49 Nanostructured materials, including W 18 O 49 It has excellent full-spectrum sunlight absorption ability and good photothermal conversion ability. 5+Excellent catalytic active sites are provided. By utilizing the synergistic effect of the photothermal effect and multiple catalytic sites, the catalyst of the present invention can convert CO2 and H2O into methane with high efficiency and selectivity under sunlight. The catalytic process overcomes the problem that traditional reactions require an external heat source. The raw materials used in the preparation method of the catalyst of the present invention are low in cost and easy to obtain, do not involve the use of precious metals, have a simple preparation process, low equipment requirements, are environmentally friendly, and meet the requirements of sustainable development. The catalyst of the present invention achieves efficient and highly selective conversion of CO2 into methane through a gentle, environmentally friendly and energy-saving approach, which is in line with the sustainable development energy strategy and has broad application prospects.
[0039] The relevant specific embodiments of the present invention are as follows:
[0040] Example 1
[0041] This embodiment provides a method for preparing a catalyst for producing methane by directly driving water and CO2 using solar energy, comprising the following steps:
[0042] 1) 30 mL of anhydrous ethanol was taken as a solvent, and then 27.0 mg of niobium pentachloride was weighed and transferred to the anhydrous ethanol, and stirred to dissolve at room temperature;
[0043] 2) Weigh 200 mg of tungsten hexachloride and transfer it to the above niobium pentachloride ethanol solution, stir at room temperature, and dissolve to form a yellow solution;
[0044] 3) The yellow solution was transferred to a hydrothermal reactor, kept at 200°C for 12 h, then cooled to room temperature, the precipitate was collected, washed and dried to obtain Nb-doped W 18 O 49 Catalyst, denoted as Nb 0.20 -W 18 O 49 .
[0045] Example 2
[0046] The difference between this embodiment and embodiment 1 is that the amount of niobium pentachloride in step 1) is changed to 13.5 mg, and the obtained catalyst is recorded as Nb 0.10 -W 18 O 49 .
[0047] Example 3
[0048] The difference between this embodiment and embodiment 1 is that the amount of niobium pentachloride in step 1) is changed to 20.6 mg, and the obtained catalyst is recorded as Nb 0.16 -W 18 O 49 .
[0049] Example 4
[0050] The difference between this embodiment and embodiment 1 is that the amount of niobium pentachloride in step 1) is changed to 40.6 mg, and the obtained catalyst is recorded as Nb 0.30 -W 18 O 49 .
[0051] Comparative Example 1
[0052] The difference between Comparative Example 1 and Example 1 is that niobium pentachloride is not added, and the other conditions are the same. The obtained sample is recorded as W 18 O 49 .
[0053] Comparative Example 2
[0054] The difference between Comparative Example 2 and Example 1 is that niobium pentachloride is not added, and other conditions are the same. The obtained sample is calcined at 600°C in an air atmosphere, with a heating rate of 4°C / min and a holding time of 2.5h. The sample obtained after calcination is recorded as WO3.
[0055] Comparative Example 3
[0056] The difference between Comparative Example 3 and Example 1 is that the sample obtained in Example 1 is calcined at 600°C in an air atmosphere, with a heating rate of 4°C / min and a holding time of 2.5h. The sample obtained after calcination is recorded as Nb-WO3.
[0057] The catalysts prepared in the above examples were analyzed by XRD. Figure 1 As shown, the characteristic peaks at 2θ≈23.5° and 47.8° correspond to the monoclinic W 18 O 49 (010) and (020) planes of (JCPDS No.71-2450) indicate that W 18 O 49 The catalyst Nb prepared in Example 1 0.20 -W 18 O 49 The XRD pattern mainly shows that W 18 O 49 The diffraction peaks of , indicating that Nb element doping does not change its crystal phase. Figure 1 The XRD partial enlarged image on the right shows that Nb doped W 18 O 49 The (010) diffraction peak of Nb 5+ (64pm) has a higher 6+ (60pm) and W 5+ (62pm) larger ionic radius, Nb 5+ Enter W 18 O 49Substituting part of W in the lattice 6+ or W 5+ ions, leading to W 18 O 49 The lattice of W is slightly expanded and distorted, which slightly increases the corresponding interplanar spacing. XRD test results show that Nb is successfully doped into W 18 O 49 in the crystal lattice.
[0058] Figure 2 2a and 2b show W prepared in Comparative Example 1 18 O 49 SEM images of the catalyst. Figure 2 c~f are Nb prepared in Example 1 0.20 -W 18 O 49 SEM image of the catalyst. It can be seen from the SEM image that pure W 18 O 49 It presents a sea urchin-like structure composed of nanowires, while Nb 0.20 -W 18 O 49 The flower-like structure morphology is composed of nanosheets, and the results show that Nb doping causes W 18 O 49 morphological changes.
[0059] Figure 3 a, 3b and 3c show the Nb prepared in Example 1 0.20 -W 18 O 49 TEM, HRTEM and element distribution of the catalyst. The HRTEM image shows that W 18 O 49 The lattice fringes of the (010) crystal plane, Figure 3 The element distribution diagram shown in c shows that Nb is evenly distributed in W 18 O 49 In the structure.
[0060] Figure 4 The XPS spectra of the catalysts prepared in Example 1 and Comparative Example 1, respectively. Figure 4 a is the XPS full spectrum of the two catalysts. The results show that Nb prepared in Example 1 0.20 -W 18 O 49 The catalyst contains W, O and Nb elements. Figure 4 bd show the high-resolution XPS spectra of Nb, O, and W. The binding energy of W4f and O1s moves to a lower binding energy after Nb doping, indicating that Nb doping regulates the W 18 O 49 The electronic structure of .
[0061] Figure 5 The UV-visible absorption spectra of the catalysts prepared in Examples 1 to 4 and Comparative Example 1 respectively show that the pure W prepared in Comparative Example 1 18 O 49 It has wide spectrum light absorption capability from UV to vis to NIR, indicating that W 18 O 49 It is a carrier with high light absorption properties.
[0062] Application examples:
[0063] The catalysts prepared in Examples 1 to 4 and Comparative Examples 1 to 3 were applied to the photocatalytic CO2 reduction reaction. The specific application steps are as follows:
[0064] 1) Weigh 5 mg of the catalyst and ultrasonically disperse it in 0.8 mL of deionized water to form a suspension. The suspension was evenly coated on a 2.5 cm × 2.5 cm glass sheet and dried in a 60 ° C vacuum oven. The glass sheet coated with the catalyst was then transferred to the bottom of a 170 mL quartz reactor, and 1 mL of deionized water was dripped near it. CO2 gas was continuously introduced into the reactor for 20 min and the reactor was sealed.
[0065] 2) Using Xe lamp as the light source, different filters were used to obtain illumination conditions in different wavelength ranges, including UV-vis (320-780nm, 0.40W·cm -2 ), UV-vis-NIR (320-2500nm, 2.60W·cm -2 )、vis(420-780nm,0.35W·cm -2 )、NIR(800-2500nm,1.1W·cm -2 ) and vis-NIR (420-2500nm, 2.20W·cm -2 ), respectively, photocatalytic CO2 reduction reaction was carried out, sampling was carried out every 1 hour for detection, and the reaction lasted for 5 hours; the gas products were analyzed using a gas chromatograph.
[0066] Figure 6 The catalysts prepared in Examples 1-4 and Comparative Example 1 were tested under UV-vis (320-780 nm, 0.40 W·cm -2 ) irradiated by photocatalytic CO2 reduction reaction, wherein the Nb prepared in Example 1 0.20 -W 18 O 49 The catalyst has the best performance, with the corresponding CH4 and CO production rates of 14.50 and 8.67 μmol·g cat -1 ·h -1, the selectivity of CH4 is 62.6%. 18 O 49 The corresponding CH4 and CO production rates are 0.57 and 0.32 μmol·g cat - 1 ·h -1 .
[0067] like Figure 7 As shown in Figure 2, the CH4 and CO generation rates corresponding to the WO3 catalyst prepared in Comparative Example 2 are 0.43 and 0.74 μmol·g cat - 1 ·h -1 The generation rates of CH4 and CO corresponding to the Nb-WO3 catalyst prepared in Comparative Example 3 were 0.86 and 0.75 μmol·g cat -1 ·h -1 .
[0068] Figure 8 a shows Nb 0.20 -W 18 O 49 The surface temperature of the catalyst changes with time under different light conditions. Under UV-vis irradiation, its surface temperature is stable at around 62.0°C; under UV-vis-NIR irradiation, its surface temperature is stable at 165.6°C, indicating that the catalyst has good photothermal conversion ability. The significant absorption of near-infrared light not only improves the utilization rate of sunlight, but also provides a significant light-induced heating effect for the reaction. Figure 8 b shows Nb 0.20 -W 18 O 49 The photocatalytic CO2 reduction performance of the catalyst under different light conditions. The generation rates of CH4 and CO under UV-vis-NIR irradiation were 20.27 and 4.28 μmol·g cat -1 ·h -1 , CH4 selectivity increased to 82.6%.
[0069] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A catalyst for producing methane by directly driving water and carbon dioxide with solar energy, characterized in that: The catalyst is a Nb-doped W 18 O 49 The nanomaterial has a mass fraction of Nb element in the catalyst of 3.88-10.29wt.%.
2. The method for preparing the catalyst according to claim 1, characterized in that: The steps include: 1) Weigh a certain amount of tungsten-containing raw material and niobium-containing raw material respectively, add them into ethanol, and stir and dissolve them at room temperature to form a solution; 2) The solution is transferred to a hydrothermal reactor, sealed and kept at 180-200°C for 12-24 hours; then cooled to room temperature, the precipitate is collected, washed and dried to obtain Nb-doped W 18 O 49 Nanomaterial, which is the target catalyst.
3. The preparation method according to claim 2, characterized in that: In step 1), the tungsten-containing raw material is a tungsten-containing soluble salt.
4. The preparation method according to claim 3, characterized in that: In step 1), the tungsten-containing raw material is tungsten hexachloride.
5. The preparation method according to claim 2, characterized in that: In step 1), the niobium-containing raw material is a soluble salt containing niobium.
6. The preparation method according to claim 5, characterized in that: In step 1), the niobium-containing raw material is niobium pentachloride.
7. The preparation method according to claim 2, characterized in that: In step 1), the concentration of tungsten in the solution is 0.013-0.025 mol / L, and the molar ratio of niobium to tungsten is 0.10-0.30:
1.
8. Use of the catalyst as claimed in claim 1 in direct solar energy-driven production of methane from water and carbon dioxide.
9. The use according to claim 8, characterized in that: The carbon dioxide conversion reaction is carried out in a gas-solid reaction system.
10. The use according to claim 9, characterized in that: The operation is as follows: weigh a certain amount of catalyst, disperse it in a sealed container, introduce a mixed gas of carbon dioxide and water vapor, and react under light.
Citation Information
Patent Citations
Preparation method of oxygen-deficit tungsten oxide
CN110563042A
Nb2O5 / W18O49 heterojunction nanofiber photocatalyst as well as preparation method and application thereof
CN118105970A
Reducing apparatus and reducing method of carbon dioxide using solar light
KR1020130044704A
Cited By
Preparation method of full-spectrum-response plasmon photocatalyst for reducing carbon dioxide to prepare methane
CN120054486A
Preparation method of plasmonic photocatalyst for carbon dioxide reduction to produce methane with full spectrum response
CN120054486B