Surface-catalyzed modified TiMn-based hydrogen storage alloys and their preparation and application
By introducing a hydrogen dissociation catalyst onto the surface of a TiMn-based hydrogen storage alloy, a stable catalytic interface is formed, which solves the problem of insufficient H2 molecule dissociation rate at low temperatures in TiMn alloys. This achieves rapid hydrogen absorption and efficient hydrogen storage performance at low temperatures, making it suitable for rapid hydrogen charging at low temperatures and engineering hydrogen storage applications.
Patent Information
- Application Number
- CN202611350011.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-02
- Publication Date
- 2026-11-17
AI Technical Summary
Commercial TiMn-based hydrogen storage alloys exhibit insufficient H2 molecule dissociation rates at low temperatures, resulting in poor low-temperature hydrogen absorption kinetics and limiting their application in low-temperature rapid hydrogen charging, intermittent hydrogen sources, and engineering hydrogen storage beds.
Hydrogen dissociation catalysts, such as Ni, Ni-P, Ni2P, Mo2C, and Mo2N, are introduced onto the surface of TiMn-based hydrogen storage alloy particles. Stable catalytic interfaces are formed through low-energy ball milling or mechanical composite methods to promote the dissociation of H2 molecules and the migration of hydrogen atoms.
It significantly improves the hydrogen absorption kinetics of TiMn alloys from room temperature to below 80 °C, shortens the initial hydrogen absorption induction period and t50 and t90 times, maintains the hydrogen storage capacity, reduces the activation difficulty, and is low in cost and suitable for large-scale application.
Smart Images

Figure CN123105545A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the fields of solid-state hydrogen storage materials and metal hydride hydrogen storage technology, specifically to a composite hydrogen storage material in which a hydrogen dissociation catalyst is introduced on the surface of TiMn-based hydrogen storage alloy particles, its preparation method, and its application in rapid hydrogen absorption and storage at room temperature or below 80°C. Background Technology
[0002] TiMn-based hydrogen storage alloys are typical metal hydride hydrogen storage materials, characterized by high reversible hydrogen storage capacity, moderate hydrogen absorption and desorption platform pressure, relatively low raw material cost, and good engineering foundation. They are suitable for applications such as low-temperature solid-state hydrogen storage, hydrogen buffering, hydrogen purification, hydrogen compression, and mobile hydrogen sources.
[0003] However, commercial TiMn-based hydrogen storage alloys still face significant low-temperature kinetic challenges in practical applications. TiMn alloy surfaces typically exhibit the formation of Ti oxide, Mn oxide, or Ti / Mn composite oxide layers. These oxide layers hinder the adsorption and dissociation of H2 molecules on the alloy surface and further suppress hydrogen atoms from entering the alloy lattice. Therefore, unmodified TiMn alloys often require higher temperatures, higher hydrogen pressures, or multiple hydrogen adsorption / desorption cycles to achieve activation.
[0004] For low-temperature hydrogen storage systems ranging from room temperature to below 80 °C, insufficient dissociation rate of H2 molecules on the alloy surface is one of the key factors limiting hydrogen absorption kinetics. Specifically, this manifests as a long initial hydrogen absorption induction period, low initial hydrogen absorption rate at low temperatures, and a short t0... 50 and t 90 The long charging time and the inability to fully utilize the effective hydrogen absorption capacity within a short period limit the application of TiMn-based hydrogen storage alloys in low-temperature rapid hydrogen charging, intermittent hydrogen sources, and engineered hydrogen storage beds.
[0005] Existing technologies for improving the hydrogen absorption performance of TiMn alloys typically include high-temperature activation, mechanical crushing, ball milling, noble metal modification, or surface coating. However, high-temperature activation increases energy consumption and equipment complexity; excessive ball milling leads to severe pulverization, increased bed pressure drop, and decreased engineering packing performance; noble metal catalysts are expensive and not conducive to large-scale applications; while simple carbon material composites are beneficial for heat transfer and dispersion, they cannot effectively solve the problem of insufficient low-temperature dissociation capacity of H2 molecules. Therefore, a low-cost, scalable surface catalytic modification method suitable for the post-treatment of commercial TiMn-based alloys, capable of promoting H2 dissociation and hydrogen overflow at room temperature or below 80°C, is still needed. Summary of the Invention
[0006] To address the aforementioned problems, the purpose of this application is to provide a TiMn-based hydrogen storage alloy composite material with a surface-introduced hydrogen dissociation catalyst and its preparation method. This material, by constructing a low-temperature H2 dissociation-hydrogen overflow catalytic interface on the surface of TiMn-based hydrogen storage alloy particles, increases the surface dissociation rate of H2 molecules under low-temperature conditions, promotes the migration of active hydrogen atoms from the catalyst to the surface and interior of the TiMn alloy, thereby reducing the difficulty of low-temperature activation of the material and improving the hydrogen absorption kinetics from room temperature to below 80 °C.
[0007] The following technical solution is adopted in this application.
[0008] According to one aspect of this application, a surface-catalyzed TiMn-based hydrogen storage alloy composite material is provided. The composite material comprises TiMn-based hydrogen storage alloy particles and a hydrogen dissociation catalyst distributed on the surface of the TiMn-based hydrogen storage alloy particles; the hydrogen dissociation catalyst is used to promote the low-temperature adsorption and dissociation of H2 molecules and the migration of hydrogen atoms into the interior of the TiMn-based hydrogen storage alloy.
[0009] The composite material includes TiMn-based hydrogen storage alloy particles and a hydrogen dissociation catalyst distributed on the surface of the TiMn-based hydrogen storage alloy particles.
[0010] Furthermore, the hydrogen dissociation catalyst is selected from one or more active phases such as Ni, Ni-P, Ni-B, Ni-Mo, Ni2P, Mo2C, MoC, Mo2N, MoN, and MoS2, or one or more of the aforementioned active phases supported on a carbon support in a carbon-supported composite; the carbon material of the carbon support is selected from one or more of graphite, expanded graphite, acetylene black, carbon black, carbon nanotubes, graphene, N-doped carbon, or porous carbon. Preferably, the hydrogen dissociation catalyst is selected from one or more of Ni, Ni-P, Ni-B, Ni2P, Mo2C or Mo2N in the active phase, and carbon-supported composites Ni2P / C, Mo2C / C or Mo2N / C; more preferably, the hydrogen dissociation catalyst is one or more of Ni-P, Ni2P / C or Mo2C / C. The active phase in the carbon-supported composite catalyst comprises 5–60 wt% by mass, with the remainder being a carbon support; preferably, the active phase content is 10–40 wt%; more preferably, the active phase content is 20–25 wt%. The Ni2P / C, Mo2C / C, or Mo2N / C composite catalyst can be prepared by impregnation-supporting-drying-phosphating, carbonizing, or nitriding treatment. The content of the hydrogen dissociation catalyst is 0.1–10 wt% of the total mass of the composite material, preferably 0.5–5 wt%, and more preferably 1–3 wt%.
[0011] Furthermore, the TiMn-based hydrogen storage alloy is TiMn, TiMn2, or TiMn. 1.5 TiMn-based alloys, including TiMnCr, TiMnV, and TiMnCrV, or those containing one or more of the elements Cr, V, Fe, Zr, Ni, Co, Mo, Al, La, and Ce; The particle size of the TiMn-based hydrogen storage alloy particles is 10–300 μm, preferably 20–100 μm, and more preferably 30–80 μm; preferably, the median particle size of the TiMn-based hydrogen storage alloy particles is 40–65 μm. Alternatively, coarser TiMn-based hydrogen storage alloy particles of 0.3–1.0 mm can be selected according to the bed pressure drop and filling requirements.
[0012] Furthermore, the composite material further includes one or more of thermally conductive and / or electrically conductive carbon carriers; the carbon material of the carbon carrier is selected from one or more of graphite, expanded graphite, acetylene black, carbon black, carbon nanotubes, graphene, N-doped carbon, or porous carbon; the content of the carbon material is 0.1–10 wt% of the composite material, preferably 0.5–5 wt%.
[0013] Secondly, the preparation method of the TiMn-based hydrogen storage alloy composite material includes the following steps: (1) Preparation of TiMn particles: TiMn-based hydrogen storage alloy is crushed and particle size is controlled by standard sieve to obtain TiMn-based hydrogen storage alloy particles; the obtained TiMn-based hydrogen storage alloy particles are dried under certain pressure and temperature, or in an inert atmosphere and / or H2 at a certain temperature to remove adsorbed water, weakly adsorbed gas and loose surface impurities; after the treatment is completed, the particles are cooled to room temperature under inert atmosphere protection and sealed for storage. (2) Catalyst preparation: If it is a carbon-supported composite: the Ni precursor and / or Mo precursor are dissolved or dispersed in water, ethanol or a water-ethanol mixture; then a carbon support is added, and after impregnation, ultrasonic dispersion and / or stirring loading, the mixture is dried at 60–100 °C for 4–12 h to obtain the metal precursor / carbon composite precursor. Subsequently, depending on the type of target catalyst, the metal precursor or metal precursor / carbon composite precursor is subjected to phosphating, carbonization, reduction, sulfidation or nitriding treatment to obtain a hydrogen dissociation catalyst. After the treatment is completed, it is cooled to below 50 °C in an inert atmosphere and sealed for storage. (3) Surface introduction: Mechanical compounding is carried out using low-energy ball milling, roller milling, or V-type mixing method. TiMn particles and catalyst, or TiMn particles, catalyst and carbon materials, are ground and mixed using a low-energy ball milling method. Alternatively, a drum or V-type mixing method can be used to mix TiMn particles with the catalyst, or TiMn particles, catalyst and carbon materials, by loading them into a drum mixer or V-type mixer. After mechanical bonding is completed, the resulting material is dried at a certain temperature and pressure, and then cooled and sealed for storage under N2 or Ar protection.
[0014] Further, in step (1), the particle size of the TiMn-based hydrogen storage alloy particles is 10-300 μm, preferably 20-100 μm, and more preferably 30-80 μm; preferably, the median particle size of the particles is 40-65 μm, and the mass proportion of fine powder with a particle size less than 10 μm is not higher than 5%; the obtained TiMn-based hydrogen storage alloy particles are vacuum dried at 80-120 °C and an absolute pressure not higher than (less than or equal to) 100 Pa for 4-8 h, or treated in an inert atmosphere at 80-200 °C for 1-4 h, or treated in an H2 / Ar mixed atmosphere containing 1-10 vol.% H2 at 100-250 °C for 0.5-2 h to remove adsorbed water, weakly adsorbed gas and loose surface impurities; after treatment, the particles are cooled to room temperature under an inert atmosphere (such as one or more of nitrogen and argon) and sealed for storage.
[0015] Further, in step (2), the Ni precursor is selected from one or more of nickel nitrate hexahydrate, nickel chloride hexahydrate, nickel acetate, or nickel acetylacetonate; the Mo precursor is selected from one or more of ammonium heptamolybdate tetrahydrate, ammonium molybdate, sodium molybdate, molybdenum pentachloride, or molybdenum acetylacetonate; the carbon support, whether added or not, is selected from one or more of conductive carbon black, acetylene black, activated carbon, graphene, reduced graphene oxide, or expanded graphite, preferably one or two of reduced graphene oxide or expanded graphite; The phosphating treatment is performed by phosphating (sodium hypophosphite monohydrate) at 300-450 °C for 1-4 h in an atmosphere of N2 and / or Ar. The amount of sodium hypophosphite monohydrate added in the phosphating treatment is calculated based on the molar amount of Ni element, and the P / Ni molar ratio is 3:1-8:1, preferably 4:1-6:1. The carbonization process involved carbonizing at 600–800 °C for 1–4 h in a carbon-containing reducing atmosphere (CH4 / H2 mixture, where CH4 volume fraction was 20 vol.% and H2 volume fraction was 80 vol.%). The reduction treatment involves reducing the sample at 200–450 °C for 0.5–4 h in an H2 / Ar or H2 / N2 atmosphere containing 5–20 vol.% H2. The nitriding treatment was carried out in a nitrogen-containing atmosphere of 10–30 vol.% NH3 / N2 mixed gas at 500–800 °C for 1–4 h.
[0016] Furthermore, in step (3), the low-energy ball milling method uses one or more grinding media of zirconium oxide, agate or stainless steel, with a ball-to-material mass ratio of 0.5:1–5:1, a rotation speed of 50–300 rpm, a total effective processing time of 0.2–3 h, and uses an intermittent method to control the material temperature not to exceed 60 ℃. Mix by drum or V-type mixing at 10–60 rpm for 0.5–4 h; for mechanically introduced catalysts, vacuum dry the composite material at 60–120 °C and an absolute pressure not exceeding 100 Pa for 4–12 h. After mechanical composite, the resulting material is vacuum dried at 60–120 °C and an absolute pressure not exceeding 100 Pa for 4–12 h. The amount of Ni2P / C or Mo2C / C added is 0.5 to 5 wt% of the total mass of the composite material, more preferably 1 to 3 wt%.
[0017] Thirdly, the surface-catalyzed TiMn-based hydrogen storage alloy composite material is used for cryogenic hydrogen storage applications. Further, the composite material is placed in a hydrogen atmosphere and subjected to hydrogen absorption at 20–80 °C and 0.1–10 MPa, preferably 25–60 °C and 1–5 MPa.
[0018] The advantage of this application is that First, this application constructs a low-temperature H2 dissociation catalytic interface on the surface of a TiMn-based hydrogen storage alloy, enabling H2 molecules to preferentially adsorb and dissociate at catalytic sites such as Ni, Ni-P, Ni2P, Mo2C, or Mo2N, generating active hydrogen atoms. These active hydrogen atoms then migrate to the alloy surface through the catalyst / TiMn interface and subsequently enter the TiMn alloy lattice. This process weakens the barrier of the surface oxide layer to the direct dissociation of H2, thereby reducing the difficulty of low-temperature activation of the TiMn alloy.
[0019] Second, this application can significantly improve hydrogen absorption kinetics from room temperature to below 80 °C. Compared with the unmodified TiMn alloy, the surface-modified catalytic material has a shorter initial hydrogen absorption induction period and an increased initial hydrogen absorption rate. 50 and t 90 The time is shortened, and the target hydrogen absorption capacity can be reached more quickly under the same temperature and hydrogen pressure.
[0020] Third, this application adopts a low-content surface catalyst modification method, in which the catalyst is mainly distributed on the surface of TiMn particles rather than replacing a large amount of the hydrogen storage host phase. Therefore, it can maintain the main hydrogen storage capacity and hydrogen absorption / desorption plateau characteristics of TiMn alloy while improving low-temperature kinetics.
[0021] Fourth, this application preferably uses non-precious metal catalysts such as Ni, Ni-P, Ni2P, Mo2C, and Mo2N to avoid the large-scale use of precious metals such as Pd, Pt, and Ru, which has the advantages of low cost, readily available raw materials, and strong potential for large-scale preparation.
[0022] Fifth, the preparation process described in this application is applicable to the post-processing modification of commercial TiMn-based hydrogen storage alloy particles. Chemical plating, impregnation reduction, low-energy ball milling, and mechanical fusion all have engineering scale-up potential and can be integrated with existing hydrogen storage alloy crushing, screening, filling, and activation processes.
[0023] Sixth, further compounding with carbon materials such as expanded graphite, graphene, carbon black, or carbon nanotubes on the basis of introducing catalysts can simultaneously improve catalyst dispersibility, interparticle thermal conductivity, and local stress buffering capacity during cycling, which is beneficial to improving the rapid hydrogen charging stability of hydrogen storage beds. Attached Figure Description
[0024] Figure 1 The images show SEM and TEM images of the product obtained in Example 1. SEM reveals that the TiMn alloy particles maintain a complete micron-scale morphology (approximately 300–700 μm), with their surface covered by a uniform Ni2P / C composite layer, exhibiting obvious roughening and granulation characteristics. TEM further shows that Ni2P nanoparticles (approximately 50 nm) are uniformly distributed on the TiMn alloy surface, forming a tight interfacial contact with the matrix, without obvious independent phase isolation or desorption. Simultaneously, the carbon layer exists on the surface in a continuous but not completely dense form. These results demonstrate that Ni2P / C can construct a stable multi-point contact catalytic interface on the TiMn alloy surface, providing effective active sites for H2 dissociation and achieving tight coupling with the hydrogen storage matrix.
[0025] Figure 2The images show SEM and TEM images of the product obtained in Example 2. SEM reveals that the TiMn alloy particles maintain a complete micron-scale structure, with Mo2C / C and expanded graphite structural layers on their surface, exhibiting a more pronounced layered / sheet-like coverage. TEM results show that Mo2C nanoparticles are mainly distributed in the interface region at a relatively large size (approximately 50 nm), with only some particles exhibiting clear lattice fringes and directly contacting the TiMn alloy surface. Simultaneously, a distinct expanded graphite sheet network structure is observed in the outer layer, forming a continuous coverage and coating between the particles and the interface region. These results indicate that Mo2C / C and expanded graphite can construct a synergistic structure of "catalytic particles – carbon layer – thermally conductive network" on the TiMn surface, achieving the coexistence of catalytic site distribution and a structured carbon network. Detailed Implementation
[0026] The present application is described in detail below with reference to the embodiments, but the present application is not limited to these embodiments. Unless otherwise specified, the TiMn-based hydrogen storage alloy in the embodiments of the present application is a commercial TiMn-based hydrogen storage alloy, and the raw materials can be purchased commercially.
[0027] The low-temperature hydrogen absorption performance in the examples can be evaluated using a volumetric or gravimetric hydrogen storage testing device. Before testing, the sample is placed in the test chamber, evacuated, and then heated or hydrogen gas is introduced at the target temperature. The changes in hydrogen absorption pressure, the hydrogen absorption rate-time curve, and the PCT curve are recorded. Kinetic parameters include the initial hydrogen absorption induction period, the initial hydrogen absorption rate, and t0. 50 t 90 And the hydrogen absorption capacity over a fixed time period.
[0028] Example 1: TiMn-based hydrogen storage alloy mechanically modified with Ni2P / C catalyst A TiMn-based hydrogen storage alloy composite material with a Ni2P / C hydrogen dissociation catalyst introduced on its surface is prepared according to the following steps: 1. Preparation of Ni2P / C catalyst: In this embodiment, the Ni precursor is nickel nitrate hexahydrate, Ni(NO3)2·6H2O; the phosphorus source is sodium hypophosphite monohydrate, NaH2PO2·H2O; the carbon support is Vulcan XC-72 conductive carbon black; and the protective gas is high-purity nitrogen with a volume purity of not less than 99.999%. Nickel nitrate and hypophosphite are commonly used Ni and P sources for the preparation of Ni2P. Using a separated bed phosphating can reduce the direct deposition of sodium-containing byproducts on the carbon support surface; the phosphorus-containing reducing gas generated by hypophosphite during heat treatment can complete the reduction and phosphating of Ni species.
[0029] The specific steps are as follows: 1) Carbon carrier pretreatment: Weigh 4.00 g of Vulcan XC-72 conductive carbon black, place it in a vacuum drying oven, and dry it for 6 h at 120℃ and a vacuum degree not exceeding -0.09 MPa to remove the moisture adsorbed on the surface of the carbon material. After drying, transfer the carbon black to a desiccator and cool it to room temperature.
[0030] 2) Preparation of Ni precursor solution: Weigh 3.92 g Ni(NO3)2·6H2O, add it to a mixed solvent consisting of 20 mL deionized water and 10 mL anhydrous ethanol, and stir magnetically for 20 min at room temperature to completely dissolve Ni(NO3)2·6H2O, resulting in a green and transparent nickel nitrate solution.
[0031] 3) Ni-supported precursor: 4.00 g of pre-dried XC-72 carbon black was slowly added to a nickel nitrate solution while stirring. The mixture was then ultrasonically dispersed for 30 min at a power of 200–300 W (240 W in this case). The mixture was then magnetically stirred in a 60 ℃ water bath for 4 h. The resulting slurry was then subjected to slow solvent evaporation at 80 ℃. The resulting solid was vacuum dried at 80 ℃ for 12 h. The dried solid was then gently ground and passed through a 100-mesh sieve.
[0032] 4) Separate bed phosphating: Weigh 7.50 g of NaH2PO2·H2O as the phosphorus source. Evenly spread the nickel nitrate-loaded carbon black precursor in the downstream (downstream of the nitrogen flow, away from the inlet) quartz boat, and spread the NaH2PO2·H2O in the upstream (upstream of the nitrogen flow, closer to the inlet) quartz boat. Maintain a distance of 3–8 cm (6 cm in this case) between the two quartz boats.
[0033] 5) Place the two quartz boats in the constant temperature zone of the tube furnace and purge the pipeline with nitrogen at 300 mL / min for 30 min; then adjust the nitrogen flow rate to 150 mL / min. -1 The temperature was increased from room temperature to 200 °C at a rate of 2 °C / min and held for 30 min; then increased to 350 °C at a rate of 2 °C / min and held at 350 °C for 2 h; after the holding period, the temperature was naturally cooled to below 50 °C under nitrogen protection; the sample was transferred to an inert atmosphere glove box; a Ni2P / C catalyst with a Ni2P mass content of 20% was obtained. 2. Pretreatment of TiMn-based alloys: 100.0 g of commercial TiMn-based hydrogen storage alloy was weighed and subjected to jaw crushing and sieving to obtain particles with a diameter of 0.3–0.7 mm. "TiMn" indicates a nominal atomic ratio of Ti:Mn of 1:1. The TiMn-based hydrogen storage alloy particles were vacuum dried at 100 °C and an absolute pressure not exceeding 100 Pa for 6 h to remove adsorbed water, weakly adsorbed gases, and loose surface impurities. After treatment, the particles were cooled to room temperature under nitrogen protection and stored in a sealed container.
[0034] 3. Mechanical mixing of Ni2P / C and TiMn alloys: 1) Weigh out 98.00 g of pretreated TiMn alloy particles and 2.00 g of 20% Ni2P / C catalyst. Add both to a 500 mL zirconia ball mill jar, and add zirconia balls with a diameter of 5 mm. The ball-to-material mass ratio is 1:1.
[0035] 2) Low-energy ball milling was performed under argon protection under the following conditions: rotation speed: 120 rpm; single ball milling time: 30 min; number of ball milling cycles: 2; cooling down for 15 min between two ball milling cycles; total effective ball milling time: 60 min. After ball milling, the particle size of the composite particles was controlled by a combination of standard sieving and air classification. A small number of large particles were removed using an 80 μm standard sieve, and fine powder with a particle size of less than 10 μm was removed by air classification, resulting in a median particle size of 55 μm.
[0036] The Ni2P / C catalytically modified TiMn-based hydrogen storage alloy prepared in this embodiment was subjected to hydrogen absorption tests at 25 °C and an initial hydrogen pressure of 3.0 MPa. The comparative example was unmodified commercial TiMn-based hydrogen storage alloy particles with a particle size of 30–80 μm. In this application, the initial hydrogen absorption induction period refers to the time elapsed from when the hydrogen pressure in the reactor reaches 3.0 MPa until the sample's hydrogen absorption first reaches 0.05 wt%. The maximum hydrogen absorption of 1.60 wt.% refers to the sample's hydrogen absorption rate remaining below 0.005 wt%·min for 10 consecutive minutes under specified temperature and hydrogen pressure. -1 The equilibrium hydrogen absorption rate reached at time t 50 and t 90These refer to the time elapsed from the start of hydrogen absorption timing until the sample's hydrogen absorption reaches 50% and 90% of the maximum hydrogen absorption capacity during this process, respectively. Test results show that, compared to the unmodified TiMn-based hydrogen storage alloy, the initial hydrogen absorption induction period of the Ni2P / C catalytically modified composite material was shortened from 10.0 min to 2.0 min, t50 from 18 min to 6 min, and t90 from 45 min to 17 min; the hydrogen absorption capacity at 10 min increased from 0.65 wt% to 1.30 wt%, and at 60 min increased from 1.48 wt% to 1.60 wt%.
[0037] The hydrogen absorption / desorption cycle test was conducted under the following conditions: hydrogen was absorbed for 60 min at 25 ℃ and 3.0 MPa hydrogen pressure, followed by hydrogen release from the reactor and desorption under vacuum conditions of 80 ℃ and 100 Pa absolute pressure for 60 min. After desorption, the sample was cooled to 25 ℃ under vacuum conditions, and then hydrogen absorption was repeated 10 times. The hydrogen absorption capacity retention rate was calculated as the ratio of the maximum hydrogen absorption in the 10th cycle to the maximum hydrogen absorption in the 1st cycle. After 10 hydrogen absorption / desorption cycles, the hydrogen absorption capacity of the Ni2P / C catalytically modified composite material was maintained from 1.60 wt% in the 1st cycle to 1.54 wt% in the 10th cycle, with a capacity retention rate of 96.5%. 90 The activation induction period at low temperatures was 18.5 min. Under the same conditions, the hydrogen absorption capacity of the unmodified TiMn-based hydrogen storage alloy decreased from 1.48 wt% in the first cycle to 1.31 wt% in the tenth cycle, with a capacity retention rate of 88.5%. These results indicate that Ni2P / C catalytic modification can significantly shorten the low-temperature activation induction period of TiMn-based hydrogen storage alloys, increase the room-temperature hydrogen absorption rate, and improve their cycling kinetic stability.
[0038] Example 2: TiMn-based hydrogen storage alloy synergistically modified with Mo2C / C catalyst and expanded graphite 1. Preparation of Mo2C / C catalyst: In this embodiment, the following were selected: the molybdenum source was ammonium heptamolybdate tetrahydrate, (NH4)6Mo7O24·4H2O; the carbon support was Vulcan XC-72 conductive carbon black; the co-solvent was 30 wt% aqueous hydrogen peroxide solution; and the carbonization atmosphere was a 20 vol% CH4 / H2 mixed gas.
[0039] 1) Drying of carbon carrier: Weigh 4.00 g of XC-72 carbon black and dry it under vacuum at 120 ℃ for 6 h.
[0040] 2)(NH4)6Mo7O 24 Preparation of 4H2O solution: Weigh 1.73 g of (NH4)6Mo7O24 Add 4H₂O to 25 mL of deionized water and stir at 50 °C. Slowly add 1.0 mL of 30% hydrogen peroxide aqueous solution and continue stirring for 20 min until ammonium heptamolybdate is completely dissolved, yielding a clear or light yellow molybdenum precursor solution.
[0041] 3) Mo precursor loading: Slowly add 4.00 g of pre-dried XC-72 to (NH4)6Mo7O 24 • In 4H2O solution, ultrasonically disperse for 30 min; magnetically stir at 60 ℃ for 4 h; evaporate the solvent at 80 ℃; vacuum dry at 100 ℃ for 12 h; gently grind and pass through a 100 mesh sieve.
[0042] 4) Carbonization: The precursor was evenly spread in a quartz boat and placed in the constant temperature zone of a tube furnace. It was purged with 300 mL / min of high-purity Ar for 30 min; the temperature was then increased to 300 °C at 5 °C / min under an Ar atmosphere; and held at 300 °C for 1 h to carbonize (NH4)6Mo7O. 24 • Decompose the 4H2O precursor; switch the atmosphere to a 20 vol% CH4 / H2 mixed gas with a total flow rate of 100 mL / min; raise the temperature to 700 ℃ at 3℃ / min; hold at 700 ℃ for 2 h; after the holding period, switch to Ar gas; cool to below 50 ℃ under Ar protection; remove and seal for storage in an inert atmosphere.
[0043] 2. Pretreatment of expanded graphite: Weigh 1.00 g of expanded graphite, dry it under vacuum at 120 °C for 6 h, cool it and store it in an argon atmosphere.
[0044] 3. Mechanical mixing of Mo2C / C and TiMn alloys 1) Weigh 97.00 g of TiMn particles ("TiMn" indicates a nominal atomic ratio of Ti:Mn of 1:1), and vacuum dry the TiMn-based hydrogen storage alloy particles at 100℃ and an absolute pressure not exceeding 100 Pa for 6 h to remove adsorbed water, weakly adsorbed gases, and loose surface impurities. After treatment, cool to room temperature under nitrogen protection and seal for storage. 2.00 g of 20% Mo2C / C catalyst. Add both to a 500 mL zirconia ball mill jar, adding zirconia balls with a diameter of 5 mm, at a ball-to-material mass ratio of 1:1. Perform low-energy ball milling under argon protection at a speed of 100 rpm for 30 min, with a forward rotation of 15 min, a stop of 5 min, and a reverse rotation of 15 min.
[0045] 2) Add the above 99.00 g TiMn-Mo2C / C composite particles and 1.00 g pre-dried expanded graphite into a ball mill. The rotation speed is 30 rpm, the mixing time is 60 min, the atmosphere is Ar, and the loading coefficient is 30%–50% of the effective volume of the mixing container.
[0046] The Mo2C / C-expanded graphite co-modified TiMn-based hydrogen storage alloy prepared in this embodiment was subjected to hydrogen absorption tests at 25 °C and an initial hydrogen pressure of 3.0 MPa. The control group consisted of unmodified commercial TiMn-based hydrogen storage alloy particles with a particle size of 30–80 μm. The initial hydrogen absorption induction period, maximum hydrogen absorption capacity, and t were also measured. 50 and t 90 The definition is the same as in Example 1. Test results show that, compared to the unmodified TiMn-based hydrogen storage alloy, the initial hydrogen absorption induction period of the composite material was shortened from 10.0 min to 3.0 min. 50 The time was shortened from 18.0 min to 8.5 min, t 90 The time required for hydrogen absorption was shortened from 45 min to 23 min; the hydrogen absorption rate at 10 min increased from 0.65 wt% to 1.10 wt%, and the hydrogen absorption rate at 60 min increased from 1.48 wt% to 1.56 wt%. Under the same charge, reactor structure, and heat exchange conditions, the maximum temperature rise was defined as the difference between the highest temperature at the center of the sample bed and the initial temperature. The maximum temperature rise for unmodified TiMn was 4.5 ℃, while that for the composite material in this embodiment was reduced to 3.2 ℃.
[0047] The hydrogen absorption / desorption cycle conditions were as follows: hydrogen absorption was performed at 25 °C and 3.0 MPa hydrogen pressure for 60 min, followed by hydrogen desorption at 80 °C and a vacuum pressure not exceeding 100 Pa for 60 min. After cooling to 25 °C, the next cycle began, and this process was repeated 10 times. After 10 cycles, the maximum hydrogen absorption capacity of the composite material in this embodiment decreased from 1.56 wt% to 1.49 wt%, with a hydrogen absorption capacity retention rate of 95.8%, and the t90 of the 10th cycle was 25 min. Under the same conditions, the maximum hydrogen absorption capacity of unmodified TiMn decreased from 1.48 wt% to 1.31 wt%, with a capacity retention rate of 88.5%. These results indicate that the synergistic introduction of Mo2C / C catalyst and expanded graphite can improve the low-temperature hydrogen absorption kinetics of TiMn-based hydrogen storage alloys, improve heat transfer during hydrogen absorption, and enhance cycle stability.
[0048] Comparative Example 1: Unmodified commercial TiMn-based hydrogen storage alloy Commercial TiMn-based hydrogen storage alloys were crushed and their particle size was controlled by standard sieving to obtain TiMn-based hydrogen storage alloy particles with a particle size of 30–80 μm and a median particle size of 40–65 μm, wherein the mass proportion of fine powder with a particle size of less than 10 μm was not higher than 5%. The obtained particles were vacuum dried at 100 °C and an absolute pressure not exceeding 100 Pa for 6 h, and then cooled and sealed under argon protection. No Ni2P / C, Mo2C / C, Ni or other H2 dissociation catalysts were introduced, and no carbon materials such as expanded graphite were added.
[0049] The obtained unmodified TiMn-based hydrogen storage alloy was subjected to hydrogen absorption and desorption cycle tests according to the same charge amount, temperature, hydrogen pressure, and test procedure as in Example 1. The test results showed that the initial hydrogen absorption induction period of this sample at 25 °C and an initial hydrogen pressure of 3.0 MPa was 10.0 min. 50 For 18.0 min, t 90 The hydrogen absorption capacities at 45 min, 10 min, and 60 min were 0.65 wt.% and 1.48 wt.%, respectively. After 10 hydrogen absorption / desorption cycles, the maximum hydrogen absorption capacity decreased from 1.48 wt.% to 1.31 wt.%, with a capacity retention of 88.5%. Compared to Example 1, the unmodified TiMn-based hydrogen storage alloy exhibited a longer initial hydrogen absorption induction period. 50 and t 90 The significant increase indicates that TiMn particles without surface catalytic modification have a weak ability to dissociate H2 molecules at low temperatures and migrate active hydrogen.
[0050] Comparative Example 2: TiMn-based hydrogen storage alloy with only composite carbon materials 99.00 g of commercial TiMn-based hydrogen storage alloy particles with a particle size of 30–80 μm and 1.00 g of expanded graphite were weighed. The TiMn particles and expanded graphite were vacuum dried for 6 h at 100–120 °C and an absolute pressure not exceeding 100 Pa. The dried TiMn particles and expanded graphite were added to a drum mixer or V-type mixer and mixed at 30 rpm for 60 min under argon protection to obtain a TiMn-1 wt.% expanded graphite composite material, without the addition of H2 dissociation catalysts such as Ni, Ni-P, Ni2P, Mo2C, or Mo2N. The obtained material was subjected to hydrogen absorption testing under the same conditions as in Example 1. The test results showed that its initial hydrogen absorption induction period was 8.2 min, t 50 It is 15.2 min, t 90The hydrogen absorption was 0.76 wt.% and 1.50 wt.% at 38.0 min, 10 min, and 60 min, respectively. Compared with unmodified TiMn, expanded graphite can improve heat transfer and hydrogen absorption kinetics to some extent, but the improvement is significantly lower than that of the Ni2P / C catalytic modified material in Example 1, indicating that adding carbon materials alone cannot replace the surface H2 dissociation catalyst.
[0051] Comparative Example 3: Ni-based physical mixture sample without effective interfacial contact 98.00 g of commercial TiMn-based hydrogen storage alloy particles with a particle size of 30–80 μm and a median particle size D50 of 40–65 μm, and 2.00 g of Ni powder with a particle size of 1–10 μm were weighed. Both raw materials were vacuum dried at 100 ℃ and an absolute pressure not exceeding 100 Pa for 6 h, and then cooled under argon protection. Subsequently, the TiMn particles and Ni powder were added to a V-type mixer and mixed at 20 rpm for 30 min under argon protection; no grinding balls were added during the mixing process, and no ball milling, mechanical fusion, or other high-shear treatments were performed. After mixing, the resulting sample was vacuum dried at 100 ℃ and an absolute pressure not exceeding 100 Pa for 4 h, and then sealed and stored under argon protection to obtain a TiMn-2 wt.% Ni physical mixture sample.
[0052] The obtained material was subjected to hydrogen absorption testing under the same conditions as in Example 1. Because the Ni powder only had loose physical contact with the TiMn particles and did not form a uniform and stable catalytic interface on the TiMn surface, its low-temperature hydrogen absorption induction period and t... 90 Although there was some improvement, the degree of improvement was significantly lower than that of the Ni2P / C low-energy ball-milled modified sample, indicating that the uniform fixation of the catalyst on the surface of TiMn particles and effective interfacial contact are important conditions for promoting H2 dissociation and hydrogen overflow.
[0053] The comparison results between the examples and comparative examples show that this application does not simply add a second phase material to the TiMn-based hydrogen storage alloy, but rather constructs a low-temperature H2 dissociation-hydrogen overflow catalytic interface on the surface of TiMn alloy particles. This interface can improve the dissociation efficiency of H2 molecules at room temperature or below 80 °C and promote the migration of active hydrogen atoms into the interior of the TiMn alloy, thereby achieving low-temperature rapid activation and low-temperature rapid hydrogen absorption.
[0054] Comparative Example 4: Ni2P / C physical mixture sample without effective interfacial contact Weigh 98.00 g of particles with a diameter of 30–80 μm and a median particle size D. 50Commercial TiMn-based hydrogen storage alloy particles of 40–65 μm and 2.00 g of the same Ni2P / C catalyst as in Example 1, wherein the Ni2P content in the Ni2P / C catalyst is 20 wt.%. Both raw materials were vacuum dried at 100 °C and an absolute pressure not exceeding 100 Pa for 6 h, and then cooled under argon protection.
[0055] Subsequently, TiMn particles and Ni2P / C catalyst were added to a V-type mixer and mixed at 20 rpm for 30 min under argon protection. No grinding media were added during the mixing process, and no low-energy ball milling, mechanical fusion, or other high-shear treatments were performed. After mixing, the resulting sample was vacuum dried at 100 °C and an absolute pressure not exceeding 100 Pa for 4 h, then cooled and sealed under argon protection to obtain a TiMn-based hydrogen storage alloy with a simple physical mixture of Ni2P / C.
[0056] The obtained material was subjected to hydrogen absorption testing under the same conditions as in Example 1. This comparative example used the same TiMn particles, Ni2P / C catalyst type and dosage as Example 1, the only difference being the absence of low-energy ball milling. Because Ni2P / C is mainly distributed as loose aggregates between TiMn particles, it failed to uniformly fix on the TiMn surface and form a stable multi-point interfacial contact, resulting in a lower initial hydrogen absorption induction period and a shorter t0... 50 and t 90 Although there is some improvement compared to unmodified TiMn, the improvement is significantly less than that in Example 1, indicating that the effective Ni2P / C-TiMn interface formed by low-energy ball milling is an important factor in promoting H2 dissociation, hydrogen overflow, and rapid hydrogen absorption at low temperature.
[0057] Example 3: Preparation of Ni2P / rGO modified TiMn-based hydrogen storage alloy by mechanical fusion The process and conditions were the same as in Example 1, except that conductive carbon black was replaced with rGO in the catalyst preparation. 98.50 g of pretreated TiMn particles and 1.50 g of Ni2P / reduced graphene oxide catalyst with a Ni2P content of 20 wt.% were weighed and added to a mechanical fusion apparatus. The mixture was treated at 600 rpm for 20 min under argon protection, and the material temperature was kept below 55 °C by jacket cooling. After treatment, the composite material was vacuum dried at 100 °C and an absolute pressure not exceeding 100 Pa for 6 h to obtain a Ni2P / rGO mechanically fused modified TiMn-based hydrogen storage alloy.
[0058] This embodiment illustrates that, in addition to low-energy ball milling, mechanical fusion can also fix the catalyst on the surface of TiMn particles and form an effective H2 dissociation-hydrogen overflow interface.
[0059] Example 4: Mo2N / C low-energy ball-milled modified TiMn-based hydrogen storage alloy The process and conditions were the same as in Example 1, except that the catalyst prepared was a Mo2N / C catalyst. The Mo precursor loading process for the Mo2N / C catalyst was carried out according to the precursor loading process of the Mo2C / C catalyst in Example 2, using ammonium heptamolybdate tetrahydrate as the Mo source and Vulcan XC-72 conductive carbon black as the carbon support to prepare a Mo precursor / carbon composite precursor. Subsequently, instead of CH4 / H2 carbonization, nitriding was performed in a 20 vol.% NH3 / N2 mixed gas, where the NH3 volume fraction was 20 vol.% and the N2 volume fraction was 80 vol.%. Specifically, the Mo precursor / carbon composite precursor was heated to 300 °C in an Ar atmosphere and held for 1 h, then switched to a 20 vol.% NH3 / N2 mixed gas, heated to 700 °C at 3 °C / min and held for 2 h, and after cooling, a Mo2N / C catalyst with a Mo2N mass content of 20 wt.% was obtained.
[0060] 98.00 g of pretreated TiMn particles and 2.00 g of Mo2N / C catalyst with a Mo2N content of 20 wt.% were weighed and added to a zirconia ball mill jar at a ball-to-particle ratio of 1:1. The mixture was ball-milled at 150 rpm for 20 min under argon protection, cooled for 10 min, and then ball-milled again for 20 min, for a total effective milling time of 40 min. After ball milling, the mixture was vacuum-dried at 100 ℃ for 6 h to obtain a Mo2N / C modified TiMn-based hydrogen storage alloy.
[0061] Example 5: TiMn-based hydrogen storage alloy synergistically modified with Ni / C and carbon nanotubes The process and conditions were the same as in Example 1, except that the catalyst prepared was a Ni / C catalyst, and carbon nanotubes were further added as a thermally / electrically conductive carbon material. The Ni precursor loading process for the Ni / C catalyst was carried out according to the precursor loading process of the Ni2P / C catalyst in Example 1, using nickel nitrate hexahydrate as the Ni source and Vulcan XC-72 conductive carbon black as the carbon support to prepare the Ni precursor / carbon composite precursor. Subsequently, instead of phosphating, a reduction treatment was performed in a 10 vol.% H2 / Ar mixed gas, where the H2 volume fraction was 10 vol.% and the Ar volume fraction was 90 vol.%. Specifically, the Ni precursor / carbon composite precursor was heated to 350 °C at 2 °C / min in a 10 vol.% H2 / Ar atmosphere, held at that temperature for 2 h, and cooled to obtain a Ni / C catalyst with a Ni mass content of 20 wt.%.
[0062] 97.00 g of TiMn particles and 2.50 g of Ni / C catalyst with a Ni content of 20 wt.% were weighed and ball-milled at 100 rpm for 45 min under argon protection. Then, 0.50 g of carbon nanotubes were added, and the mixture was stirred in a V-type mixer at 25 rpm for 60 min. After mixing, the mixture was vacuum-dried at 100 ℃ for 6 h to obtain a Ni / C-carbon nanotube synergistic modified TiMn-based hydrogen storage alloy.
[0063] Example 6: Ni2P / C modified TiMn-based hydrogen storage alloy with low catalyst content The process and conditions were the same as in Example 1, except that 99.50 g of TiMn particles and 0.50 g of Ni2P / C catalyst with a mass content of 20 wt.% were weighed and compounded under the same low-energy ball milling conditions as in Example 1 to obtain a TiMn-based hydrogen storage alloy containing 0.5 wt.% Ni2P / C.
[0064] Example 7: Ni2P / C modified TiMn-based hydrogen storage alloy with high catalyst content The process and conditions were the same as in Example 1, except that 95.00 g of TiMn particles and 5.00 g of Ni2P / C catalyst with a mass content of 20 wt.% were weighed and compounded under the same low-energy ball milling conditions as in Example 1 to obtain a TiMn-based hydrogen storage alloy containing 5 wt.% Ni2P / C.
[0065] The data in the table above show that the hydrogen dissociation catalyst can significantly shorten the initial hydrogen absorption induction period and t of TiMn-based hydrogen storage alloys. 50 and t 90 The catalyst increases hydrogen absorption within 10 minutes, indicating that it promotes low-temperature H2 dissociation and the migration of active hydrogen into the TiMn alloy. The amount of catalyst added significantly affects hydrogen absorption kinetics and effective hydrogen storage capacity: too low an amount results in insufficient active sites, while too high an amount dilutes the TiMn hydrogen storage matrix. Therefore, the preferred addition amount is 0.5–5 wt.%, more preferably 1–3 wt.%. The preparation method of this invention employs various fusion methods, with low-energy ball milling and mechanical fusion being preferred for catalyst surface fixation. Low-energy ball milling, in particular, avoids excessive pulverization while forming an effective catalytic interface, making it a preferred method. Thermally / electrically conductive carbon materials such as expanded graphite, reduced graphene oxide, and carbon nanotubes further improve catalyst dispersion and bed heat transfer, which is beneficial for enhancing rapid hydrogen absorption stability.
[0066] Comparative Example 5: Catalyst content below the lower limit of protection The process and conditions were the same as in Example 1, except that 99.95 g of TiMn particles and 0.05 g of Ni2P / C catalyst were weighed and compounded using the same low-energy ball milling method as in Example 1. The Ni2P / C content was only 0.05 wt.%, which is lower than the defined lower limit of 0.1 wt.%.
[0067] Due to the low catalyst content, the H2 dissociation active sites on the surface of TiMn particles are not adequately covered, and its low-temperature hydrogen absorption kinetics are close to those of unmodified TiMn.
[0068] Comparative Example 6: Catalyst content exceeds the protection limit The process and conditions were the same as in Example 1, except that 88.00 g of TiMn particles and 12.00 g of Ni2P / C catalyst were weighed and compounded using the same low-energy ball milling method as in Example 1. The Ni2P / C content was 12 wt.%, which is higher than the upper limit of 10 wt.%.
[0069] While an excess of catalyst can shorten the hydrogen absorption time, it will significantly dilute the TiMn hydrogen storage matrix and easily lead to catalyst agglomeration and detachment during cycling, resulting in a decrease in hydrogen absorption capacity per unit mass and cycle stability.
[0070] Comparative Example 7: TiMn particle size is below the protection range The process and conditions were the same as in Example 1, except that the TiMn alloy was crushed and graded to 3-8 μm, and then ball-milled with 2 wt.% Ni2P / C under the same conditions as in Example 1.
[0071] The sample initially absorbed hydrogen quickly, but its high fine powder content and dense packing increased gas flow resistance. During the circulation process, significant agglomeration and bed compaction occurred, resulting in a decrease in circulation capacity retention.
[0072] Comparative Example 8: TiMn particle size is higher than the protection range The process and conditions were the same as in Example 1, except that the TiMn alloy was sieved to 350–500 μm and compounded with 2 wt.% Ni2P / C under the same conditions as in Example 1.
[0073] Due to the small specific surface area of the particles, the catalyst contact interface on a unit mass of TiMn is insufficient, leading to an increased diffusion path of active hydrogen into the particle interior, resulting in t 50 and t 90 A significant increase.
[0074] Comparative Example 9: High-energy, long-term ball milling The process and conditions were the same as in Example 1, except that 98.00 g of TiMn particles and 2.00 g of Ni2P / C were weighed and continuously ball-milled at 500 rpm for 4 h under argon protection. Other conditions were the same as in Example 1.
[0075] High-energy, long-term ball milling leads to severe refinement of TiMn particles, resulting in particle D 50 The particle size was approximately 7 μm, with fine powder comprising about 38% of the particles smaller than 10 μm. The sample initially absorbed hydrogen quickly, but after cycling, it exhibited significant agglomeration, pulverization, and capacity decay, indicating the necessity of the low-energy, short-time ball milling specified in this application.
[0076] Comparative Example 10: Using non-thermally conductive inert inorganic materials The process and conditions were the same as those in Comparative Example 2, except that 99.00 g of TiMn particles and 1.00 g of SiO2 powder were weighed and compounded under the same V-type mixing conditions as in Comparative Example 2, without the addition of H2 dissociation catalyst or thermally conductive carbon material.
[0077] Comparative Example 11 The process and conditions were the same as those in Comparative Example 2, except that the 1.00 g expanded graphite in Comparative Example 2 could be replaced with 1.00 g of XC-72 conductive carbon black, while the rest of the preparation and testing conditions remained unchanged.
[0078] As can be seen from the comparative examples and embodiments above, the performance improvement of the present invention mainly comes from the H2 dissociation-hydrogen overflow catalytic interface formed on the surface of TiMn particles, rather than simply adding carbon materials, simple physical mixing, or excessive particle refinement. The Ni2P / C low-energy ball-milled modified sample exhibits the best overall performance, characterized by a short induction period and low t 90 Low hydrogen absorption capacity, high hydrogen absorption rate in 10 min and high cycle retention rate; the Mo2C / C and expanded graphite synergistic modification of the sample can reduce bed temperature rise while improving hydrogen absorption kinetics, and the heat transfer enhancement effect is more obvious.
[0079] In contrast, samples with only expanded graphite or XC-72 conductive carbon black showed limited improvement, indicating that carbon materials cannot replace surface H2 dissociation catalysts; Ni powder or N i2 The performance of the P / C simple physical mixing sample was lower than that of the low-energy ball-milled sample, indicating that effective interfacial contact is crucial. Too low a catalyst content results in insufficient active sites, while too high a content dilutes the TiMn hydrogen storage matrix. Excessively fine particles or prolonged high-energy ball milling reduces cycle stability, while excessively coarse particles are detrimental to hydrogen absorption kinetics. These results demonstrate that the catalyst type, dosage, particle size, and low-energy mechanical composite method specified in this invention are reasonable and have a synergistic effect.
Claims
1. A surface catalytically modified TiMn-based hydrogen storage alloy composite material, characterized by: The composite material includes TiMn-based hydrogen storage alloy particles and a hydrogen dissociation catalyst distributed on the surface of the TiMn-based hydrogen storage alloy particles.
2. The composite material according to claim 1, characterized in that: The hydrogen dissociation catalyst is selected from one or more active phases such as Ni, Ni-P, Ni2P, Mo2C, MoC, Mo2N, MoN, etc., or one or more of the aforementioned active phases supported on a carbon support in a carbon-supported composite. The carbon material of the carbon support is selected from one or more of graphite, expanded graphite, acetylene black, carbon black, carbon nanotubes, graphene, N-doped carbon, or porous carbon. Preferably, the hydrogen dissociation catalyst is selected from one or more of Ni, Ni-P, Ni-B, Ni2P, Mo2C or Mo2N in the active phase, and carbon-supported composites Ni2P / C, Mo2C / C or Mo2N / C; more preferably, the hydrogen dissociation catalyst is one or more of Ni-P, Ni2P / C or Mo2C / C. The active phase in the carbon-supported composite catalyst comprises 5–60 wt% by mass, with the remainder being a carbon support; preferably, the active phase content is 10–40 wt%; more preferably, the active phase content is 20–25 wt%. The Ni2P / C, Mo2C / C, or Mo2N / C composite catalyst can be prepared by impregnation-supporting-drying-phosphating, carbonizing, or nitriding treatment. The content of the hydrogen dissociation catalyst is 0.1–10 wt% of the total mass of the composite material, preferably 0.5–5 wt%, and more preferably 1–3 wt%.
3. The composite material according to claim 1, characterized in that: The TiMn-based hydrogen storage alloy is one or more of TiMn, TiMn2, TiMn 1.5 , TiMnCr, TiMnV, TiMnCrV, or the aforementioned TiMn-based alloy further containing one or more of Cr, V, Fe, Zr, Ni, Co, Mo, Al, La, Ce. The TiMn-based hydrogen storage alloy particles have a particle size of 10–300 μm, preferably 20–100 μm, more preferably 30–80 μm; preferably, the median particle size of the TiMn-based hydrogen storage alloy particles is 40–65 μm. Alternatively, coarser TiMn-based hydrogen storage alloy particles of 0.3–1.0 mm can be selected according to the bed pressure drop and filling requirements.
4. The composite material according to claim 1, characterized in that: The composite material further includes one or more of thermally conductive and / or electrically conductive carbon carriers; the carbon material of the carbon carrier is selected from one or more of graphite, expanded graphite, acetylene black, carbon black, carbon nanotubes, graphene, N-doped carbon or porous carbon; the content of the carbon material is 0.1–10 wt% of the composite material, preferably 0.5–5 wt%.
5. A method for producing a TiMn-based hydrogen storage alloy composite material as claimed in any one of claims 1 to 4, characterized by: Includes the following steps: (1) Preparation of TiMn particles: TiMn-based hydrogen storage alloy is crushed and particle size is controlled by standard sieve to obtain TiMn-based hydrogen storage alloy particles; the obtained TiMn-based hydrogen storage alloy particles are dried under certain pressure and temperature, or in an inert atmosphere and / or H2 at a certain temperature to remove adsorbed water, weakly adsorbed gas and loose surface impurities; after the treatment is completed, the particles are cooled to room temperature under inert atmosphere protection and sealed for storage. (2) Catalyst preparation: If it is a carbon-supported composite: the Ni precursor and / or Mo precursor are dissolved or dispersed in water, ethanol or a water-ethanol mixture; then a carbon support is added, and after impregnation, ultrasonic dispersion and / or stirring loading, the mixture is dried at 60–100 °C for 4–12 h to obtain the metal precursor / carbon composite precursor. Subsequently, depending on the type of target catalyst, the metal precursor or metal precursor / carbon composite precursor is subjected to phosphating, carbonization, reduction, sulfidation or nitriding treatment to obtain a hydrogen dissociation catalyst. After the treatment is completed, it is cooled to below 50 °C in an inert atmosphere and sealed for storage. (3) Surface introduction: Mechanical compounding is carried out using low-energy ball milling, roller milling, or V-type mixing method. TiMn particles and catalyst, or TiMn particles, catalyst and carbon materials, are ground and mixed using a low-energy ball milling method. Alternatively, a drum or V-type mixing method can be used to mix TiMn particles with the catalyst, or TiMn particles, catalyst and carbon materials, by loading them into a drum mixer or V-type mixer. After mechanical bonding is completed, the resulting material is dried at a certain temperature and pressure, and then cooled and sealed for storage under N2 or Ar protection.
6. The preparation method according to claim 5, characterized in that: In step (1), the particle size of the TiMn-based hydrogen storage alloy particles is 10–300 μm, preferably 20–100 μm, and more preferably 30–80 μm; preferably, the median particle size of the particles is 40–65 μm, and the mass proportion of fine powder with a particle size less than 10 μm is not higher than 5%; the obtained TiMn-based hydrogen storage alloy particles are vacuum dried at 80–120 °C and an absolute pressure not higher than (less than or equal to) 100 Pa for 4–8 h, or treated in an inert atmosphere at 80–200 °C for 1–4 h, or treated in an H2 / Ar mixed atmosphere containing 1–10 vol.% H2 at 100–250 °C for 0.5–2 h to remove adsorbed water, weakly adsorbed gas and loose surface impurities; after treatment, the particles are cooled to room temperature under an inert atmosphere (such as one or more of nitrogen and argon) and sealed for storage.
7. The preparation method according to claim 5, characterized in that: In step (2), the Ni precursor is selected from one or more of nickel nitrate hexahydrate, nickel chloride hexahydrate, nickel acetate, or nickel acetylacetonate; the Mo precursor is selected from one or more of ammonium heptamolybdate tetrahydrate, ammonium molybdate, sodium molybdate, molybdenum pentachloride, or molybdenum acetylacetonate; the carbon support, whether added or not, is selected from one or more of conductive carbon black, acetylene black, activated carbon, graphene, reduced graphene oxide, or expanded graphite, preferably one or two of reduced graphene oxide or expanded graphite. The phosphating treatment is performed by phosphating (sodium hypophosphite monohydrate) at 300-450 °C for 1-4 h in an atmosphere of N2 and / or Ar. The amount of sodium hypophosphite monohydrate added in the phosphating treatment is calculated based on the molar amount of Ni element, and the P / Ni molar ratio is 3:1-8:1, preferably 4:1-6:
1. The carbonization process involved carbonizing at 600–800 °C for 1–4 h in a carbon-containing reducing atmosphere (CH4 / H2 mixture, where CH4 volume fraction was 20 vol.% and H2 volume fraction was 80 vol.%). The reduction treatment involves reducing the sample at 200–450 °C for 0.5–4 h in an H2 / Ar or H2 / N2 atmosphere containing 5–20 vol.% H2. The nitriding treatment was carried out in a nitrogen-containing atmosphere of 10–30 vol.% NH3 / N2 mixed gas at 500–800 °C for 1–4 h.
8. The method of claim 5, wherein: In step (3), the low-energy ball milling method uses one or more grinding media of zirconium oxide, agate or stainless steel, with a ball-to-material mass ratio of 0.5:1–5:1, a rotation speed of 50–300 rpm, a total effective processing time of 0.2–3 h, and uses an intermittent method to control the material temperature not to exceed 60 ℃. Mix by drum or V-type mixing at 10–60 rpm for 0.5–4 h; for mechanically introduced catalysts, vacuum dry the composite material at 60–120 °C and an absolute pressure not exceeding 100 Pa for 4–12 h. After mechanical composite, the resulting material is vacuum dried at 60–120 °C and an absolute pressure not exceeding 100 Pa for 4–12 h. The amount of Ni2P / C or Mo2C / C added is 0.5 to 5 wt% of the total mass of the composite material, more preferably 1 to 3 wt%.
9. A surface-catalytically modified TiMn-based hydrogen storage alloy composite material according to any one of claims 1-4 for use in cryogenic hydrogen storage.
10. Use according to claim 9, characterized in that: The above composite material is placed in a hydrogen atmosphere and subjected to hydrogen absorption at 20–80 °C and 0.1–10 MPa, preferably at 25–60 °C and 1–5 MPa.