A composite hydrogen storage alloy particle, bed, preparation method, application, and hydrogen storage device.
By introducing aluminum/copper powder, graphite, and metal fibers into hydrogen storage alloy particles to construct a three-dimensional network structure, the problems of volume expansion and decreased thermal conductivity of hydrogen storage alloys during hydrogen absorption and desorption cycles were solved, achieving high-efficiency hydrogen storage material stability and fast reaction rate.
Patent Information
- Application Number
- CN202611359729.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-03
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies have failed to effectively address the problems of pulverization, sedimentation, and decreased thermal conductivity of hydrogen storage alloys due to volume expansion during hydrogen absorption and desorption cycles, especially in repeated reversible hydrogen absorption and desorption cycles, where alloy particles break, containers are damaged, and heat exchange is not timely.
Aluminum/copper powder is used as an elastic buffer and thermal conductive material, flake graphite/microcrystalline graphite/expanded graphite is used as a lubricating material, and metal fiber is used as a rigid skeleton material to construct a three-dimensional network structure. The integral porous block is formed by binder to achieve the synergistic functions of elastic buffer, rigid support and efficient thermal conduction.
It effectively suppresses the volume expansion effect of hydrogen storage alloys, prevents pulverization and deposition, extends the service life of hydrogen storage devices, improves thermal conductivity, significantly accelerates the hydrogen absorption and desorption rate, and maintains hydrogen storage capacity. The volume expansion rate is reduced to less than 10%, and the thermal conductivity is increased by more than 10 times.
Smart Images

Figure CN123105546A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of solid hydrogen storage material technology, specifically relating to a composite hydrogen storage alloy particle, bed, its preparation method, application, and hydrogen storage device. Background Technology
[0002] Solid-state hydrogen storage technology has shown great potential in vehicle-mounted hydrogen storage and stationary energy storage due to its advantages of high volumetric hydrogen storage density and low-pressure safety. However, solid-state hydrogen storage technology faces a core bottleneck in engineering applications: the hydrogen storage alloy undergoes lattice expansion during hydrogen absorption, with its volume expanding by 15% to 25%, and shrinks after hydrogen release. Repeated hydrogen absorption and release cycles lead to serious problems.
[0003] During the reversible hydrogen absorption and desorption cycle, repeated volume changes of hydrogen storage alloys can lead to the following serious problems: (1) Alloy pulverization: The huge internal stress causes the alloy particles to break into fine powder, the particle size of the powder drops from the hundreds of micrometers to the micrometers, the specific surface area increases sharply, and it is easily oxidized and degraded; (2) Container damage: The powder settles and accumulates under the action of gravity, the bottom density increases, the expansion of the accumulation area is limited during subsequent hydrogen absorption, and the accumulated stress is generated on the bottle wall, which leads to container deformation or even rupture; (3) Decreased thermal conductivity: The porosity of the alloy bed changes after pulverization, the contact thermal resistance increases, and the heat cannot be exchanged in time during the hydrogen absorption and desorption process, which reduces the reaction rate.
[0004] To overcome the above problems, researchers have proposed several solutions: CN114507798A discloses a method for preparing magnesium-based hydrogen storage alloy blocks by pressing magnesium-nickel-rare earth alloy powder. However, the alloy powder used in this method is prepared by atomization powder preparation, which results in high production costs, and the material can only be effectively charged and decharged with hydrogen at 300°C, thus limiting its practical application.
[0005] CN118687076A discloses a method for filling solid hydrogen storage cylinders using PTFE or CMC solution as dispersion, aluminum powder, graphite or carbon nanotubes as heat transfer materials, and thermosetting epoxy resin as additive. The cured epoxy resin provides some buffering for the volume expansion of the alloy powder during absorption and desorption, but due to the lack of skeletal support, long-term cycling leads to pulverization and sedimentation problems.
[0006] CN121516851A discloses a method for preparing hydrogen storage particles by using a volatile organic solvent as a dispersant and combining fiber materials with alloy powder, which gives the prepared particles a certain skeletal structure to improve the powder's resistance to pulverization. However, this method does not add a good thermally conductive material.
[0007] CN121516815A relates to an anti-pulverization composite hydrogen storage particle, which comprises hydrogen storage alloy powder and fiber material, with the fiber material accounting for 3-50% by weight. By adding a dispersant to improve mixing efficiency and pressing the material into granular blocks, composite hydrogen storage block particles with a "reinforced concrete" structure can be obtained. However, this solution relies solely on the fiber material to provide anti-pulverization capability, without addressing the synergistic effect of elastic buffer components and lubricating components, nor optimizing thermal conductivity.
[0008] CN122256757A discloses a composite hydrogen storage briquette with high thermal conductivity and resistance to cracking and pulverization, and its preparation method. The briquette, by mass percentage, comprises 85%–90% hydrogen storage alloy powder, 2%–5% binder, 2%–5% expanded graphite, and 5%–8% negative expansion material. Expanded graphite is used to construct a thermally conductive network, the binder to improve mechanical strength, and the negative expansion material is introduced to generate compressive prestress to counteract the hydrogen absorption and expansion of the alloy. While this approach addresses both thermal conductivity and pulverization resistance, its core mechanism relies on the compressive prestress of the negative expansion material. Negative expansion materials (such as ZrW2O8) are inherently expensive, and their compatibility with the hydrogen storage alloy remains to be verified. Furthermore, this approach does not incorporate metal fibers as a rigid framework and lacks ductile materials such as aluminum / copper powder as stress buffering media.
[0009] CN105731378A discloses an organic polymer / AB5 or AB2 composite hydrogen storage material and its preparation method, employing an organic solution mixing method, with a composite ratio of hydrogen storage alloy particles to organic polymer of 1:1 or 1:2. However, this method has an excessively high organic polymer content (33%~50%), which severely dilutes the hydrogen storage capacity of the hydrogen storage alloy.
[0010] Furthermore, CN119393671A discloses a hydrogen storage component and its preparation method, employing a structure with alternating support layers and hydrogen storage layers. The support layers are formed of fibers, while the hydrogen storage layers are formed of a mixture of hydrogen storage material and thermally conductive material. This scheme is a layered alternating structure rather than a three-dimensional network integrated structure. The fibers only serve as layered supports rather than a three-dimensional skeleton that runs through the entire material, thus its synergistic effect in resisting volume expansion is limited.
[0011] In summary, existing technologies have not yet achieved synergistic optimization of elastic buffering, rigid support, efficient heat conduction, and overall curing.
[0012] Therefore, developing a composite hydrogen storage material that can effectively suppress volume expansion while maintaining high thermal conductivity and structural stability has become a pressing technical challenge in the field of solid-state hydrogen storage technology. Summary of the Invention
[0013] To address the above technical problems, the purpose of this invention is to provide a composite hydrogen storage alloy particle. This composite hydrogen storage alloy particle introduces aluminum powder / copper powder as an elastic buffer and thermal conductive material, flake graphite / microcrystalline graphite / expanded graphite as a lubricating material, and metal fiber as a rigid skeleton material to construct a three-dimensional network structure with synergistic functions of "elastic buffer, rigid support, efficient thermal conductivity, and overall solidification". This effectively suppresses the volume expansion effect of the hydrogen storage alloy, prevents stress concentration caused by pulverization and deposition, and extends the service life of hydrogen storage cylinders or hydrogen storage devices.
[0014] To achieve the above objectives, the present invention adopts the following technical solution: A composite hydrogen storage alloy particle, based on a total weight of 100 parts, comprises the following components: The hydrogen storage alloy powder comprises 65-99.6 parts by weight, the thermally conductive material comprises 0.1-10 parts by weight, the lubricating material comprises 0.1-5 parts by weight, the fiber skeleton material comprises 0.1-10 parts by weight, and the binder comprises 0.1-10 parts by weight. The thermally conductive material is metal powder; The lubricating material is any one of flake graphite, microcrystalline graphite, or expanded graphite. The fiber skeleton material is a metal fiber material; The metal fiber material includes any one of stainless steel fiber material, copper fiber material, nickel fiber material or organic fiber material; The hydrogen storage alloy powder, thermally conductive material, lubricating material, and fiber skeleton material are bonded together by the binder to form an integral porous block with a three-dimensional network structure, namely, composite hydrogen storage alloy particles.
[0015] Preferably, the hydrogen storage alloy powder is at least one of AB5, AB2 or BCC type hydrogen storage alloys, with a particle size of 50-400 mesh.
[0016] Preferably, the thermally conductive material has a micron-sized spherical or sheet-like structure with a particle size of 10-200 μm; the metal powder includes aluminum powder or copper powder; and the thermally conductive material accounts for 1-10 wt% of the composite hydrogen storage alloy particles by mass. The lubricating material accounts for 1 to 5 wt% of the mass percentage in the composite hydrogen storage alloy particles.
[0017] Preferably, the fiber skeleton material accounts for 1-5 wt% of the composite hydrogen storage alloy particles by mass. The fiber skeleton material has a length of 0.5~10mm and a diameter of 10~500μm.
[0018] Preferably, the adhesive is a high-temperature resistant inorganic adhesive or a modified silicone adhesive; The binder accounts for 2-8 wt% of the mass in the composite hydrogen storage particles.
[0019] A composite hydrogen storage alloy bed is prepared from the aforementioned composite hydrogen storage alloy particles.
[0020] A method for preparing a composite hydrogen storage alloy bed includes the following steps: S1. Pretreatment: The fiber skeleton material is cleaned and degreased, and the thermally conductive material and lubricating material are dried respectively; S2. Dry mixing: The hydrogen storage alloy powder, pretreated thermal conductive material and lubricating material are put into a mixer and mixed at low speed under the protection of inert gas, so that the lubricating material is evenly coated on the surface of the hydrogen storage alloy particles. S3. Fiber dispersion: Gradually add the fiber skeleton material to the mixed powder obtained in step S2 and stir to make the fibers evenly distributed and form a preliminary network skeleton; S4. Wet mixing: Add binder and continue mixing until a homogeneous mixture is formed. The solid content of the mixture should be controlled at 65-99.6%. S5. Molding: Fill the mixture obtained in step S4 into a hydrogen storage container or mold, and pre-form it under pressure; S6. Curing: Place the molded body obtained in step S5 in a vacuum oven for curing treatment to cross-link and cure the adhesive, forming an integral porous block. S7. Activation treatment: After vacuuming and cooling, hydrogen gas is introduced for activation, and the product is obtained.
[0021] In step S2, the inert gas is nitrogen or argon; the mixture is slow-speed mixed at a rotation speed of 20-100 r / min for 10-60 min. In step S3, the fibers are uniformly distributed by high-speed dispersion at 100-500 r / min or mechanical stirring for 5-30 min. In step S5, a pressure of 5~50MPa is applied for preforming; In step S6, a curing process is carried out by vacuum insulation at 60~105℃ for 3~24h. In S7, a vacuum is drawn for 2 to 6 hours at a temperature of 80 to 150°C.
[0022] Among the above selections of inert gases, nitrogen can be used for general active alloys, while argon is used for high-activity alloys with a particle size of less than 50 micrometers to prevent oxidation during the mixing process.
[0023] Application of a composite hydrogen storage alloy particle in the preparation of a highly stable hydrogen storage material that suppresses volume expansion.
[0024] A hydrogen storage device includes a hydrogen storage container and composite hydrogen storage alloy particles filled in the hydrogen storage container, wherein the composite hydrogen storage alloy particles are the composite hydrogen storage particles described above. The hydrogen storage device is any one of a vehicle-mounted solid hydrogen storage system, a stationary solid hydrogen storage system, or a portable solid hydrogen storage device.
[0025] Compared with the prior art, the present invention has at least the following technical effects: This invention provides a composite hydrogen storage alloy particle. This composite hydrogen storage alloy particle introduces metal powders such as aluminum powder / copper powder as elastic buffer and thermal conductive materials, flake graphite / microcrystalline graphite / expanded graphite as lubricating materials, and metal fibers as rigid skeleton materials to construct a three-dimensional network structure with synergistic functions of "elastic buffer, rigid support, efficient thermal conductivity, and overall solidification". This effectively suppresses the volume expansion effect of the hydrogen storage alloy, prevents stress concentration caused by pulverization and deposition, and extends the service life of hydrogen storage cylinders or hydrogen storage devices.
[0026] The composite hydrogen storage alloy particles prepared by this method have a product that suppresses volume expansion. This is achieved through the synergistic effect of a triple mechanism: the constraint of the metal fiber skeleton, the plastic deformation buffer of aluminum / copper powder, and the lubrication and guiding of graphite. The macroscopic volume expansion rate of the composite hydrogen storage particles can be reduced to less than 10% (compared to 15-25% for traditional materials), which greatly reduces the design safety factor requirements of hydrogen storage containers.
[0027] The finished product has excellent anti-pulverization properties. After hydrogen absorption and desorption cycles, the material still maintains a bulk structure with no obvious powder generation, thus avoiding bed blockage and increased pressure drop.
[0028] The thermal conductivity of the finished particles is greatly improved, all based on the efficient thermal conduction pathway constructed by aluminum powder and metal fibers, which increases the equivalent thermal conductivity of the composite material by more than 10 times compared with pure alloy powder (from 0.34 W / (m·K) to more than 5 W / (m·K) in Example 1), and significantly accelerates the hydrogen absorption and desorption rate.
[0029] The finished particles can reach near-saturation hydrogen absorption within 4-5 minutes, while pure alloy powder requires 10 minutes, more than doubling the hydrogen absorption rate. Furthermore, the addition of thermally conductive, lubricating, and fiber-reinforced materials did not significantly affect the alloy's hydrogen storage capacity. The maximum hydrogen absorption capacities in Examples 1-3 reached 1.89 wt%, 1.75 wt%, and 2.1 wt%, respectively, comparable to pure alloy powder, and the capacity retention rate was over 98% after 10 cycles.
[0030] In summary, this invention is the first to integrate four mechanisms—elastic buffering (plastic deformation of aluminum / copper powder), rigid support (three-dimensional metal fiber skeleton), lubrication and sliding (interlayer slippage of graphite), and overall curing (binder)—into a single material system, resulting in a synergistic effect among them. The plastic deformation of aluminum / copper powder absorbs some of the expansion stress, the lubrication of graphite allows for the release of shear stress through minute relative displacements between particles, the metal fiber skeleton provides global constraint to prevent macroscopic expansion, and the binder cures all components into a unified whole to prevent localized loosening. This multi-scale stress management strategy of "microscopic buffering + mesoscopic lubrication + macroscopic constraint + overall curing" is the core innovation that distinguishes this invention from all existing technologies. Attached Figure Description
[0031] Figure 1 This is a schematic diagram of the microstructure of the composite hydrogen storage particles of the present invention; Figure 2 The hydrogen absorption curve of the hydrogen storage alloy bed in Example 1 during 10 cycles of experiment; Figure 3 The images show a comparison of the appearance of the hydrogen storage alloy bed in Example 1 and Comparative Example 1 before and after 10 hydrogen absorption and desorption cycles. Figure 4 This is a comparison chart of the thermal conductivity of the alloy bed in Example 1 and the pure alloy powder in Comparative Example 3; Figure 5 This is a comparison of the hydrogen absorption kinetics curves of the alloy bed in Example 1 and the pure alloy powder in Comparative Example 3. Detailed Implementation
[0032] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the present invention will be briefly introduced below in conjunction with the accompanying drawings and descriptions of the embodiments or the prior art. Obviously, the following description of the structure of the accompanying drawings is only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort. It should be noted that the description of these embodiments is for the purpose of helping to understand the present invention, but does not constitute a limitation of the present invention.
[0033] One specific embodiment of the present invention is as follows: A composite hydrogen storage alloy particle, based on a total weight of 100 parts, comprises the following components: The hydrogen storage alloy powder comprises 65-99.6 parts by weight, the thermally conductive material comprises 0.1-10 parts by weight, the lubricating material comprises 0.1-5 parts by weight, the fiber skeleton material comprises 0.1-10 parts by weight, and the binder comprises 0.1-10 parts by weight. The thermally conductive material is a metal powder such as aluminum powder or copper powder; The lubricating material is any one or more of flake graphite, microcrystalline graphite, or expanded graphite. The fiber skeleton material is a metal fiber material; The metal fiber material includes any one of stainless steel fiber material, copper fiber material, nickel fiber material or organic fiber material; The hydrogen storage alloy powder, thermally conductive material, lubricating material, and fiber skeleton material are bonded together by the binder to form an integral porous block with a three-dimensional network structure, namely, composite hydrogen storage alloy particles.
[0034] The hydrogen storage alloy powder is at least one of type AB5, AB2, or BCC hydrogen storage alloys, with a particle size of 50-400 mesh. Among them, type AB5 (containing LaNi) 5、 LaNi5Mm (Mm is a Ce-rich mixed rare earth alloy), AB2 type (TiMn2, ZrMn2, etc. alloys) or BCC type (V Ti Cr, Ti V Cr Mn and other alloys).
[0035] The thermally conductive material has a micron-sized spherical or sheet-like structure with a particle size of 10~200μm.
[0036] The thermally conductive material comprises 1-10 wt% of the composite hydrogen storage alloy particles by mass. The lubricating material comprises 1-5 wt% of the composite hydrogen storage alloy particles by mass. The fiber skeleton material comprises 1-5 wt% of the composite hydrogen storage alloy particles by mass; the length of the fiber skeleton material is 0.5-10 mm, and the diameter is 10-500 μm. The binder is a high-temperature resistant inorganic binder or modified silicone; the binder comprises 2-8 wt% of the composite hydrogen storage particles by mass.
[0037] A method for preparing a composite hydrogen storage alloy bed includes the following steps: (1) Pretreatment: clean and degrease the metal fibers; dry the aluminum powder and graphite.
[0038] (2) Dry mixing: Put 65~99.6 parts of hydrogen storage alloy powder, 0.1~10 parts of thermal conductive material and 0.1~5 parts of lubricating material into a mixer and mix at a low speed of 20~100r / min for 10~60min under inert gas protection to ensure that graphite is evenly coated on the surface of alloy particles.
[0039] (3) Fiber dispersion: 0.1 to 10 parts of fiber skeleton material are gradually added to the mixed powder obtained in step (2), and high-speed dispersion or mechanical stirring at 100 to 500 r / min is used for 5 to 30 min to make the fibers evenly distributed and form a preliminary network skeleton to avoid fiber agglomeration.
[0040] (4) Wet mixing: Add 0.1 to 10 parts of binder and continue mixing until a uniform mixture is formed. The solid content after mixing is controlled at 65 to 99.6%.
[0041] (5) Molding: Fill the mixture obtained in step (4) into a hydrogen storage container or mold and apply a pressure of 5~50MPa for pre-molding.
[0042] (6) Curing: Place the molded body obtained in step (5) in a vacuum oven and keep it at 60~105℃ for 3~24h to allow the adhesive to crosslink and cure, forming an integral porous block.
[0043] (7) Activation treatment: Vacuum at 80~150℃ for 2~6h, cool and then introduce hydrogen for initial activation to make the material achieve the best hydrogen absorption and desorption performance.
[0044] After the above-mentioned composite hydrogen storage alloy particles are prepared, they are used as hydrogen storage alloy beds. Their structure and shape remain stable after hydrogen absorption and desorption, reducing stress concentration caused by alloy powder accumulation due to pulverization after hydrogen absorption and desorption. The hydrogen storage alloy powder used in this scheme is a commercial hydrogen storage alloy (including AB5, AB2, or BCC type hydrogen storage alloys).
[0045] The particle size requirement for hydrogen storage alloy powder is 0.048mm~0.27mm (i.e. 50~300 mesh).
[0046] The performance testing methods for the following examples and comparative examples are as follows: Volume expansion rate test: The volume of the hydrogen storage alloy bed was measured after activation (initial state) and after each hydrogen absorption / desorption cycle (desorption state) using either the displacement method or the vernier caliper method. The volume expansion rate was calculated using the following formula: Volume expansion rate (%) = (Volume after cycle - Initial volume) / Initial volume × 100% Thermal conductivity test: The equivalent thermal conductivity of the composite hydrogen storage particle block was tested at room temperature using the laser flash method (LFA) or steady-state heat flow method. The sample size was a circular piece with a diameter of 12.7 mm and a thickness of 1-3 mm. Before the test, the sample was coated with a graphite coating on both sides to enhance light absorption.
[0047] Hydrogen absorption / desorption cycle test: The hydrogen storage alloy bed is placed in a high-pressure reaction vessel, and high-purity hydrogen gas at 3~5MPa is introduced at 10℃ to absorb hydrogen. After hydrogen absorption saturation, the temperature is raised to 50℃, and the valve is opened to release hydrogen to atmospheric pressure, completing one hydrogen absorption / desorption cycle. The amount of hydrogen absorbed (wt%) is recorded for each cycle, and the above operation is repeated for 10 cycles.
[0048] Hydrogen absorption kinetics test: At a constant temperature of 10℃ and a hydrogen pressure of 3MPa, the hydrogen absorption rate of the hydrogen storage alloy bed was recorded as a function of time until hydrogen absorption saturation.
[0049] Hydrogen storage capacity retention rate calculation: Hydrogen storage capacity retention rate (%) = (hydrogen absorption in the nth cycle / hydrogen absorption in the 1st cycle) × 100%.
[0050] Example 1: A composite hydrogen storage alloy particle is prepared by the following method: Raw material: AB2 (Ti) with a particle size of 200 mesh 27 Mn 35 Cr 27 The Zr8Mm3 (Mm represents other Ce-rich rare earth elements) hydrogen storage alloy comprises 92 parts by weight, 3 parts by weight of binder, 2 parts by weight of flake graphite, 2 parts by weight of stainless steel fiber (3 mm in length and 50 μm in diameter), and 1 part by weight of aluminum powder.
[0051] Preparation method: Stepwise mixing: First, hydrogen storage alloy powder, flake graphite, stainless steel fiber, and aluminum powder are placed in a mixer and dry-mixed with nitrogen gas (60 r / min, 30 min). After mixing, a binder (potassium silicate) is added to ensure that all components are mixed evenly to obtain an alloy powder mixture. The powder mixture is then filled into a mold with a diameter of 60 mm and an inner diameter of 15 mm. It is then cold-pressed using a press (pressure 20 MPa) to form a mold (diameter 60 mm, inner diameter 15 mm, height 25 mm). Finally, it is dried in a vacuum oven at 105 °C for 5 h to obtain a composite hydrogen storage alloy bed.
[0052] like Figure 1 The diagram shown is a schematic diagram of the microstructure of the composite hydrogen storage particles prepared in Example 1.
[0053] Example 2: A composite hydrogen storage alloy particle is prepared by the following method: The mass fraction of AB5 type (LaNi5) hydrogen storage alloy with a particle size of 300 mesh is 85 parts, binder (potassium silicate) 5 parts, expanded graphite 3 parts, copper fiber (length 3mm, diameter 50μm) 4 parts, and copper powder 3 parts.
[0054] Stepwise mixing: First, place the alloy, expanded graphite, copper fiber, and copper powder in a mixer and dry mix them with nitrogen (50 r / min for 40 min). After mixing, add the binder to ensure that all components are mixed evenly to obtain an alloy powder mixture. Fill the powder mixture into a mold with a diameter of 60 mm and an inner diameter of 15 mm. Then, use a press to cold press the mixture (pressure 25 MPa) to form it (diameter 60 mm, inner diameter 15 mm, height 25 mm). Finally, place it in a vacuum oven and dry it at 80°C for 10 h to obtain the hydrogen storage alloy bed.
[0055] The hydrogen storage alloy bed prepared in this embodiment was tested according to the above performance test method. After 10 hydrogen absorption and desorption cycles, the volume expansion rate was 8%, the thermal conductivity was 4.8 W / (m·K), the maximum hydrogen absorption capacity was 1.75 wt%, the capacity retention rate was 97.7%, and the hydrogen absorption saturation time was 4 minutes.
[0056] Example 3: A composite hydrogen storage alloy particle is prepared by the following method: BCC (V) with a particle size of 100 mesh 75 Ti 11.5 Cr 11.5 The Fe2) type hydrogen storage alloy has 78 parts by weight, 8 parts by weight of binder (potassium silicate), 4 parts by weight of flake graphite, 5 parts by weight of nickel fiber (5 mm in length and 80 μm in diameter), and 5 parts by weight of aluminum powder.
[0057] Stepwise mixing: First, the alloy, flake graphite, nickel fiber, and aluminum powder are placed in a mixer and dry-mixed with nitrogen gas (40 r / min, 50 min). After mixing, the binder is added to ensure that all components are mixed evenly to obtain an alloy powder mixture. The powder mixture is then filled into a mold with a diameter of 60 mm and an inner diameter of 15 mm. It is then cold-pressed using a press (pressure 30 MPa) to form a mold (diameter 60 mm, inner diameter 15 mm, height 25 mm). Finally, it is placed in a vacuum oven and dried at 95 °C for 8 h to obtain a hydrogen storage alloy bed.
[0058] The hydrogen storage alloy bed prepared in this embodiment was tested according to the above performance test method. After 10 hydrogen absorption and desorption cycles, the volume expansion rate was 7%, the thermal conductivity was 5.2 W / (m·K), the maximum hydrogen absorption capacity was 2.1 wt%, the capacity retention rate was 98.6%, and the hydrogen absorption saturation time was 4 minutes.
[0059] Comparative Example 1: Contains only binder, excluding fibers, graphite, and aluminum powder. AB2 type (Ti) with a particle size of 200 mesh 27 Mn 35 Cr 27The Zr8Mm3 hydrogen storage alloy (Mm is other Ce-rich rare earth elements) has 96 parts by mass and 4 parts by mass of binder.
[0060] Stepwise mixing: First, the alloy and binder are mixed evenly to obtain an alloy powder mixture. The mixture is then filled into a mold with a diameter of 60 mm and an inner diameter of 15 mm, and cold-pressed using a press (pressure 20 MPa) to form a hydrogen storage alloy bed (diameter 60 mm, inner diameter 15 mm, height 25 mm). The hydrogen storage alloy bed is then placed in a vacuum oven for drying at 105℃ for 5 hours. After drying, the hydrogen storage alloy bed is obtained and placed in a reaction vessel for hydrogen absorption and desorption cycle testing.
[0061] Tests showed that Comparative Example 1 exhibited a volume expansion rate of 22% and a thermal conductivity of 0.5 W / (m·K) after 10 hydrogen adsorption / desorption cycles. The bed also showed severe cracking and significant pulverization (e.g., ...). Figure 3 (As shown on the right).
[0062] Comparative Example 2: Contains binder and graphite, but contains no fiber or aluminum powder. AB2 type (Ti) with a particle size of 200 mesh 27 Mn 35 Cr 27 The Zr8Mm3 hydrogen storage alloy (Mm is other Ce-rich rare earth elements) has 93 parts by mass, 4 parts by binder, and 3 parts by flake graphite.
[0063] Stepwise mixing: First, the alloy, graphite and binder are mixed evenly to obtain an alloy powder mixture; the mixture is filled into a mold with a diameter of 60 mm and an inner diameter of 15 mm, and formed by cold pressing (pressure 20 MPa) to form a diameter of 60 mm, an inner diameter of 15 mm and a height of 25 mm. Then, it is placed in a vacuum oven and dried at 105 °C for 5 hours to obtain a hydrogen storage alloy bed. The hydrogen storage alloy bed is placed in a reaction vessel to conduct hydrogen absorption and desorption cycle test experiments.
[0064] Tests showed that Comparative Example 2 had a volume expansion rate of 18% and a thermal conductivity of 1.2 W / (m·K) after 10 hydrogen absorption and desorption cycles, and the bed showed obvious cracks and partial pulverization.
[0065] Comparative Example 3: Pure alloy powder Weigh out 200 mesh AB2 type (Ti) 27 Mn 35 Cr 27 400g of Zr8Mm3 (Mm represents other Ce-rich rare earth elements) hydrogen storage alloy powder was used, and the thermal conductivity of the alloy powder was tested. A portion of the alloy powder was then activated, and hydrogen absorption and desorption kinetics tests were performed using the same procedure as in Example 1.
[0066] The thermal conductivity of Comparative Example 3 was 0.34 W / (m·K), the hydrogen absorption saturation time was 10 minutes, and the maximum hydrogen absorption capacity was 1.90 wt%.
[0067] The performance test results are summarized and compared in Table 1 below: Table 1
[0068] Results analysis: Analysis based on Table 1: The results of the volume expansion rate variation show that Examples 1-3 all exhibit excellent anti-expansion performance. Compared with Comparative Example 1 (containing only binder), the volume expansion rate of Example 1 after 10 cycles decreased from 22% to 9%, a reduction of 59%; compared with Comparative Example 2 (containing binder and graphite), the volume expansion rate of Example 1 after 10 cycles decreased from 18% to 9%, a reduction of 50%. This indicates that although the lubricating effect of graphite has a certain effect, the optimal anti-expansion effect can only be achieved when the rigid skeleton constraint of metal fibers and the plastic deformation buffer of aluminum / copper powder are introduced simultaneously. All three mechanisms are indispensable and have a significant synergistic effect.
[0069] The thermal conductivity test results show that the thermal conductivity of Example 1 (>5W / (m·K)) is about 14.7 times higher than that of the pure alloy powder of Comparative Example 3 (0.34W / (m·K)) and also significantly higher than that of Comparative Example 2 (1.2W / (m·K)). This indicates that the efficient thermal conduction pathway constructed by aluminum powder and metal fibers is significantly better than the thermal conductivity improvement by graphite alone.
[0070] The hydrogen absorption kinetics test results showed that the hydrogen absorption saturation time (5 min) of Example 1 was reduced by half compared with that of Comparative Example 3 (10 min), indicating that the improvement in thermal conductivity directly promoted the hydrogen absorption and desorption reaction rate.
[0071] All embodiments exhibited a capacity retention rate exceeding 97% after 10 cycles, demonstrating the superior performance of the present invention in suppressing pulverization and maintaining hydrogen storage capacity.
[0072] In summary, this invention achieves a significant reduction in volume expansion rate, a significant improvement in thermal conductivity, and an effective guarantee of cycle stability through a four-fold synergistic mechanism of "elastic buffering of aluminum / copper powder + lubrication and guiding of graphite + rigid skeleton of metal fiber + overall curing of binder". The technical effect is significantly better than that of the comparative examples, proving the advanced nature and practicality of the technical solution of this invention.
[0073] Analysis based on the attached diagram: Performance Test 1: The hydrogen storage alloy bed was subjected to hydrogen absorption at 10℃ and hydrogen release at 50℃, and the amount of hydrogen absorbed was recorded each time.
[0074] like Figure 2The figure shows the hydrogen absorption curve of the hydrogen storage alloy bed in Example 1 during 10 cycles of experiment.
[0075] Combination Figure 2 It can be seen that after 10 hydrogen absorption and desorption cycles, the hydrogen absorption and desorption capacity of the hydrogen storage alloy bed remains basically stable (capacity retention rate of 98.4%).
[0076] like Figure 3 The image shown is a comparison of the appearance of the hydrogen storage alloy bed in Example 1 and Comparative Example 1 before and after 10 hydrogen absorption and desorption cycles.
[0077] Combination Figure 3 It can be seen that after 10 cycles of hydrogen absorption and desorption, the hydrogen storage alloy bed was taken out and compared with the photos of the bed after 10 cycles of hydrogen absorption and desorption. It was found that the alloy bed did not change significantly after 10 cycles, with only a small amount of loose powder appearing at the edge.
[0078] Volume expansion rate test results: 3% after 1 cycle, 8% after 5 cycles, and 9% after 10 cycles.
[0079] Performance Test 2: The thermal conductivity of the prepared hydrogen storage alloy bed was tested.
[0080] like Figure 4 The figure shown is a comparison of the thermal conductivity of the alloy bed in Example 1 and the pure alloy powder in Comparative Example 3.
[0081] Test results are as follows Figure 4 The results show that the thermal conductivity of the hydrogen storage alloy bed prepared in Example 1 is significantly improved compared with that of the pure alloy powder in Comparative Example 3, with the thermal conductivity increasing from 0.34 W / (m·K) to over 5 W / (m·K).
[0082] Performance Test 3: The hydrogen storage alloy bed material was subjected to hydrogen absorption and desorption performance tests. The prepared hydrogen storage alloy bed was placed in a reaction vessel, vacuumed at 80°C for 3 hours, and then cooled to 10°C to complete activation.
[0083] like Figure 5 The figure shown is a comparison of the hydrogen absorption kinetics curves of the hydrogen storage alloy bed prepared in Example 1 and the pure alloy powder in Comparative Example 3.
[0084] Depend on Figure 5 It can be seen that the maximum hydrogen absorption capacity of the alloy in the hydrogen storage alloy bed is 1.89 wt%, which is comparable to the hydrogen absorption capacity of the pure alloy powder in Comparative Example 3 (1.90 wt%). The results show that the added material did not have a significant impact on the hydrogen storage capacity of the alloy. The hydrogen storage alloy bed can approach the saturation state of hydrogen absorption in 5 minutes, while Comparative Example 3 requires 10 minutes to reach the saturation state. The hydrogen storage alloy bed has a superior hydrogen absorption kinetic performance.
[0085] Finally, it should be noted that the above description is merely a preferred embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A composite hydrogen storage alloy particle, characterized in that, Based on a total weight of 100 parts, it includes the following components: The hydrogen storage alloy powder comprises 65-99.6 parts by weight, the thermally conductive material comprises 0.1-10 parts by weight, the lubricating material comprises 0.1-5 parts by weight, the fiber skeleton material comprises 0.1-10 parts by weight, and the binder comprises 0.1-10 parts by weight. The thermally conductive material is metal powder; The lubricating material is any one of flake graphite, microcrystalline graphite, or expanded graphite. The fiber skeleton material is a metal fiber material; The metal fiber material includes any one of stainless steel fiber material, copper fiber material, nickel fiber material or organic fiber material; The hydrogen storage alloy powder, thermally conductive material, lubricating material, and fiber skeleton material are bonded together by the binder to form an integral porous block with a three-dimensional network structure, namely, composite hydrogen storage alloy particles.
2. The composite hydrogen storage alloy particles according to claim 1, characterized in that, The hydrogen storage alloy powder is at least one of AB5, AB2 or BCC type hydrogen storage alloys, with a particle size of 50-400 mesh.
3. The composite hydrogen storage alloy particles according to claim 1, characterized in that, The thermally conductive material has a micron-sized spherical or sheet-like structure with a particle size of 10~200μm; The metal powder includes aluminum powder or copper powder; The thermally conductive material accounts for 1-10 wt% of the mass percentage in the composite hydrogen storage alloy particles; The lubricating material accounts for 1 to 5 wt% of the mass percentage in the composite hydrogen storage alloy particles.
4. The composite hydrogen storage alloy particles according to claim 1, characterized in that, The fiber skeleton material accounts for 1-5 wt% of the mass percentage in the composite hydrogen storage alloy particles; The fiber skeleton material has a length of 0.5~10mm and a diameter of 10~500μm.
5. The composite hydrogen storage alloy particles according to claim 1, characterized in that, The adhesive is a high-temperature resistant inorganic adhesive or a modified organic silicone adhesive; The binder accounts for 2-8 wt% of the mass in the composite hydrogen storage particles.
6. A composite hydrogen storage alloy bed, characterized in that, It is prepared from the composite hydrogen storage alloy particles as described in any one of claims 1 to 5.
7. A method for preparing a composite hydrogen storage alloy bed as described in claim 6, characterized in that, Includes the following steps: S1. Pretreatment: The fiber skeleton material is cleaned and degreased, and the thermally conductive material and lubricating material are dried respectively; S2. Dry mixing: The hydrogen storage alloy powder, pretreated thermal conductive material and lubricating material are put into a mixer and mixed at low speed under the protection of inert gas, so that the lubricating material is evenly coated on the surface of the hydrogen storage alloy particles. S3. Fiber dispersion: Gradually add the fiber skeleton material to the mixed powder obtained in step S2 and stir to make the fibers evenly distributed and form a preliminary network skeleton; S4. Wet mixing: Add binder and continue mixing until a homogeneous mixture is formed. The solid content of the mixture should be controlled at 65-99.6%. S5. Molding: Fill the mixture obtained in step S4 into a hydrogen storage container or mold, and pre-form it under pressure; S6. Curing: Place the molded body obtained in step S5 in a vacuum oven for curing treatment to cross-link and cure the adhesive, forming an integral porous block. S7. Activation treatment: After vacuuming and cooling, hydrogen gas is introduced for activation, and the product is obtained.
8. The preparation method according to claim 7, characterized in that, In step S2, the inert gas is nitrogen or argon; the mixture is slow-speed mixed at a rotation speed of 20-100 r / min for 10-60 min. In step S3, the fibers are uniformly distributed by high-speed dispersion at 100-500 r / min or mechanical stirring for 5-30 min. In step S5, a pressure of 5~50MPa is applied for preforming; In step S6, a curing process is carried out by vacuum insulation at 60~105℃ for 3~24h. In S7, a vacuum is drawn for 2 to 6 hours at a temperature of 80 to 150°C.
9. The application of the composite hydrogen storage alloy particles as described in any one of claims 1 to 5 in the preparation of highly stable hydrogen storage materials that suppress volume expansion.
10. A hydrogen storage device, characterized in that, The invention includes a hydrogen storage container and composite hydrogen storage alloy particles filled in the hydrogen storage container, wherein the composite hydrogen storage alloy particles are the composite hydrogen storage particles according to any one of claims 1 to 5. The hydrogen storage device is any one of a vehicle-mounted solid hydrogen storage system, a stationary solid hydrogen storage system, or a portable solid hydrogen storage device.
Citation Information
Patent Citations
Organic polymer / AB5 or AB2 composite hydrogen storage material and preparation method thereof
CN105731378A
Magnesium-based hydrogen storage alloy block and preparation method thereof
CN114507798A
Anti-pulverization composite hydrogen storage particle and preparation method thereof
CN121516815A
Sodium-ion battery hard carbon negative electrode material, preparation method thereof and sodium-ion battery
CN121516851A
Composite hydrogen storage briquette with high thermal conductivity and cracking and pulverization resistance and preparation method of composite hydrogen storage briquette