A nano-NbF5-catalyzed Mg-RE(Y,Pr)-based Mg 24 Y5 type composite hydrogen storage material and its preparation method
By adding rare earth elements Y and Pr and transition metals Ni, Zr, Mn, and Zn to magnesium-based alloys, and using nano-NbF5 catalysts and rapid quenching ball milling processes, a nanocrystalline Mg-RE(Y, Pr)-based Mg24Y5 composite hydrogen storage material was prepared. This solved the problems of high thermal stability and poor hydrogen absorption and desorption performance of magnesium-based alloys, achieving high efficiency in hydrogen absorption and desorption and a simplified preparation process.
Patent Information
- Application Number
- CN202611526246.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-29
- Publication Date
- 2026-11-17
AI Technical Summary
Existing magnesium-based alloy hydrides have high thermal stability, poor thermodynamic and kinetic properties of hydrogen absorption and desorption, and low efficiency in mass production.
By adding multiple rare earth elements Y and Pr, as well as transition metal elements Ni, Zr, Mn and Zn, combined with vacuum rapid quenching and nano NbF5 catalyst, a Mg-RE(Y, Pr)-based Mg24Y5 type composite hydrogen storage material with nanocrystalline structure was prepared, and its hydrogen absorption and desorption performance was improved by mechanical ball milling process.
It significantly improves the hydrogen absorption and desorption kinetics and thermodynamic stability of hydrogen storage materials, reduces the hydrogen desorption temperature, simplifies the activation process, and is suitable for large-scale preparation.
Smart Images

Figure CN123105547A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of solid-state hydrogen storage materials technology, and in particular provides a Mg-RE(Y,Pr)-based Mg catalyst catalyzed by nano-NbF5. 24 Y5 type composite hydrogen storage material and its preparation method. Background Technology
[0002] Hydrogen energy is considered an ideal alternative to traditional fossil fuels. As a clean energy source, hydrogen energy has many advantages: 1) Vast and diversified hydrogen reserves. Hydrogen is the most abundant element on Earth, and its development and utilization are highly sustainable. Unlike fossil fuels, hydrogen is a renewable energy source and can be produced through renewable energy technologies such as water electrolysis, thus achieving sustainable utilization. 2) Compared to traditional fuels, hydrogen has a higher calorific value (1.43 × 10⁻⁶). 8 (J / kg). Compared to gasoline, ethanol, and metallurgical coke, hydrogen energy is 300%, 390%, and 450% higher, respectively, making it a high-energy-density and highly efficient energy source. 3) Most importantly, as a representative of clean energy, the main product of hydrogen combustion is pure water, completely avoiding the emissions of toxic and harmful substances such as carbon monoxide, incompletely combusted hydrocarbons, and heavy metal residues found in traditional fuels. Therefore, the development and application of hydrogen energy is considered the most direct and effective strategy for achieving the "dual-carbon goal."
[0003] The application of hydrogen energy involves multiple stages, including: efficient and inexpensive hydrogen production, efficient and safe hydrogen storage and transportation, and rapid refueling and safe use of hydrogen. While hydrogen production has mature and practical solutions, efficient and safe hydrogen storage lacks a satisfactory solution and remains the main technological bottleneck hindering the large-scale application of hydrogen energy. Currently, the main methods of hydrogen storage include high-pressure gaseous hydrogen storage, cryogenic liquid hydrogen storage, and metal hydride solid-state hydrogen storage. High-pressure gaseous hydrogen storage technology involves pressurizing hydrogen to 35–70 MPa and storing it in a pressure-resistant container. Its main advantages are high storage capacity and efficiency. However, it faces challenges such as high container manufacturing costs, high energy consumption, and safety risks. Cryogenic liquid hydrogen storage involves cryogenically cooling hydrogen to -252°C to liquefy it, significantly increasing the hydrogen density per unit volume. This method is suitable for large-scale and long-distance transportation, offering advantages such as high purity and compact container structure. It should be noted that this method has extremely high energy consumption, expensive container manufacturing costs, and requires very good thermal insulation performance. Solid-state hydrogen storage technology is widely recognized as the most promising hydrogen storage method due to its excellent safety performance, high volumetric hydrogen storage density, and low operating pressure. Hydrogen storage alloys adsorb hydrogen through a mechanism that involves the reaction of hydrogen with a metal to form metal hydrides. The principle is that when hydrogen interacts with the alloy, hydrogen molecules are broken down into hydrogen atoms under the catalysis of the metal. These hydrogen atoms then diffuse through interstitial spaces into the interstitial spaces of the crystal lattice and bond with the metal, forming a metal compound with a specific structure through an exothermic reaction. This reaction is reversible: the forward reaction involves the metal absorbing hydrogen and releasing heat; the reverse reaction involves the decomposition of the metal hydride, releasing hydrogen and absorbing heat. By adjusting conditions such as temperature and pressure, the forward and reverse reactions can be repeatedly driven, enabling the material to adsorb and desorb hydrogen.
[0004] Hydrogen storage alloys are generally categorized as A x B yIn hydrogen storage alloys, type A elements typically have a strong affinity for hydrogen, meaning they readily form hydrides and provide the majority of the hydrogen storage capacity. During hydrogen absorption, they preferentially combine with hydrogen to form stable hydrides. Type B elements have a relatively weaker affinity for hydrogen and primarily weaken the AH bond strength by controlling the alloy's electronic structure, lattice constant, and phase stability. This reduces hydride stability and improves the reversibility and kinetics of hydrogen desorption. Both types work synergistically to achieve a balance between hydrogen storage capacity and reversible hydrogen desorption performance. Among the many discovered hydrogen storage alloys, Mg-based alloys possess advantages such as high hydrogen storage density (7.6% MgH2), low cost, and abundant resources, making them promising candidates for widespread application in hydrogen storage technology. However, the slow hydrogen absorption / desorption kinetics and high absorption / desorption temperatures of magnesium-based alloys hinder their practical application. To overcome these drawbacks, researchers have employed various methods and strategies, including element addition or substitution, reducing particle and grain size, doping with catalytic additives, and combining with other materials. Alloying with transition elements is an effective method to improve the hydrogen storage performance of Mg-based alloys. Studies have found that the hydrogen absorption enthalpies of Mg-In and Mg-In-Y alloys are 68.1 and 62.9 kJ / mol H2, respectively. Alloying Mg with Ni can also significantly improve the thermodynamic and kinetic properties of dehydrogenation. For example, Mg2Ni alloys can reversibly absorb and dehydrogenate hydrogen at 250 °C, and their hydrogenation / dehydrogenation kinetics are significantly faster than those of pure Mg alloys. Alloying Mg with rare earth elements (REs) has also been found to be a promising approach. Numerous studies have shown that adding appropriate amounts of rare earth elements significantly reduces the desorption temperature of Mg-RE alloys and greatly increases the dehydrogenation rate. Some researchers have reported that Mg-RE alloys irreversibly convert to MgH2 and REH during the first hydrogen absorption process. 2-3 The formation of RE hydrides reduces the hydrogen absorption capacity, but it has a good catalytic effect on the hydrogen absorption and desorption reactions of the Mg-MgH2 system. In addition, the addition of rare earth elements significantly changes the microstructure of the alloy, thereby promoting the hydrogen absorption and desorption kinetics.
[0005] Compared to other rare earth elements, Y has a smaller relative atomic mass. This means that, with the same Mg / RE atomic ratio, Mg-Y alloys have a higher hydrogen absorption capacity than Mg-RE (RE = La, Ce, Pr, Nd, and Sm) alloys. Studies have investigated the hydrogen storage performance of Mg3Y alloys, showing a hydrogen absorption capacity exceeding 4.0 wt.%, higher than Mg3La. Compared to industrial MgH2, Mg... 24The hydrogen desorption kinetics of Y5 alloys are also significantly improved. The addition of Y improves the hydrogen absorption and desorption kinetics of Mg and its alloys, mainly due to the catalytic effect of the YH2 / YH3 phase and the change in microstructure. Furthermore, the combination of rare earth Y and transition metal elements with Mg has been widely reported, such as Mg-Zn-Y, Mg-In-Y, Mg-Y-Ti, Mg-Y-Fe, Mg-Cu-Y, Mg-Y-Ni, and Mg-Cu-Ni-Y alloys. Studies have found that these additives can improve kinetics, lower activation energy, reduce hydrogen desorption temperature, and increase hydrogen absorption / desorption rates. Therefore, it is certain that Y-doped Mg-based alloys have better hydrogen storage performance than pure Mg / MgH2.
[0006] This invention reduces the thermal stability of Mg-based hydrides and improves their hydrogen absorption and desorption kinetics by adding multiple rare earth elements Y and Pr, as well as transition metal elements Ni, Zr, Mn, and Zn. A precursor alloy with a nanocrystalline structure is obtained through vacuum rapid quenching. Based on this, a small amount of catalyst NbF5 is added, followed by mechanical ball milling for an appropriate time to obtain a nanocrystalline microstructure and form a highly active surface on the alloy particles, significantly improving the hydrogen storage performance of the patented alloy. On the one hand, the addition of metal elements Ni, Zr, Mn, and Zn promotes hydrogen dissociation and reduces the bonding strength of Mg-H bonds; on the other hand, the catalyst NbF5 not only improves ball milling efficiency but also promotes the introduction of high-density crystal defects and improves the surface activity of the ball-milled particles. The particle and grain refinement caused by ball milling greatly shortens the diffusion distance of hydrogen atoms, thereby significantly increasing the hydrogen absorption and desorption rate. Summary of the Invention
[0007] Based on the above analysis, the embodiments of the present invention aim to provide a Mg-RE(Y,Pr)-based Mg catalyst catalyzed by nano-NbF5. 24 Y5 type composite hydrogen storage material and its preparation method are intended to solve at least one of the following problems of existing magnesium-based alloy hydrides: high thermal stability, poor thermodynamic and kinetic properties of hydrogen absorption and desorption, and low efficiency of batch preparation.
[0008] On one hand, embodiments of the present invention provide a Mg-RE(Y,Pr)-based Mg catalyst catalyzed by nano-NbF5. 24 Y5-type composite hydrogen storage material is characterized by containing multiple rare earth elements Y and Pr, as well as metallic elements Zr, Ni, Mn, and Zn, and adding the catalyst NbF5. Its composition is: Mg 48 Y 11-x Pr x Ni 3-y-z-m Zr y Mn z Zn m+ n wt.% NbF5, where x, y, z, m are atomic ratios, 0<x≤3, 0<y≤1, 0<z≤1, 0<m≤0.5, n is the percentage of NbF5 in the master alloy, and 4≤n≤10.
[0009] Preferably, x:y:z:m=1:0.3:0.6:0.2, and n=6.
[0010] In another aspect, the embodiments of the present invention further provide a nano NbF5 catalyzed Mg-RE(Y, Pr)-based Mg 24 Y5 type composite hydrogen storage material preparation method, which is used for preparing the composite hydrogen storage material, and the steps are as follows: S1: Batching is carried out according to the preset chemical formula composition, wherein a certain proportion of burning loss is added during the weighing of Mg and rare earth elements Y and Pr. S2: Alloy smelting is carried out in a vacuum smelting furnace, the prepared raw materials are sequentially placed in a magnesia crucible, the furnace cover is closed, vacuum pumping is performed to reach a preset vacuum degree, then high-purity helium gas or a helium-argon mixed gas with a volume ratio of 1:1 is charged as a protective gas, the raw materials are melted by arc smelting, induction heating smelting or other heating methods, after holding for a period of time, the alloy is poured into a copper mold to obtain a cylindrical master alloy ingot. S3: The melt-spinning treatment is carried out in a vacuum melt-spinning furnace, the master alloy ingot prepared in step S2 is placed in a quartz tube with a slit at the bottom, and induction heating is performed until the ingot is completely melted. Under the action of protective gas pressure, the liquid alloy is ejected from the slit at the bottom of the quartz tube onto the surface of a rotating water-cooled copper roller, so as to obtain an alloy ribbon with uniform thickness. In the metallurgical industry, this treatment process is called rapid solidification or melt-spinning, and the surface linear velocity of the rotating copper roller is called the spinning speed. This method can realize rapid solidification of liquid metal or alloy, so that the alloy obtains an ultra-fine microstructure.
[0011] S4: The melt-spun alloy ribbon is mechanically crushed and sieved to obtain alloy powder, the sieved alloy powder, a certain amount of nano NbF5 catalyst and stainless steel grinding balls are loaded together into a stainless steel ball milling tank, the tank is evacuated and then filled with high-purity argon, and ball milling is carried out in an omnidirectional planetary high-energy ball mill to obtain ball-milled powder, that is, the composite hydrogen storage material.
[0012] Specifically, the mass percentage of the burning loss of Mg and rare earth elements Y and Pr in S1 is 5% to 10%.
[0013] Specifically, the specific process and parameters in S2 are: evacuate to 1×10 -2 ~5×10 -5 Pa, introduce high-purity helium gas or a helium-argon mixed gas with a volume ratio of 1:1 at 0.01~0.1MPa as the protective gas, and heat to 1300~1400℃.
[0014] Specifically, the nozzle slit width at the bottom of the quartz tube in S3 is 0.3±0.005mm, and the linear speed of the water-cooled copper roller is 3~20m / s.
[0015] Specifically, the rapid quenching alloy strip described in S3 has a thickness between 100 and 350 μm and a width of 2 to 30 mm (the width depends on the length of the nozzle slit). The rapid quenching alloy strip has a nanocrystalline structure with a grain size of 30 to 150 nm.
[0016] Specifically, in step S4, the ball milling process is as follows: after evacuating the ball mill jar, high-purity argon gas is introduced, and the ball mill is carried out in an all-around planetary high-energy ball mill for 3 to 8 hours, preferably 4 hours, with a ball-to-material ratio of 20:1 and a rotation speed of 250 rpm; during the ball milling process, the ball mill is stopped for 0.5 hours every hour of operation to prevent the temperature of the ball mill jar and abrasive from becoming too high.
[0017] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects: The composite hydrogen storage material disclosed in this invention has high hydrogen storage capacity, excellent hydrogen absorption and desorption kinetics, and hydrogen absorption and desorption cycle stability. This result is achieved through a perfect combination of scientific component design and preparation process.
[0018] (i) In terms of the composition design of the master alloy, trace amounts of multi-element rare earth elements Y and Pr are added, along with small amounts of metallic elements Zr, Ni, Mn, and Zn for alloying, which reduces the stability of Mg-based hydrides and improves their hydrogen absorption and desorption kinetics. Mg and Y can form the main phase Mg of the alloy. 24 Y5, Mg can form PrMg with Pr. 12 In Mg-based alloys, various intermetallic compounds can be formed, such as Mg₂Ni with Ni, ZrMn₂ with Zr, and MgZn₂ with Zn. Some of these intermetallic compounds are hydrogen-absorbing phases themselves, while others, although not hydrogen-absorbing, play a positive role in the hydrogen absorption and desorption processes of Mg-based alloys. Simultaneously, rare earth elements Y and Pr can form YH₃ and PrH₃ with hydrogen. These hydrides are dispersed in the alloy matrix and can serve as nuclei for heterogeneous nucleation of magnesium hydrides, exhibiting a significant catalytic effect on the hydrogen absorption and desorption processes of Mg-based alloys.
[0019] (ii) In terms of the preparation process, a master alloy ingot is first obtained by vacuum melting, and then rapidly quenched after secondary remelting to obtain an alloy ribbon with a nanocrystalline structure. The numerous grain boundaries provide excellent channels for hydrogen atom diffusion, while the rapid quenching generates various crystal defects and strain energies within the alloy that facilitate hydrogen diffusion, further improving the alloy's hydrogen absorption and desorption kinetics. The nanocrystalline structure produced by rapid quenching facilitates subsequent mechanical crushing and makes the preparation of alloy powder easier.
[0020] (iii) This invention employs a mechanical method to pulverize rapidly quenched alloy sheets, adding a small amount of NbF5 catalyst and subjecting them to short-term mechanical ball milling. While maintaining the nanocrystalline structure of the rapidly quenched alloy, it promotes the introduction of high-density crystal defects and improves the surface activity of the ball-milled particles, thereby enhancing the hydrogen storage and activation performance of the magnesium-based alloy. The hydrogen absorption process requires almost no incubation period. After ball milling, the NbF5 nanocatalyst and the matrix alloy particles form a large number of highly active phase interfaces, further improving the thermodynamics and kinetics of hydrogen absorption and desorption in the composite material.
[0021] On the one hand, the catalytic effect of NbF5 lies in its very low hardness, making it extremely easy to break under external force. During ball milling, it has a significant lubricating effect on the alloy particles, preventing the matrix material from adhering to the milling jar wall, improving milling efficiency, and resulting in finer, less aggregated alloy particles. On the other hand, nano-NbF5 ultrafine particles can be uniformly distributed among magnesium-based alloy particles, forming numerous active interfaces between the matrix alloy and the catalyst. These interfaces provide excellent nucleation sites for the formation and decomposition of hydrides.
[0022] (iv) By adding nano-NbF5 catalyst and selecting appropriate ball milling time, the present invention obtains ball milling material particles that are approximately spherical. Short ball milling time ensures that there are no excessive amorphous phases in the ball milling material and ensures that the powder dispersion of the ball milling material is good without serious agglomeration or even welding, thereby ensuring that the activation performance, hydrogen absorption capacity and kinetics of the material are significantly improved.
[0023] (v) The composite hydrogen storage material disclosed in this invention has good hydrogen absorption and desorption kinetics and thermodynamic properties. Compared with existing magnesium-based hydrogen storage materials, its thermodynamic stability is significantly reduced (i.e., excellent hydrogen desorption kinetics) and its hydrogen desorption temperature is reduced (i.e., it has better hydrogen absorption and desorption performance at the same temperature, especially hydrogen desorption performance). Moreover, the fully activated composite hydrogen storage material can be obtained without a complicated activation process.
[0024] (vi) The preparation process and equipment / instruments of the composite hydrogen storage material of the present invention all adopt the current mature operation and equipment, which are easy to realize the process, and the various raw materials are easy to purchase, making them suitable for large-scale preparation and wide-ranging application.
[0025] In this invention, the above-described technical solutions can be combined with each other to achieve more preferred combinations. Other features and advantages of this invention will be set forth in the following description, and some advantages may become apparent from the description or be learned by practicing the invention. The objects and other advantages of this invention can be realized and obtained from what is particularly pointed out in the description and drawings. Attached Figure Description
[0026] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0027] Figure 1 The diagrams show the phases of binary alloy systems with different compositions. They are mainly used for the auxiliary design and analysis of alloy composition and phase composition. In the diagram, (a) Mg-Y; (b) Mg-Pr; (c) Mg-Ni; (d) Mg-Zr; (e) Zr-Mn; and (f) Mg-Zn.
[0028] Figure 2 These are medium-frequency vacuum induction melting furnaces and rapid quenching furnaces, mainly used for melting and rapid quenching of master alloys. In the figure, (a) is a vacuum melting furnace and (b) is a vacuum rapid quenching furnace.
[0029] Figure 3 Examples 1 show the alloy ingot and the rapidly quenched alloy strip. The rapidly quenched alloy strip is approximately 145 μm thick, has a nanocrystalline structure, and an average grain size of approximately 38 nm. In the figure, (a) is the alloy ingot; and (b) is the rapidly quenched alloy strip.
[0030] Figure 4 The images show the SEM morphology of the as-cast alloys in Examples 1-6. It can be observed that the as-cast master alloys have a multiphase structure, containing Mg. 24 Y5 main phase, PrMg 12 Phases: Mg2Ni phase, ZrMn2 phase, and MgZn2 phase.
[0031] Figure 5 The XRD diffraction patterns of the as-cast alloys in Examples 1-6 reveal that the as-cast alloys possess a multiphase structure, and the analytical results are consistent with... Figure 4 The conclusion is consistent.
[0032] Figure 6 The SEM images show the morphology of the ball-milled composite powders from Examples 1-6. It can be observed that the ball-milled material particles are approximately spherical, and the dispersion between particles is good, with no severe aggregation.
[0033] Figure 7 The XRD diffraction patterns of the ball-milled composite powders in Examples 1-6 are shown. It can be observed that the diffraction peaks of the ball-milled material are significantly broadened, which is clearly a result of grain refinement and increased lattice stress caused by ball milling.
[0034] Figure 8are the HRTEM morphologies and SAED diffraction rings of the ball-milled composite powders of Examples 1 to 6. The results show that the ball-milled material has a microstructure dominated by nanocrystals. DETAILED DESCRIPTION
[0035] The design concept and mechanism of the present invention are further described in detail below with reference to the accompanying drawings, examples and comparative examples, so as to make the technical solution of the present invention clearer, which is not intended to limit the scope of the present invention.
[0036] The present invention discloses a Mg-RE(Y, Pr)-based Mg 24 Y5 type composite hydrogen storage material, the chemical formula of its composition is: Mg 48 Y 11-x Pr x Ni 3-y-z-m Zr y Mn z Zn m + n wt.% NbF5, where x, y, z, m are atomic ratios, 0<x≤3, 0<y≤1, 0<z≤1, 0<m≤0.5, n is the percentage of NbF5 in the master alloy, and 4≤n≤10.
[0037] Preferably, the atomic ratio x:y:z:m=1:0.3:0.6:0.2, and n=6.
[0038] Through research, the present invention finds that element substitution can reduce the thermal stability of Mg-based alloy hydrides and improve their hydrogen absorption and desorption kinetic properties. Among various alloying elements, rare earth elements in particular have the most significant effect. The selection of the addition amount of each component and its specific action mechanism are as follows: Y and Pr: As is well known, all rare earth elements are hydrogen-absorbing elements. Therefore, adding rare earth elements to improve the performance of hydrogen storage materials has become a natural choice. Especially in AB5 type hydrogen storage alloys, rare earth elements are even more indispensable. It is a consensus in the solid-state hydrogen storage academia that adding a trace amount of rare earth elements can significantly reduce the thermal stability of magnesium hydride and improve the hydrogen absorption and desorption kinetics of magnesium-based alloys. From Figure 1 (a, b) it can be seen that Y and Pr can form Mg 24 Y5 phase and PrMg 12The presence of these phases significantly reduces the thermal stability of magnesium hydrides. The addition of Y and Pr forms YH3 and PrH3 hydrides during hydrogen absorption. These hydrides themselves possess high thermal stability. Although they do not directly participate in the hydrogen absorption and desorption process, their dispersed distribution within the alloy allows them to act as nuclei for heterogeneous nucleation during the hydrogen absorption and desorption phase transition, thus accelerating the reaction rate and acting as a catalyst. Furthermore, the addition of rare earth elements Y and Pr significantly reduces the bonding strength of the Mg-H bonds, improving the thermodynamic properties of magnesium hydrides to some extent. It should be noted that rare earth elements Y and Pr have a high specific gravity; excessive addition of Y and Pr will inevitably lead to a significant decrease in the mass hydrogen storage density of the alloy and an increase in raw material costs.
[0039] Ni: In solid-state hydrogen storage materials, the catalytic effect of Ni is widely recognized, even comparable to that of Pd. Especially in AB5 type alloys, Ni's role is irreplaceable. The necessary condition for a material to absorb hydrogen is the dissociation of hydrogen molecules into hydrogen atoms on the material surface. Hydrogen can hardly dissociate on the surface of pure magnesium, mainly because the dissociation energy of hydrogen on magnesium is extremely high. To provide the energy required for hydrogen molecule dissociation, magnesium must be heated to a very high temperature. Studies have found that adding a certain amount of Ni to magnesium-based alloys significantly reduces the hydrogen dissociation energy, even making it negligible. This catalytic effect of Ni is comparable to that of Pd and V. The addition of Ni can simultaneously improve the hydrogen absorption and desorption kinetics and thermodynamics of magnesium-based alloys. Figure 1 It can be observed that Ni exists in the magnesium-based alloy in the form of Mg2Ni, which is another important reason why Ni improves the hydrogen storage performance of magnesium-based alloys. As is well known, Mg2Ni is an excellent hydrogen-absorbing phase. When this phase comes into contact with hydrogen in the magnesium-based alloy, it preferentially reacts with hydrogen to form Mg2NiH4 hydride. This hydride has a strong catalytic effect on hydrogen absorption in the magnesium-based alloy, acting as a "hydrogen pump effect." It is important to note that the amount of Ni added should not be too large, otherwise a large amount of Mg2Ni phase will be formed, significantly reducing the hydrogen storage capacity of the alloy, as the hydrogen absorption capacity of Mg2NiH4 is only 3.6 wt.%. Furthermore, Ni is a precious metal, and the excessive use of Ni will inevitably significantly increase the cost of raw materials.
[0040] Zr and Mn: As is well known, metallic Zr and Mg cannot be dissolved in each other. Figure 1 Therefore, the hydrogen storage performance of magnesium-based alloys cannot be improved by the direct reaction of Zr with Mg. However, the combined addition of Zr and Mn can form the ZrMn2 phase ( Figure 1 e). The ZrMn2 phase is a hydrogen-absorbing phase that preferentially forms ZrMn2H3 hydrides in magnesium-based alloys, accelerating the hydrogen absorption reaction and exhibiting a significant "hydrogen pump effect." The study also found that the ZrMn2 phase is dispersed at the grain boundaries of magnesium-based alloys, generating a large amount of Mg. 24The Y5 / ZrMn2 phase interface provides an excellent pathway for hydrogen atom diffusion. Simultaneously, the interface offers preferential nucleation sites for hydride formation, factors that are highly beneficial for improving the thermodynamics and kinetics of hydrogen absorption and desorption in the alloy. Besides forming intermetallic compounds with Zr, another important role of Mn is its synergistic effect with Ni, lowering the dissociation energy of hydrogen molecules on the alloy surface and accelerating the hydrogen absorption reaction process in magnesium-based alloys. It is important to note that the Zr and Mn contents must be appropriate; excessive Zr and Mn will significantly reduce the hydrogen storage capacity of magnesium-based alloys and decrease their activation performance.
[0041] Zn: Similar to other transition metals, the addition of appropriate amounts of Zn to magnesium-based alloys can significantly reduce the dissociation energy of hydrogen molecules into hydrogen atoms, thereby improving the hydrogen absorption and desorption kinetics of the alloy. Zn in the alloy is mainly distributed in the form of MgZn2 at the grain boundaries of the magnesium-based alloy, forming a large amount of Mg... 24 The Y5 / MgZn2 phase interface provides a good channel for hydrogen atom diffusion. Simultaneously, the phase interface also provides preferential nucleation sites for the formation of magnesium-based hydrides, further improving the hydrogen absorption kinetics of the alloy. The addition of Zn can reduce the bonding strength of Mg-H bonds, which has a certain effect on improving the thermodynamics of magnesium-based alloys. Another effect of Zn is to increase the brittleness of magnesium-based alloys, which is very beneficial for improving the activation performance and subsequent powder processing properties of the alloy. It should be noted that MgZn2 does not absorb hydrogen; the addition of Zn will inevitably lead to a decrease in the hydrogen storage capacity of magnesium-based alloys.
[0042] After comparing the hydrogen storage capacity, activation performance, and kinetic performance of the alloy with a series of parameters, the optimal ratio of x, y, z, m was found to be x:y:z:m=1:0.3:0.6:0.2, and the optimal content of NbF5 catalyst n=6.
[0043] Specifically, the hydrogen storage alloy has a nanocrystalline structure with an average grain size of 30–150 nm. By alloying with rare earth elements and metallic elements, and combining it with a rapid quenching and ball milling process, significant improvements in the thermodynamics and kinetics of hydrogen absorption and desorption can be achieved.
[0044] Specifically, the Mg-RE(Y,Pr)-based Mg provided by this invention 24 Y5 type composite hydrogen storage alloy has good activation performance and hydrogen absorption and desorption performance. Under the conditions of 280℃ and 3MPa, it can store hydrogen with a capacity of ≥5.22 wt.%; after 200 hydrogen absorption and desorption cycles, the capacity retention rate is ≥93.5%; it can be widely used as a solid hydrogen storage material in various scenarios such as hydrogen fuel cells.
[0045] The present invention also provides a method for preparing the hydrogen storage alloy, specifically comprising the following steps: S1: Prepare the ingredients according to the preset chemical formula, with a certain proportion of burn-off loss added when weighing Mg, rare earth Y and Pr; S2: Place the prepared raw materials in a magnesium oxide crucible in sequence, evacuate the vacuum, fill with protective gas and heat to obtain a molten liquid master alloy; pour the alloy into a copper mold, and obtain a master alloy ingot after solidification.
[0046] S3: Place the ingot prepared in step S2 into a quartz tube with a slit at the bottom, and induction heat it until the ingot is completely melted. Under the pressure of the protective gas, the liquid alloy is sprayed from the slit at the bottom of the quartz tube onto the surface of a rotating water-cooled copper roller to obtain a fast-quenched alloy strip with a thickness between 100 and 350 μm.
[0047] S4: The rapidly quenched alloy strip prepared in S3 is mechanically crushed and sieved to obtain alloy powder. The sieved alloy powder, together with a certain amount of nano NbF5 catalyst and stainless steel grinding balls, is loaded into a stainless steel ball mill jar. After vacuuming, high-purity argon gas is introduced, and the mixture is ball-milled in an all-around planetary high-energy ball mill to obtain ball-milled powder, which is the composite hydrogen storage material.
[0048] After secondary remelting, the master alloy ingot undergoes rapid quenching, which further improves the uniformity of the alloy composition. Rapid quenching (cooling rate >1000℃ / s) yields a precursor with ultrafine grains (nanoscale). The rapidly quenched alloy has a columnar crystalline structure, and its numerous grain boundaries provide excellent channels for hydrogen atom diffusion, which is particularly beneficial for improving the hydrogen absorption and desorption kinetics of Mg-based alloys. In addition, the rapidly quenched alloy structure contains a high density of crystal defects, including dislocations, stacking faults, twins, and numerous grain boundaries. This microstructure is extremely beneficial for improving the thermodynamic and kinetic properties of the alloy. Unlike the crystal defects formed after mechanical ball milling of the master alloy ingot, the ultrafine structure and crystal defects obtained by rapid quenching have high stability. After multiple hydrogen absorption and desorption cycles, the grains are not prone to agglomeration and growth. In terms of hydrogen absorption and desorption performance, it not only has excellent hydrogen absorption and desorption kinetics but also good stability during hydrogen absorption and desorption cycles.
[0049] Rapidly quenched alloy flakes are mechanically crushed and sieved, then subjected to short-term mechanical ball milling after the addition of a nano-NbF5 catalyst. This treatment improves the surface condition of the alloy while maintaining its microstructure in the rapidly quenched state, leveraging the characteristics and advantages of both rapid quenching and ball milling processes. During ball milling, the nano-NbF5 catalyst is uniformly distributed on the alloy surface, forming a highly active coating layer that fully exerts its catalytic effect, thereby improving the thermodynamics and kinetics of hydrogen absorption and desorption. On one hand, the catalytic effect of nano-NbF5 lies in its very low hardness, which facilitates the formation of a highly active coating layer on the alloy particle surface during ball milling, significantly improving the hydrogen absorption and desorption kinetics. On the other hand, nano-NbF5 provides excellent lubrication during ball milling, significantly reducing the possibility of alloy particles adhering to the ball mill jar wall and improving milling efficiency. It is precisely this combination of rapid quenching, ball milling, and catalyst addition that results in a substantial improvement in the thermodynamics and kinetics of hydrogen absorption and desorption.
[0050] Specifically, the mass percentage of Mg, rare earth Y and Pr lost during burning in S1 is 5% to 10%. Mg, rare earth Y and Pr are easily volatilized and will be lost during the batching and heating melting process, so a certain amount of loss needs to be added to make up for it.
[0051] Specifically, the order and operation of placing the raw materials in step S2 are as follows: The cleaned raw materials are mixed according to the specified proportions and placed sequentially in the magnesium oxide crucible. The bulk rare earth elements Y and Pr are mixed and placed at the bottom of the crucible; sponge Zr is placed on top of the rare earth elements Y and Pr; electrolytic Ni and Mn are placed on top of the sponge Zr; and metallic Mg and Zn are placed on top. This placement order is determined by the melting point and solid solubility of the metals, allowing them to melt sequentially from low to high melting point, effectively reducing the burn-off of magnesium and rare earth elements, resulting in a more stable alloy composition and a more uniform element distribution.
[0052] Specifically, the specific operation for melting the raw materials in step S2 is as follows: vacuuming to 5×10 -3 At pressures above 0.01-0.1 MPa, high-purity helium or a 1:1 helium-argon mixture is introduced as a protective gas. The alloy is then melted using medium-frequency induction heating, ensuring all raw materials are completely melted. The molten alloy temperature is controlled at approximately 1300-1400℃ and held for 3-5 minutes to achieve complete homogenization of the alloy composition. The liquid alloy is then poured into a copper mold and allowed to cool to room temperature to obtain a master alloy ingot.
[0053] Specifically, the rapid quenching process in step S3 involves loading the cast alloy bar into a quartz tube with a narrow slit at the bottom, and using induction heating to completely melt it. The liquid alloy (approximately 1300°C) is continuously sprayed from the narrow slit at the bottom onto the surface of a rotating water-cooled copper roller under the pressure of a protective gas (approximately 1.05 atm). The surface linear velocity (quenching rate) of the copper roller is 3–20 m / s, and the water inlet flow rate is ≥20 m³ / s. 3 / h, water temperature 18~20℃. After cooling to room temperature, the rapidly quenched alloy strip described in the patent is obtained, with a thickness of 100~350μm and a grain size in the range of 30~150nm.
[0054] It is important to emphasize that the most critical process parameters for rapid quenching are as follows: 1) Quenching Rate: Quenching rate refers to the surface linear velocity of the rotating copper roller. Determining a suitable quenching rate is a key technical parameter. There is no single quenching rate suitable for all alloys; the optimal quenching rate varies with the alloy's composition. A suitable quenching rate ensures that the rapidly quenched alloy strip has an almost completely nanocrystalline structure. Too high a quenching rate will result in more amorphous phases in the alloy, leading to a decrease in hydrogen storage capacity and kinetic properties; too low a quenching rate will cause significant grain coarsening in the alloy, reducing hydrogen absorption and desorption kinetic properties.
[0055] 2) Quartz tube nozzle width: The nozzle slit width is a key technical parameter. An excessively large slit will result in excessive flow of the liquid alloy, reducing the cooling effect during solidification and preventing the acquisition of an ultra-fine columnar crystal structure. An excessively small slit will cause the liquid alloy to solidify at the nozzle, resulting in discontinuous rapid quenching. Furthermore, a nozzle that is too small will increase the rapid quenching time, reducing production efficiency.
[0056] 3) Rapid Quenching Initiation Temperature: The rapid quenching initiation temperature of the liquid alloy is a key technical parameter. The optimal rapid quenching initiation temperature for this patented alloy is approximately 1300℃. If the temperature is much lower than 1300℃, the fluidity of the liquid alloy will be very poor, resulting in a slow flow rate through the nozzle and even solidification clogging the nozzle. Another problem with excessively low casting temperatures is poor roller adhesion when the liquid alloy contacts the rapid quenching roller, significantly reducing the cooling rate of the alloy and making it impossible to obtain an ultra-fine crystal structure. If the rapid quenching initiation temperature of the liquid alloy is much higher than 1300℃, the low viscosity of the alloy will result in poor roller adhesion, reducing the cooling capacity during rapid quenching and leading to a decrease in the performance of the rapidly quenched alloy.
[0057] 4) Cooling water flow rate and temperature of copper rollers: The flow rate and temperature of cooling water for copper rollers must also meet the requirements, otherwise it will affect the microstructure of the rapidly quenched thin strip and thus affect the hydrogen storage performance of the alloy.
[0058] Specifically, the specific parameters of the ball milling process in S4 are: ball-to-material ratio of 20:1, ball mill speed of 250 rpm, and ball milling time of 3 to 8 hours; the preferred ball milling time is 4 hours.
[0059] During ball milling, the ball mill is stopped for 0.5 hours every hour of continuous operation to prevent the temperature of the milling jar and abrasive from becoming too high. Excessive temperature can cause decomposition of the nano-NbF5 catalyst, thus reducing its catalytic effect. Determining the appropriate ball milling time is crucial and significantly impacts the catalyst's performance. On one hand, excessively long milling times will introduce a large amount of amorphous phase, reducing the material's hydrogen storage capacity. The optimal milling time ensures that too many amorphous phases are present in the milled material. On the other hand, a suitable milling time ensures good powder dispersion without severe agglomeration, thus preventing a significant decrease in the material's hydrogen absorption capacity. Excessively long milling times will result in a large amount of amorphous phase in the microstructure, and agglomeration due to cold welding between particles will also reduce the material's hydrogen absorption and desorption performance. Furthermore, excessively long milling times will severely affect the material preparation efficiency, which is unacceptable for industrialization.
[0060] Based on the above component design and preparation method, the specific components and preparation processes of the present invention's design embodiments and comparative examples are as follows: Example 1: Mg 48 Y 10 Pr1Ni 1.9 Zr 0.3 Mn 0.6 Zn 0.2 + 6 wt.% NbF5 (rapid quenching + ball milling) Example 2: Mg 48 Y9Pr2Ni 1.9 Zr 0.3 Mn 0.6 Zn 0.2 + 6 wt.% NbF5 (rapid quenching + ball milling) Example 3: Mg 48 Y 10 Pr1Ni 1.2 Zr 1.0 Mn 0.6 Zn 0.2 + 6 wt.% NbF5 (rapid quenching + ball milling) Example 4: Mg 48 Y 10 Pr1Ni 1.5 Zr 0.3 Mn 1.0 Zn 0.2 + 6 wt.% NbF5 (rapid quenching + ball milling) Example 5: Mg 48 Y 10 Pr1Ni 1.6 Zr 0.3 Mn 0.6 Zn0.5 + 6 wt.% NbF5 (rapid quenching + ball milling) Example 6: Mg 48 Y8Pr3Ni 1.9 Zr 0.3 Mn 0.6 Zn 0.2 + 6 wt.% NbF5 (rapid quenching + ball milling) Example 7: Mg 48 Y 10 Pr1Ni 1.9 Zr 0.3 Mn 0.6 Zn 0.2 + 4 wt.% NbF5 (rapid quenching + ball milling) Example 8: Mg 48 Y 10 Pr1Ni 1.9 Zr 0.3 Mn 0.6 Zn 0.2 + 10 wt.% NbF5 (rapid quenching + ball milling) Example 9: Mg 48 Y 10 Pr1Ni 1.9 Zr 0.3 Mn 0.6 Zn 0.2 + 6 wt.% NbF5 (rapid quenching + ball milling for 3 hours) Example 10: Mg 48 Y 10 Pr1Ni 1.9 Zr 0.3 Mn 0.6 Zn 0.2 + 6 wt.% NbF5 (rapid quenching + ball milling for 8 hours) Example 11: Mg 48 Y 10 Pr1Ni 1.9 Zr 0.3 Mn 0.6 Zn 0.2 + 6 wt.% NbF5 (3m / s rapid quenching + ball milling) Example 12: Mg 48 Y 10 Pr1Ni 1.9 Zr 0.3 Mn 0.6 Zn 0.2 + 6 wt.% NbF5 (20 m / s rapid quenching + ball milling) Comparative Example 1: Mg 48 Y 10 Pr1Ni1.9 Zr 0.3 Mn 0.6 Zn 0.2 (Quick quenching + ball milling) Comparative Example 2: Mg 48 Y 10 Pr1Ni 1.9 Zr 0.3 Mn 0.6 Zn 0.2 + 2 wt.% NbF5 (rapid quenching + ball milling) Comparative Example 3: Mg 48 Y 10 Pr1Ni 1.9 Zr 0.3 Mn 0.6 Zn 0.2 + 15 wt.% NbF5 (rapid quenching + ball milling) Comparative Example 4: Mg 48 Y 10 Pr1Ni 1.9 Zr 0.3 Mn 0.6 Zn 0.2 + 6 wt.% NbF5 (rapid quenching + ball milling for 1 hour) Comparative Example 5: Mg 48 Y 10 Pr1Ni 1.9 Zr 0.3 Mn 0.6 Zn 0.2 + 6 wt.% NbF5 (casting + ball milling) Comparative Example 6: Mg 48 Y 10 Pr1Ni 1.9 Zr 0.3 Mn 0.6 Zn 0.2 + 6 wt.% NbF5 (1 m / s rapid quenching + ball milling) According to the chemical formulas of each embodiment, bulk metal Mg, rare earth metals Y and Pr, sponge Zr, electrolytic Mn and Ni, and bulk metal Zn were selected. The metal purity requirement was ≥99.5%. After polishing to remove the surface oxide layer, the selected bulk metals were weighed according to the stoichiometric ratio. Specifically, the proportions of Mg, Y, and Pr were increased by 5% to compensate for losses during smelting. The technical parameters for each stage of the preparation process are as follows: During induction heating, a vacuum of 1×10⁻⁶ was applied. -2 ~5×10 -4The gas is filled with high-purity helium or a helium-argon mixture with a volume ratio of 1:1 at a pressure of 0.01–0.1 MPa; the melting temperature is 1300–1400℃; and the surface linear velocity of the rapidly quenched water-cooled copper roller is 3–20 m / s. The rapidly quenched thin sheets are mechanically crushed and passed through a 200-mesh sieve, then mixed with nano-NbF5 catalyst and stainless steel grinding balls and loaded into a stainless steel ball mill jar. The mixture is then ball-milled using an omnidirectional planetary ball mill for 3–8 hours, preferably 4 hours, with the mill stopped for 0.5 hours after every hour of continuous operation.
[0061] It should be emphasized that all process parameters can be appropriately selected within the above range to prepare the hydrogen storage material powder described in the patent. Therefore, although only one typical embodiment has been given in this invention, this embodiment is applicable to preparation methods with different parameters.
[0062] Process parameters for Example 1: S1: Process parameters of Example 1: According to the chemical formula Mg 48 Y 10 Pr1Ni 1.9 Zr 0.3 Mn 0.6 Zn 0.2 The following materials were selected: bulk Mg, rare earth Y and Pr, sponge Zr, electrolytic Ni and Mn, and bulk metallic Zn. These metals had a purity ≥99.5%. They were weighed according to stoichiometric ratios, with each furnace containing 5 kg of materials: 2572 g bulk metallic Mg, 1960 g rare earth Y, 311 g rare earth Pr, 57 g sponge Zr, 234 g electrolytic Ni, 69 g electrolytic Mn, and 29 g metallic Zn.
[0063] S2: Place the weighed bulk metal into the magnesium oxide crucible of the medium-frequency induction furnace according to the designed process. Mix the bulk rare earth elements Y and Pr and place them at the bottom of the crucible. Place the sponge Zr on top of the mixed rare earth elements Y and Pr, then place the electrolytic Ni and Mn on top of the sponge Zr, and finally place the metallic Mg and Zn on top. Then close the furnace lid and evacuate for approximately 30 minutes until the vacuum level reaches 5 × 10⁻⁶. -3 Above a pressure of 0.04 MPa, high-purity helium protective gas is introduced until the pressure reaches 0.04 MPa. The power of the melting furnace is adjusted to 10 kW, and the temperature is controlled at 750 °C to melt the Mg metal. Then, the power is adjusted to 30 kW, and the temperature is controlled at 1400 °C to melt the remaining metals. The molten alloy is held in the protective gas atmosphere for 5 minutes to ensure complete homogenization of the alloy composition. The molten alloy is poured into a copper mold, and after cooling to room temperature, the mold is opened to obtain the master alloy ingot.
[0064] S3: Place the ingot prepared in step S2 inside a quartz tube with a slit at the bottom, and heat it by induction until the ingot is completely melted (about 1400°C). Under the pressure of a protective gas, spray the pre-cooled liquid alloy (about 1300°C) from the slit at the bottom of the quartz tube onto the surface of a rotating (765 rpm) water-cooled copper roller (quenching speed 15 m / s) to obtain a fast-quenched alloy strip with an average thickness of about 145 μm and an average grain size of about 38 nm.
[0065] S4: Mechanically crush the rapid-quenched alloy sheet and pass it through a 200-mesh sieve. Weigh 20 grams of the sieved alloy powder, 1.2 grams of nano-NbF5 catalyst, and 400 grams of stainless steel grinding balls, and mix them together. Place the mixture into a 250 ml stainless steel ball mill jar, evacuate, fill with high-purity argon, and then seal. Ball mill in an all-around planetary high-energy ball mill for 4 hours. The ball mill is stopped for 0.5 hours after every 1 hour of continuous operation.
[0066] The raw materials for all examples and comparative examples were weighed according to their chemical formulas, and other preparation process parameters were the same as in Example 1 unless otherwise specified.
[0067] The preparation process and catalyst addition amount of Examples 1-6 are exactly the same. The main difference is that the composition of the master alloy is different. The above examples have verified the effect of the composition change on the hydrogen storage performance of the material and screened out the master alloy composition with the best hydrogen storage performance.
[0068] The master alloy composition and preparation process of Examples 7 and 8 are exactly the same as those of Example 1, the difference being the addition of different masses of nano-NbF5 catalyst. Through the performance comparison of Examples 1, 7, and 8, the influence of the amount of catalyst added on the hydrogen storage performance of the alloy was verified, and the optimal catalyst content was selected.
[0069] The master alloy composition and catalyst addition amount in Examples 9 and 10 were exactly the same as in Example 1, the difference being the use of different ball milling times. Performance comparisons of Examples 1, 9, and 10 verified the effect of ball milling time on the hydrogen storage performance of the materials, and the optimal ball milling time was selected.
[0070] The composition of the master alloy and the amount of catalyst added in Examples 11 and 12 were exactly the same as those in Example 1, the difference being that the master alloy was subjected to different quenching rates. Through the performance comparison of Examples 1, 11, and 12, the influence of quenching rate on the hydrogen storage performance of the material was verified, and the optimal quenching rate was selected.
[0071] Comparative Example 1 has the same master alloy composition and preparation process as Example 1. The difference is that NbF5 nano-catalyst is not added during ball milling. This comparative example verifies the effect of adding nano-NbF5 catalyst on improving the hydrogen storage performance of Mg-RE based materials.
[0072] The components and preparation processes of Comparative Examples 2 and 3 were exactly the same as those of Example 1, except that nano-NbF5 catalysts exceeding the content range given in this invention were added, which verified the effect of the amount of catalyst added on the hydrogen storage performance of the material.
[0073] The composition of the master alloy and the amount of catalyst added in Comparative Example 4 are exactly the same as those in Example 1. The difference is that the ball milling time is less than the lower limit ball milling time given in this invention. The purpose is to determine the shortest ball milling time to obtain good hydrogen storage performance by comparing the performance of Comparative Example 4 and Example 1.
[0074] The master alloy composition and ball milling process of Comparative Example 5 and Example 1 are the same. The difference is that the master alloy of Comparative Example 5 was not subjected to rapid quenching treatment after melting. The purpose is to verify the effect of rapid quenching treatment on the hydrogen storage performance of Mg-RE(Y,Pr) based materials.
[0075] The difference between Comparative Example 6 and Example 1 lies in the amount of catalyst added and the master composition. The quenching rate of the master alloy in Comparative Example 6 is lower than the minimum quenching rate given in this invention. The purpose is to determine the optimal quenching rate range for rapid quenching.
[0076] The phase structure and phase composition of the ball-milled composite material were tested by XRD. The microstructure and morphology of the cast master alloy and the ball-milled composite material powder were observed by scanning electron microscopy (SEM). The morphology and microstructure of the ball-milled composite material powder were observed by high-resolution transmission electron microscopy (HRTEM). The crystal state of the ball-milled material was determined by selected area electron diffraction (SAED).
[0077] Figure 1 Phase diagrams for binary alloy systems with different compositions are shown, namely Mg-Y, Mg-Pr, Mg-Ni, Mg-Zr, Zr-Mn, and Mg-Zn systems. These phase diagrams are used to assist in the design of alloy compositions and to determine the possible phase compositions of alloys.
[0078] Figure 2 This is a vacuum induction melting and rapid quenching furnace, mainly used for melting and rapid quenching of master alloys. The maximum capacity of the melting furnace crucible is 8 kg; the rated power is 40 kW; and the ultimate vacuum degree is 5 × 10⁻⁶. -4 Pa; The diameter of the water-cooled copper roller in the rapid quenching furnace is 375mm, and the limiting quenching speed is 35m / s (the limiting speed of the copper roller is 1800rpm).
[0079] Figure 3 The images show actual photos of the alloy ingot and the rapidly quenched thin strip from Example 1. The alloy ingot is cylindrical with a diameter of φ30mm. The rapidly quenched strip is approximately 145μm thick, has a nanocrystalline structure, and an average grain size of approximately 38nm.
[0080] Figure 4 The images show the SEM morphology of the as-cast alloys in Examples 1-6. It can be observed that the as-cast master alloys have a multiphase structure, including the main phase Mg. 24Y5 and second-phase PrMg 12 Mg2Ni, ZrMn2 and MgZn2.
[0081] Figure 5 The XRD diffraction pattern of the as-cast alloy is shown. Analysis of the XRD data reveals that the alloy has a multiphase structure, including the main phase Mg. 24 Y5 and secondary phase PrMg 12 Mg2Ni, ZrMn2 and MgZn2.
[0082] Figure 6 The images show the SEM morphology of the ball-milled material powders in Examples 1-6. It can be observed that the ball-milled composite material powder particles are approximately spherical, and the dispersion between particles is good, with no severe aggregation.
[0083] Figure 7 The XRD diffraction patterns of the ball-milled powders in Examples 1-6 are shown. It can be observed that the diffraction peaks of the ball-milled powder composites are significantly broadened, which is clearly a result of grain refinement and increased lattice stress caused by ball milling.
[0084] Figure 8 The HRTEM morphology of the ball-milled composite powders in Examples 1-6 shows that the ball-milled materials have a microstructure dominated by nanocrystals.
[0085] The solid-state hydrogen storage capacity and kinetics of the material were tested using a fully automated Sieverts instrument. The hydrogen absorption temperature was 280℃, the initial hydrogen absorption pressure was 3 MPa, and the hydrogen release was performed at 280℃ and 1×10⁻⁶ MPa. -4 The test was conducted at a pressure of MPa. Using S 200 This represents the capacity retention rate of the material after 200 charge-discharge hydrogen cycles, i.e., S. 200 = C 200 / C max ×100%. C max - Saturated reversible hydrogen absorption capacity; C 200 - Reversible hydrogen uptake capacity after 200 charge-discharge cycles. The results are shown in Table 1.
[0086] Table 1 Solid-state hydrogen storage performance of the examples and comparative materials —Saturated hydrogen absorption (wt.%) at an initial hydrogen pressure of 3 MPa and 280 °C; — Hydrogen absorption rate (wt.%) within 5 minutes at an initial hydrogen pressure of 3 MPa and a temperature of 280 °C. — With an initial pressure of 1×10 -4 Hydrogen release (wt.%) within 10 minutes at MPa and 280℃.
[0087] The Mg-RE(Y,Pr)-based Mg provided by this invention 24 Y5-type hydrogen storage material exhibits high hydrogen storage capacity, good hydrogen desorption kinetics, and cycle stability, with a hydrogen storage capacity ≥ 5.22 wt.%. After 200 hydrogen absorption and desorption cycles, the capacity retention rate (S) remains high. 200 The hydrogen storage capacity is ≥93.5%. These results indicate that the composite material exhibits good reversible hydrogen absorption and desorption performance at a relatively low temperature (280℃), and the preparation process is simple and easy to operate, making it suitable for large-scale preparation. Compared with similar alloys at home and abroad, the hydrogen storage capacity and hydrogen absorption and desorption kinetics of the material of this invention are significantly improved.
[0088] Examples 1-6 show that, with the preparation process and catalyst addition amount remaining unchanged, changes in the composition of the master alloy cause significant changes in its performance, indicating that the hydrogen storage performance of the material is closely related to the amount of chemical composition.
[0089] Examples 7 and 8 used the same master alloy composition and preparation process as Example 1, but the amount of catalyst added was different. As a result, the hydrogen storage performance of the composite material was significantly changed, showing that the amount of catalyst added has a significant impact on the hydrogen storage performance of the composite material.
[0090] Examples 9 and 10 used the same master alloy composition and catalyst addition amount as Example 1, but with different ball milling times. As a result, the hydrogen storage performance of the materials changed significantly, showing that ball milling time has a significant impact on the hydrogen storage performance of Mg-RE(Y,Pr) based materials.
[0091] Examples 11 and 12 used the same master alloy composition and catalyst addition as Example 1, but the quenching rate of the master alloy was different. As a result, the hydrogen storage performance of the material was significantly changed, showing that the quenching rate of the rapid quenching has a significant impact on the hydrogen storage performance of Mg-RE(Y,Pr) based materials.
[0092] Compared with Example 1, Comparative Example 1 had the same master alloy composition and preparation process, but no catalyst was added during the ball milling process. It was found that the hydrogen storage performance of Comparative Example 1 was much lower than that of Example 1, indicating that the addition of NbF5 nano-catalyst is very effective in improving the hydrogen storage performance of Mg-RE(Y,Pr) based material.
[0093] Compared with Example 1, Comparative Examples 2 and 3 had the same master alloy composition and preparation process, but the amount of catalyst added significantly exceeded the content range given in the patent. The results showed that the hydrogen storage performance of the comparative examples was significantly lower than that of Example 1, indicating that although the nano NbF5 catalyst is very effective in improving the hydrogen storage performance of Mg-RE(Y,Pr) based materials, there is an optimal content range.
[0094] Compared with Example 1, Comparative Example 4 had the same master alloy composition and catalyst addition amount, but the ball milling time of Comparative Example 4 was less than the minimum ball milling time given in the patent. The results showed that its hydrogen storage performance was much lower than that of Example 1, indicating that if the ball milling time is less than the given minimum time, the performance of the material will be significantly reduced.
[0095] Compared with Example 1, Comparative Example 5 had the same composition of the master alloy, the amount of catalyst added, and the ball milling process, but the master alloy of Comparative Example 5 was not subjected to rapid quenching treatment. The results showed that the hydrogen storage performance of Comparative Example 5 was significantly lower than that of Example 1, especially the difference in cycle stability was more significant, demonstrating the important role of rapid quenching treatment in the hydrogen storage performance of Mg-RE(Y,Pr) based alloys.
[0096] Compared with Example 1, Comparative Example 6 had the same master alloy composition, catalyst addition amount, and ball milling time. However, the quenching rate of the master alloy in Comparative Example 6 was much lower than the minimum quenching rate given in this patent. As a result, its hydrogen storage performance was much lower than that of Example 1. This shows that although rapid quenching can significantly improve the hydrogen storage performance of Mg-RE(Y,Pr) based materials, the selection of a suitable quenching rate is very important.
[0097] In summary, this invention significantly reduces the thermal stability of Mg hydrides and improves their hydrogen absorption and desorption kinetics by adding rare earth elements Y and Pr, as well as transition metal elements Zr, Ni, Mn, and Zn. Rapidly quenchable alloy powder is prepared using mechanical pulverization, and after adding a small amount of nano-NbF5 catalyst, mechanical ball milling is performed for an appropriate time to achieve Mg-RE(Y,Pr)-based Mg... 24 The hydrogen absorption and desorption thermodynamics and kinetics of the Y5-type material have been further improved. The composite hydrogen storage material prepared by this invention has high reversible hydrogen absorption and desorption capacity, good hydrogen absorption and desorption thermodynamic and kinetic properties, and excellent cycle stability, showing high application potential in hydrogen supply carriers in various application scenarios. Moreover, the preparation process of the material is simple and easy to operate, and can fully meet the technical requirements for large-scale preparation.
[0098] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.
[0099] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within the present invention. No reference numerals in the claims should be construed as limiting the scope of the claims.
Claims
1. A nano-NbF5-catalyzed Mg-RE(Y,Pr)-based Mg 24 Y5 type composite hydrogen storage material, characterized in that... The chemical formula composition is: Mg 48 Y 11-x Pr x Ni 3-y-z-m Zr y Mn z Zn m + n wt.% NbF5, wherein x, y, z, m are atomic ratios, 0<x≤3, 0<y≤1, 0<z≤1, 0<m≤0.5, n is the percentage of the nano NbF5 catalyst in the master alloy, and 4≤n≤10.
2. The composite hydrogen storage material according to claim 1, characterized in that, The atomic ratio of the chemical formula is: x:y:z:m=1:0.3:0.6:0.2, n=6.
3. A nano-NbF5-catalyzed Mg-RE(Y,Pr)-based Mg 24 The preparation method of Y5 type composite hydrogen storage material is characterized by: The preparation of the composite hydrogen storage material according to claim 1 or 2 includes the following steps: S1. Prepare the ingredients according to the preset chemical formula, and increase the burn-off amount by a certain proportion when weighing Mg, rare earth Y and Pr. S2. Alloy melting is carried out in a vacuum melting furnace. The prepared raw materials are placed in a magnesium oxide crucible in sequence. After vacuuming, an inert protective gas is introduced and heated to obtain a molten liquid master alloy. After holding at the temperature for 3 to 5 minutes, the liquid alloy is poured into a copper mold to obtain a cylindrical master alloy ingot. S3. The rapid quenching process is carried out in a vacuum rapid quenching furnace. The cylindrical master alloy ingot prepared in S2 is placed in a quartz tube with a slit at the bottom and heated by induction until it is completely melted. Under the action of protective gas pressure, the liquid alloy is sprayed from the slit at the bottom of the quartz tube onto the surface of a rotating water-cooled copper roller to obtain a rapid quenched alloy strip. S4. The rapidly quenched alloy strip is mechanically crushed and passed through a 200-mesh sieve to obtain alloy powder. The sieved alloy powder, a set amount of nano NbF5 catalyst, and stainless steel grinding balls are loaded into a stainless steel ball mill jar. After vacuuming, high-purity argon gas is introduced, and the mixture is ball-milled in an all-around planetary high-energy ball mill to obtain ball-milled composite material powder, which is the composite hydrogen storage material.
4. The preparation method according to claim 3, characterized in that, The mass percentage of Mg, rare earth Y, and Pr lost during burning in S1 is 5% to 10%.
5. The preparation method according to claim 3, characterized in that, The specific process and parameters in S2 are as follows: evacuate to 1×10⁻⁶. -2 ~5×10 -5 Pa, introduce high-purity helium gas at 0.01~0.1MPa or a helium + argon mixture with a volume ratio of 1:1 as a protective gas, and heat to 1300~1400℃.
6. The preparation method according to claim 3, characterized in that, The nozzle slit width at the bottom of the quartz tube in S3 is 0.3±0.005mm, and the surface linear velocity of the rotating water-cooled copper roller is 3~20m / s.
7. The preparation method according to claim 3, characterized in that, The thickness of the fast-quenched alloy strip described in S3 is between 100 and 350 μm.
8. The preparation method according to claim 3, characterized in that, The fast-quenched alloy strip has a nanocrystalline structure with a grain size of 30~150nm.
9. The preparation method according to claim 3, characterized in that, The specific parameters for the ball milling process in S4 are: ball-to-material ratio 20:1, ball mill speed 250 rpm, and ball milling time 3-8 hours.
10. The preparation method according to claim 3, characterized in that, The order and specific operation of placing each raw material in S2 are as follows: after mixing the blocky rare earth Y and Pr, place them at the bottom of the crucible; place the sponge Zr on top of the rare earth Y and Pr; place the electrolytic Ni and Mn on top of the sponge Zr; and place the metallic Mg and Zn on top.