A surface-modified rare-earth hydrogen storage alloy, its preparation method and application
By modifying rare earth hydrogen storage alloys with a core-shell modified structure, the problems of high cost, low activity, and poor stability of rare earth hydrogen storage alloy catalysts have been solved, achieving high efficiency and low cost in improving catalytic performance and selectivity.
Patent Information
- Application Number
- CN202611294230.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-25
- Publication Date
- 2026-11-17
AI Technical Summary
Existing rare earth hydrogen storage alloy catalysts suffer from high cost, low activity, poor cycle stability, and insufficient selectivity, especially at high temperatures they are prone to sintering and deactivation, and CN bonds are easily broken.
A surface-modified rare earth hydrogen storage alloy with a core-shell-modification structure is constructed. The core layer is an AB5 or AB3-4 type superlattice structure, the shell layer is a Ni-rich nanocrystalline layer, and the modification layer is a rare earth oxide loaded with trace amounts of noble metal particles. The three-layer structure is constructed through hot alkaline impregnation and low-temperature oxidation treatment.
It significantly increases the number and structural stability of catalytic active sites, improves hydrogenation conversion and dehydrogenation efficiency, reduces reaction temperature, simplifies catalyst configuration, reduces costs, and achieves a synergistic balance between high activity and high selectivity.
Smart Images

Figure CN123105548A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of rare earth alloy materials technology, and in particular to a surface-modified rare earth hydrogen storage alloy, its preparation method and application. Background Technology
[0002] Organic liquid hydrogen storage technology is an important pathway to realize large-scale hydrogen energy storage and transportation. Its core lies in developing efficient and low-cost hydrogenation and dehydrogenation catalysts. Existing catalysts still face the following challenges: 1. Efficient dehydrogenation catalysts mainly rely on precious metals such as Pd and Pt, which are costly and scarce; 2. While non-precious metal catalysts or bimetallic catalysts reduce costs, their activity and selectivity are insufficient; 3. Catalysts have poor cycle stability and are prone to sintering and deactivation at high temperatures; 4. Catalysts have poor selectivity and CN bonds are easily broken at high temperatures.
[0003] Building upon this, researchers discovered that rare-earth hydrogen storage alloys possess the dual functional potential of reversible hydrogen absorption and desorption, and catalysis of organic compounds. However, the following problems limit the catalytic performance of pristine rare-earth hydrogen storage alloys: 1. Surface oxide layer obstruction: The lanthanum oxide / nickel oxide layer formed on the alloy surface under natural conditions hinders hydrogen transfer and catalytic reactions; 2. Insufficient active sites: The surface Ni atomic density is low, resulting in an insufficient number of catalytic active sites; 3. High-temperature sintering: Under LOHC dehydrogenation reaction conditions (>180℃), surface Ni particles are prone to migration and aggregation, leading to activity decay.
[0004] Therefore, it is urgent to fully develop the catalytic potential of rare earth hydrogen storage alloys in LOHC hydrogenation and hydrogen storage in order to solve the above-mentioned technical problems. Summary of the Invention
[0005] Based on the above analysis, the present invention aims to provide a surface-modified rare earth hydrogen storage alloy, its preparation method and application, in order to effectively improve at least one of the problems of low catalytic activity, poor cycle stability and insufficient selectivity of existing LOHC catalysts while controlling costs.
[0006] On one hand, the present invention provides a surface-modified rare-earth hydrogen storage alloy having a core-shell structure composed of a core layer, a shell layer, and a modification layer; the core layer has an AB5 type crystal structure or AB 3-4 The superlattice crystal structure is described; the shell is a Ni-rich nanocrystalline shell, and the Ni atom percentage of the shell minus the Ni atom percentage of the core layer is ≥10%; the modification layer is a rare earth oxide stabilizing layer; the modification layer partially covers the surface of the shell. The general chemical formula of the AB5 type crystal structure is R1. z1 La 1-z1 Ni 5-x1-y1 Al x1 M1 y1Where R1 is a rare earth element other than La, 0≤z1<1; M1 is selected from at least one of Co, Cu, Mn, Fe, Sn, V, Ti, Zr, Cr, Zn, Mo and Si, 0≤x1+y1≤1.5, 0≤x1≤1, 0≤y1≤0.6; The AB 3-4 The general chemical formula for a superlattice crystal structure is Ln x2 R2 1-x2 Ni n-z M2 z Wherein, Ln is selected from one or more of La, Ce, Pr, Nd, Sm, and Gd; R2 is selected from one or more of Y, Mg, Sm, and Gd; M2 is selected from one or more of Al, Co, Mn, Fe, Cu, Sn, Cr, and Zn, 0≤x2≤0.5, 3.0≤n≤4.0, and 0≤z≤1.5.
[0007] Further, the thickness of the shell layer is 5~200 nm. More preferably, the thickness of the shell layer is 10~100 nm.
[0008] Further, the thickness of the modified layer is 1~20 nm. More preferably, the thickness of the modified layer is 2~10 nm.
[0009] Furthermore, the coverage of the modified layer is 30-80%.
[0010] Furthermore, the surface-modified rare-earth hydrogen storage alloy also includes noble metal particles loaded between the shell layer and the modification layer; the noble metal particles are at least one of Pd, Pt and Ru; the particle size of the noble metal particles is 1~10 nm; The loading amount of the precious metal particles is 0.5 to 3 wt% of the total mass of the surface-modified rare earth hydrogen storage alloy. More preferably, the loading amount of the precious metal particles is 0.5 to 1.5 wt% of the total mass of the surface-modified rare earth hydrogen storage alloy.
[0011] On the other hand, the present invention provides a method for preparing the above-mentioned surface-modified rare earth hydrogen storage alloy, comprising the following steps: S1. Preparation of rare earth hydrogen storage alloy matrix powder; S2. The rare earth hydrogen storage alloy matrix powder is immersed in a hot alkaline solution, then washed with deionized water until neutral, and then vacuum dried. S3. The rare earth hydrogen storage alloy matrix powder processed in step S2 is subjected to oxidation treatment to obtain the surface-modified rare earth hydrogen storage alloy.
[0012] Furthermore, in the above preparation method, step S1 specifically involves: preparing rare earth hydrogen storage alloy master ingots or rare earth hydrogen storage alloy sheets using a vacuum melting process, annealing them, and then crushing and pulverizing them to obtain the rare earth hydrogen storage alloy matrix powder.
[0013] Furthermore, in the above preparation method, step S1 specifically involves: weighing each metal raw material according to the stoichiometric ratio, mixing them, placing them in the melting equipment cavity, evacuating to an absolute vacuum degree ≤ 5 Pa, filling the cavity with high-purity argon, repeating the evacuation-filling with high-purity argon (gauge pressure -0.1~0 MPa) replacement 2~3 times, and melting at 1280~1420℃ for 10~15 min under an argon protective atmosphere to obtain alloy ingots or alloy sheets, and annealing at 700~1150℃ for 12~48 h; crushing and pulverizing the annealed alloy billet to obtain rare earth hydrogen storage alloy matrix powder with a particle size of 10~80 μm.
[0014] Further, in the above preparation method, step S2 specifically involves: immersing the rare earth hydrogen storage alloy matrix powder in an alkaline solution of 1.0~10.0 mol / L at 60℃~90℃ for 1~15 min, then washing with deionized water until neutral, and finally vacuum drying. More specifically, the drying temperature is 40℃~80℃, and the drying time is 1~5 h. Even more specifically, the alkaline solution is a NaOH solution.
[0015] Further, in the above preparation method, step S3 specifically involves: placing the rare earth hydrogen storage alloy matrix powder obtained in step S2 in an oxidizing atmosphere and holding it at 200~400℃ for 0.5~3 h. More specifically, the oxidizing atmosphere is selected from a mixed atmosphere composed of oxygen and argon, and the oxygen volume fraction in the mixed atmosphere is controlled to be 1~15%.
[0016] Furthermore, it also includes step S4: loading nanoscale noble metal particles onto the surface of the rare earth hydrogen storage alloy matrix powder after step S3.
[0017] Furthermore, in step S4, a liquid-phase chemical reduction method is used, specifically: the rare earth hydrogen storage alloy matrix powder is dispersed in a precursor aqueous solution, then a reducing agent is added dropwise, and the reaction is carried out by stirring at room temperature. After the reaction is completed, the solid is separated and washed with deionized water, and then vacuum dried to obtain the surface-modified rare earth hydrogen storage alloy.
[0018] Furthermore, the precursor is selected from any one of potassium tetrachloropalladium (K₂PdCl₄), palladium chloride (PdCl₂), chloroplatinic acid (H₂PtCl₆), and ruthenium trichloride (RuCl₃). The molar concentration of the aqueous solution of the precursor is 0.001~0.01 mol / L. The reducing agent is selected from at least one of sodium borohydride, hydrazine hydrate, and ascorbic acid. The molar ratio of the reducing agent to the precursor is 2:1~10:1. The reaction time is 1~3 h.
[0019] Furthermore, step S4 employs an impregnation-hydrogen thermal reduction method, specifically: the rare earth hydrogen storage alloy matrix powder is immersed in an ethanol solution of the precursor for 2-12 hours at room temperature; after impregnation, the powder, after evaporation to remove the ethanol solvent, is placed in a tube furnace, and a mixture of hydrogen and argon gas is introduced and held at 150-300°C for 1-3 hours to obtain the surface-modified rare earth hydrogen storage alloy. Furthermore, the volume fraction of hydrogen in the mixed gas is 5-10%.
[0020] In another aspect, the present invention provides an application of the above-mentioned surface-modified rare earth hydrogen storage alloy in the catalytic hydrogenation and dehydrogenation of organic liquid hydrogen carriers.
[0021] Furthermore, the hydrogenation reaction conditions are as follows: the surface-modified rare earth hydrogen storage alloy is reacted with an organic liquid hydrogen carrier at a stirring speed of 400~600 r / min, heated to 100~180℃, hydrogen pressure of 2~10 MPa, and reaction time of 0.5~10 h.
[0022] Furthermore, the dehydrogenation reaction conditions are as follows: the hydrogenated organic liquid hydrogen carrier is brought into contact with the surface rare earth hydrogen storage alloy for reaction, the stirring speed is 400~600 r / min, the vacuum is drawn to a hydrogen partial pressure of 0~0.1 MPa, the temperature is heated to 140~200℃, and the reaction time is 2~15 h.
[0023] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects: 1. This invention proposes a unique "core-shell-modification" three-layer structure for surface modification of rare earth hydrogen storage alloys. A three-layer structure with clearly defined functional zones is constructed on the surface of the alloy particles: 1) An alloy core layer that serves as both structural support and a reversible lattice hydrogen buffer. The alloy lattice interstices can store a large amount of atomic hydrogen (lattice hydrogen), which can rapidly migrate to the surface active sites during catalysis via hydrogen overflow; simultaneously, gaseous hydrogen can continuously fill lattice hydrogen vacancies, forming a dual hydrogen supply pathway; 2) A Ni-rich catalytic active shell layer located in the middle layer, providing high-density catalytic active sites; and 3) A locally distributed rare earth oxide stabilizing modification layer on the outer layer, covering part of the Ni-rich shell surface. This forms a physical barrier to inhibit high-temperature migration and aggregation of Ni particles, prevent liquid-phase impurities from corroding the matrix, and retain a large area of exposed nickel-rich active sites. The three-layer structure forms a gradient functional zone from the inside out: "hydrogen supply from the hydrogen storage matrix - catalysis from the nickel-rich layer - stabilization from the rare earth oxide." Each layer is synergistically coupled, unlike a single two-layer structure which can simultaneously achieve high activity and long-cycle stability. This synergistic structure significantly enhances catalytic activity, substantially increasing the number of surface catalytic active sites. The surface Ni atom ratio increases from 52% to over 68%, resulting in a significant improvement in hydrogenation conversion and dehydrogenation efficiency for LOHC substrates such as NEC, both exceeding 98%, and a substantial improvement in catalytic kinetics. The rare earth oxide stabilizing layer on the surface significantly enhances structural stability, effectively suppressing the migration, agglomeration, and loss of Ni active components during cycling, while also inhibiting hydrogen-induced pulverization and phase decomposition of the alloy matrix. It can stably cycle catalytically for 20-50 times or more, with an activity retention rate of ≥88%, especially when using AB. 3-4 When used in superlattice alloys, the activity retention rate is ≥90%, and the overall performance is significantly better than that of unmodified traditional nano-hydrogen storage alloys.
[0024] 2. This invention selectively dissolves the rare earth phase on the surface of the alloy through simple hot alkaline impregnation, causing metallic Ni to accumulate and reconstruct a Ni-rich crystalline shell layer on the particle surface in situ; then, a dense and ultra-thin rare earth oxide stabilizing layer is constructed on the particle surface through a low-temperature controllable in-situ oxidation process, thereby obtaining a composite surface structure of "nickel-rich active shell layer + rare earth oxide stabilizing layer", realizing the surface modification of rare earth hydrogen storage alloys. The process is controllable, with good batch consistency, and is suitable for large-scale production.
[0025] 3. The surface-modified rare-earth hydrogen storage alloy of this invention achieves synergistic catalytic function by introducing trace amounts of noble metals. Based on a core-shell structure, trace amounts of noble metals Pd, Pt, and Ru (total loading 0.5~3 wt%) are loaded, forming a dual active center of "alloy substrate + noble metal synergistic sites." The introduction of noble metals significantly reduces the adsorption activation energy of LOHC molecules, while the alloy substrate provides hydrogen transfer channels. The synergistic effect of both significantly improves catalytic efficiency, achieving a dehydrogenation selectivity of over 95%, thus achieving a synergistic unity of high activity and high selectivity. Furthermore, the noble metal loading of this invention is extremely low, as low as 0.51~0.83 wt%, only 1 / 10~1 / 6 of that used in commercial noble metal catalysts. While maintaining the same or even higher catalytic performance, the cost of catalyst raw materials is significantly reduced, giving it significant industrial competitiveness.
[0026] 4. The surface-modified rare-earth hydrogen storage alloy of this invention possesses a nickel-rich catalytically active shell, providing more catalytically active sites for LOHC hydrogenation and dehydrogenation reactions. The equilibrium hydrogen pressure of the bulk hydride in the core alloy matches the thermodynamic window of the LOHC hydrogenation and dehydrogenation reactions, allowing the reactions to proceed under milder conditions and significantly reducing the reaction temperature. Furthermore, the surface-modified rare-earth hydrogen storage alloy of this invention can achieve bidirectional catalysis of LOHC hydrogenation and dehydrogenation through simple control of hydrogen partial pressure and reaction temperature, eliminating the need for two different catalysts for hydrogenation and dehydrogenation reactions, greatly simplifying equipment and processes, and showing broad prospects for industrialization.
[0027] In this invention, the above-described technical solutions can be combined with each other to achieve more preferred combinations. Other features and advantages of this invention will be set forth in the following description, and some advantages may become apparent from the description or be learned by practicing the invention. The objectives and other advantages of this invention can be realized and obtained through the specific points highlighted in the description. Attached Figure Description
[0028] The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. Throughout the drawings, the same reference numerals denote the same parts.
[0029] Figure 1 This is a schematic diagram of the core-shell structure of the surface-modified rare earth hydrogen storage alloy of the present invention; Figure 2 SEM image of the rare earth hydrogen storage alloy in Comparative Example 1. Figure 3 This is a SEM image of the surface-modified rare-earth hydrogen storage alloy from Example 1.
[0030] Figure label: 1. Core layer; 2. Shell layer; 3. Modification layer; 4. Noble metal particles. Detailed Implementation
[0031] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of the embodiments, and are not intended to limit the scope of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Furthermore, unless otherwise specified, the raw materials mentioned below are all commercially available products; and the process steps or preparation methods not mentioned in detail are all process steps or preparation methods known to those skilled in the art.
[0032] Definitions: Conversion rate: This measures the extent to which a reaction has proceeded, referring to the percentage of all reactants that have participated in the reaction (and been consumed) out of the total initial reactants. Specifically, in the hydrogenation reaction of LOHC, the goal is to maximize hydrogen storage. To maximize hydrogen storage, the unsaturated support (such as dibenzyltoluene, H0-DBT) needs to be converted as completely as possible to its fully hydrogenated form (H18-DBT). Therefore, the main metric for the hydrogenation reaction stage of LOHC is the conversion rate.
[0033] Selectivity: A measure of the efficiency of a reaction pathway, referring to the percentage of reactants that produce the target product out of all reactants consumed. Specifically, in the dehydrogenation reaction of LOHC, the goal is to release hydrogen efficiently and purely, and the challenge lies in suppressing side reactions; therefore, selectivity is its primary metric.
[0034] Current technologies have not fully explored the catalytic potential of rare earth hydrogen storage alloys in LOHC hydrogenation and storage. To overcome their low catalytic activity and poor stability, such as... Figure 1 As shown, the present invention provides a surface-modified rare-earth hydrogen storage alloy having a core-shell structure composed of a core layer 1, a shell layer 2, and a modification layer 3; the core layer 1 has an AB5 type crystal structure or AB 3-4 The surface-modified rare-earth hydrogen storage alloy has a superlattice crystal structure; the shell layer 2 is a Ni-rich nanocrystalline shell layer, and the Ni atomic percentage of the shell layer 2 minus the Ni atomic percentage of the core layer 1 is ≥10%; the modification layer 3 is a rare-earth oxide stabilizing layer; the modification layer 3 partially covers the surface of the shell layer 2. More preferably, the surface-modified rare-earth hydrogen storage alloy further includes noble metal particles 4 loaded between the shell layer 2 and the modification layer 3; the noble metal particles 4 are at least one of Pd, Pt, and Ru.
[0035] It should be noted that the surface-modified rare-earth hydrogen storage alloy of the present invention has a unique three-layer structure of "core-shell-modification": 1) an alloy core layer that serves as both structural support and a reversible lattice hydrogen buffer, where the alloy lattice interstices can store a large amount of atomic hydrogen (lattice hydrogen). During catalysis, lattice hydrogen can rapidly migrate to the surface active sites through hydrogen overflow to participate in the reaction; simultaneously, gaseous hydrogen can continuously fill the lattice hydrogen vacancies, forming a dual hydrogen supply pathway; 2) a Ni-rich catalytic active shell layer located in the middle layer that provides high-density catalytic active sites; and 3) a locally distributed rare-earth oxide stabilizing modification layer on the outer layer, covering part of the Ni-rich shell surface, which forms a physical barrier to inhibit the high-temperature migration and aggregation of Ni particles, prevents liquid-phase impurities from corroding the matrix, and retains a large area of exposed nickel-rich active sites. Among them, the rare-earth hydrogen storage alloy core layer is located at the center of the particle and has an AB5 type crystal structure or AB 3-4 The superlattice crystal structure provides lattice hydrogen source core structure support. A Ni-rich catalytic active shell is located on the outer surface of the core. This shell is formed by selectively removing surface rare earth phases with a hot alkaline solution and then enriching the shell, with a Ni content higher than the core (Ni atomic percentage in the shell > 60%, Ni atomic percentage in the core approximately 50%). The Ni-rich shell provides a high density of catalytic active sites and exhibits strong adsorption and activation capabilities for LOHC molecules. A rare earth oxide stabilizing layer (modification layer) is located on the outer surface of the catalytic active shell, consisting of La₂O₃, CeO₂, or their composite oxides. This layer is formed through in-situ oxidation, partially covering the surface of the catalytic active shell. It inhibits the migration and aggregation of Ni particles through steric hindrance, while simultaneously regulating the electronic structure of Ni.
[0036] Specifically, the general chemical formula of the AB5 type crystal structure is R1. z1 La 1-z1 Ni 5-x1-y1 Al x1 M1 y1Where R1 is a rare earth element other than La, 0 ≤ z1 < 1; M1 is selected from at least one of Co, Cu, Mn, Fe, Sn, V, Ti, Zr, Cr, Zn, Mo, and Si, 0 ≤ x1 + y1 ≤ 1.5, 0 ≤ x1 ≤ 1, and 0 ≤ y1 ≤ 0.6. As an example, z1 can be 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, or any range between two values. The value of x1 + y1 can be 0, 0.1, 0.3, 0.5, 0.7, 0.9, 1.1, 1.3, 1.5, or any range between two values. x1 can be 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, or any range between two values; y1 can be 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, or any range between two values. More preferably, 0.1 ≤ x1 + y1 ≤ 1.5, 0 < x1 < 1, and 0 < y1 ≤ 0.6.
[0037] It should be noted that the stoichiometric ratio of the AB5 type rare earth hydrogen storage alloy crystal structure is A:B=1:5, and the crystal structure is hexagonal CaCu5 type (space group P6 / mmm).
[0038] The AB 3-4 The general chemical formula for a superlattice crystal structure is Ln x2 R2 1-x2 Ni n-z M2 z Wherein, Ln is selected from one or more of La, Ce, Pr, Nd, Sm, and Gd; R2 is selected from one or more of Y, Mg, Sm, and Gd; M2 is selected from one or more of Al, Co, Mn, Fe, Cu, Sn, Cr, and Zn, 0≤x2≤0.5, 3.0≤n≤4.0, and 0≤z≤1.5. As an example, x2 can be 0.1, 0.2, 0.3, 0.4, 0.5, or any range between two values; n can be 3.0, 3.2, 3.4, 3.5, 3.6, 3.8, 4.0, or any range between two values; z can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, or any range between two values.
[0039] It should be noted that AB 3-4 Rare earth hydrogen storage alloys include stoichiometric types AB3, A2B7, and A5B. 19 Type AB and AB4 alloys and their non-stoichiometric alloys are superlattice structures formed by the periodic stacking of [AB5] and [A2B4] subunits along the c-axis. The aforementioned AB...3-4 The general chemical formula for the superlattice rare-earth hydrogen storage alloy should be understood as follows: the A-side elements in the alloy consist of Ln and R, and the B-side elements consist of Ni and M2, and the ratio of the total molar amount of the B-side elements to the total molar amount of the A-side elements is n. The range of values for n given in the above formula is the stoichiometric range. It is understood that in some specific alloy compositions, the molar amounts of each element are not stoichiometric, such as the alloy compositions of Examples 3, 4, and 5 of this invention. The alloys La2Y4Ni in Examples 3 and 4 are shown. 19.5 Mn 0.5 In Al, the total molar fraction of elements on side A is 2 + 4 = 6, and the total molar fraction of elements on side B is 19.5 + 0.5 + 1 = 21. A simple conversion shows that the ratio of the total molar fraction of elements on side B to the total molar fraction of elements on side A is 21 / 6 = 3.5. This falls within the range of 3.0 ≤ n ≤ 4.0, indicating a non-stoichiometric ratio AB. 3-4 A superlattice rare-earth hydrogen storage alloy. Similarly, the La alloy in Example 5... 1.5 Ce 0.5 Y4Ni 20.6 Mn 1.2 In Al, the total molar fraction of elements on side A is 1.5 + 0.5 + 4 = 6, and the total molar fraction of elements on side B is 20.6 + 1.2 + 1 = 22.8. Therefore, in the alloy of Example 5, the total molar fraction of elements on side B / the total molar fraction of elements on side A = 22.8 / 6 = 3.8, which falls within the range of 3.0 ≤ n ≤ 4.0, and also belongs to the non-stoichiometric ratio AB. 3-4 Superlattice rare earth hydrogen storage alloy.
[0040] In some specific embodiments, the thickness of the shell layer is 5 to 200 nm. For example, the thickness can be 5 nm, 10 nm, 20 nm, 25 nm, 50 nm, 75 nm, 100 nm, 150 nm, or 200 nm. More preferably, the thickness of the shell layer is 10 to 100 nm.
[0041] It should be noted that the present invention regulates the appropriate thickness of the Ni-rich catalytic active shell layer to provide sufficient catalytic active sites while ensuring the catalytic function of the alloy core layer, and at the same time, avoids the formation of excessive Ni agglomeration.
[0042] In some specific embodiments, the thickness of the modification layer is 1 to 20 nm. For example, the thickness can be 1 nm, 2 nm, 4 nm, 8 nm, 10 nm, 15 nm, or 20 nm. More preferably, the thickness of the modification layer is 2 to 10 nm.
[0043] In some specific implementations, the coverage of the modification layer is 30-80%. For example, the coverage can be 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, or 80%.
[0044] It should be noted that the present invention achieves a balance between controlling the thickness and coverage of the modification layer, which enables it to suppress the migration and aggregation of Ni particles by utilizing the steric hindrance effect, while avoiding the obstruction of hydrogen transfer and catalytic reaction due to excessive oxide layer thickness.
[0045] In some preferred embodiments, such as Figure 1 The surface-modified rare earth hydrogen storage alloy also includes noble metal particles 4 loaded between the shell layer 2 and the modification layer 3; the noble metal particles 4 are at least one of Pd, Pt and Ru; the particle size of the noble metal particles 4 is 1~10 nm (e.g., 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm). The loading of the noble metal particles is 0.5 to 3 wt% of the total mass of the surface-modified rare earth hydrogen storage alloy (e.g., 0.5 wt%, 1 wt%, 1.5 wt%, 2 wt%, 2.5 wt%, 3 wt%). More preferably, the loading of the noble metal particles is 0.5 to 1.5 wt% of the total mass of the surface-modified rare earth hydrogen storage alloy.
[0046] It should be noted that by loading noble metal particles into the gap between the Ni-rich catalytic active shell and the rare earth oxide stabilizing layer, a dual active center of "alloy substrate + noble metal synergistic site" is formed. The introduction of noble metals significantly reduces the adsorption activation energy of LOHC molecules, while the alloy substrate provides hydrogen transfer channels. The two work synergistically to greatly improve catalytic efficiency.
[0047] This invention provides a method for preparing the above-mentioned surface-modified rare-earth hydrogen storage alloy, comprising the following steps: S1. Preparation of rare earth hydrogen storage alloy matrix powder; S2. The rare earth hydrogen storage alloy matrix powder is immersed in a hot alkaline solution, then washed with deionized water until neutral, and then vacuum dried. S3. The rare earth hydrogen storage alloy matrix powder processed in step S2 is subjected to oxidation treatment to obtain the surface-modified rare earth hydrogen storage alloy.
[0048] Specifically, step S1 involves preparing rare-earth hydrogen storage alloy master ingots or rare-earth hydrogen storage alloy sheets using a vacuum melting process, followed by annealing and then crushing and pulverizing to obtain the rare-earth hydrogen storage alloy matrix powder. The vacuum melting process can be either vacuum induction melting or vacuum arc melting.
[0049] More specifically, step S1 is as follows: Weigh each metal raw material according to the stoichiometric ratio, mix them and place them in the melting equipment cavity, evacuate to an absolute vacuum degree ≤5 Pa, remove impurities such as oxygen and water vapor from the cavity, and prevent rare earth metal oxidation and burn-off and the introduction of impurities and defects during high-temperature melting. After vacuuming, high-purity argon is introduced into the cavity as a protective atmosphere. The argon gauge pressure is controlled at -0.1~0 MPa (e.g., -0.1 MPa, -0.09 MPa, -0.07 MPa, -0.05 MPa, -0.03 MPa, -0.01 MPa, 0 MPa). The vacuuming and high-purity argon replacement is repeated 2~3 times. Under the argon protective atmosphere, the temperature is raised to 1280~1420℃ (e.g., 1280℃, 1300℃, 1350℃, 1380℃, 1400℃, 1420℃) and melted for 10~15 min (e.g., 10 min, 11 min, 12 min, 13 min, 14 min, 15 min) to obtain alloy ingots or alloy sheets. This ensures that all kinds of metal raw materials are fully melted and uniformly alloyed, weakens component segregation, inclusions and amorphous impurities, and improves the overall composition and structural uniformity of the alloy melt. After melting, the resulting alloy ingots or sheets are placed in a heat treatment apparatus for high-temperature homogenization annealing. The annealing temperature is 700~1150℃ (e.g., 700℃, 750℃, 800℃, 850℃, 900℃, 950℃, 1000℃, 1050℃, 1100℃, 1150℃), and the annealing time is 12~48 h (e.g., 12 h, 18 h, 25 h, 30 h, 35 h, 40 h, 48 h). This process relies on high-temperature atomic diffusion to eliminate internal stress, lattice defects, and compositional gradients generated during melting, stabilizing the intrinsic crystal structure of the alloy and fully preserving the AB5-type hexagonal CaCu5 structure or AB... 3-4 The superlattice stacking structure enhances the structural integrity and operational stability of the alloy matrix. The annealed alloy billet is then crushed and powdered using mechanical crushing-grading sieving or argon atomization processes to precisely control the particle size, resulting in rare earth hydrogen storage alloy matrix powder with a particle size of 10–80 μm (preferably 10–60 μm), uniform particle size distribution, regular morphology, and few bulk defects.
[0050] Specifically, step S2 involves immersing the rare earth hydrogen storage alloy matrix powder in an alkaline solution at 60-90℃ (e.g., 60℃, 65℃, 70℃, 75℃, 80℃, 85℃, 90℃) at a concentration of 1.0-10.0 mol / L (e.g., 1.0 mol / L, 2.0 mol / L, 3.0 mol / L, 4.0 mol / L, 5.0 mol / L, 6.0 mol / L, 7.0 mol / L, 8.0 mol / L, 9.0 mol / L, 10.0 mol / L) for 1-15 min (e.g., 1 min, 3 min, 5 min, 7 min, 9 min, 11 min, 13 min, 15 min). The original oxide layer on the alloy particle surface preferentially dissolves, followed by the preferential dissolution of the rare earth phase on the alloy surface. Ni element undergoes only minor erosion and accumulates and reconstructs in situ on the particle surface, forming a layer with a thickness of 5-200 μm. A continuous and uniform nanoporous nickel-rich shell layer of nm. The solid-liquid ratio of the rare earth hydrogen storage alloy matrix powder and the alkaline solution is 1:5 to 1:20 (g / mL). As examples, the solid-liquid ratio can be 1:5 g / mL, 1:7 g / mL, 1:10 g / mL, 1:15 g / mL, or 1:20 g / mL. Most preferably, the solid-liquid ratio is 1:10 g / mL. After impregnation, solid-liquid separation is performed, and the solid product is washed with room temperature deionized water until the washing liquid is neutral to thoroughly remove residual alkaline solution and soluble impurities. The washed powder is placed in a vacuum drying oven and vacuum dried at 40~80 °C (e.g., 40 °C, 50 °C, 60 °C, 70 °C, 80 °C) for 1~5 h (e.g., 1 h, 2 h, 3 h, 4 h, 5 h) to obtain surface nickel-rich modified hydrogen storage alloy powder. Further, the alkaline solution is NaOH solution.
[0051] It should be noted that in step S2, by precisely controlling the temperature, concentration, and immersion time of the alkaline solution, the efficient and selective dissolution of rare earth components is achieved while effectively suppressing the loss of active nickel components, thus avoiding problems such as matrix pulverization and crystal structure collapse caused by traditional high-concentration and long-term acid etching.
[0052] Specifically, step S3 involves placing the rare-earth hydrogen storage alloy matrix powder obtained in step S2 into a tube furnace or muffle furnace and holding it in an oxidizing atmosphere at 200–400°C (e.g., 200°C, 240°C, 280°C, 300°C, 350°C, 400°C) for 0.5–3 h (e.g., 0.5 h, 1 h, 1.5 h, 2 h, 2.5 h, 3 h). The oxidizing atmosphere is selected from a mixed atmosphere composed of oxygen and argon, and the oxygen volume fraction in the mixed atmosphere is controlled to be 1–15% (e.g., 1%, 5%, 10%, 15%). This invention selects this mild and low-temperature range to achieve elemental differential oxidation: the trace amounts of rare-earth La remaining on the powder surface are oxidized in situ to generate stable La2O3; if Ce is doped in the alloy system, Ce is simultaneously and preferentially oxidized to generate CeO2.
[0053] It should be noted that the present invention uses a low-temperature controllable in-situ oxidation process to construct a dense and ultra-thin rare earth oxide stabilizing layer on the particle surface, forming a composite surface structure of "nickel-rich active shell + rare earth oxide protective layer", which solves the problems of easy corrosion of active sites, easy deterioration of surface structure, and particle pulverization and shedding during the cycle of traditional modified materials.
[0054] In some preferred embodiments, step S4 is further included: loading nanoscale noble metal particles onto the surface of the rare earth hydrogen storage alloy matrix powder after step S3.
[0055] It should be noted that noble metals possess excellent hydrogen dissociation catalytic capabilities, which can lower the energy barrier of hydrogen adsorption-desorption reactions and optimize hydrogen diffusion kinetics. Synergistically enhancing with the alloy core layer, they significantly improve the catalytic efficiency of LOHC.
[0056] Specifically, step S4 can employ a liquid-phase chemical reduction method, which involves dispersing the rare-earth hydrogen storage alloy matrix powder in a precursor aqueous solution. The precursor is selected from any one of potassium tetrachloropalladate (K₂PdCl₄), palladium chloride (PdCl₂), chloroplatinic acid (H₂PtCl₆), and ruthenium trichloride (RuCl₃). The molar concentration of the precursor aqueous solution is 0.001~0.01 mol / L (e.g., 0.001 mol / L, 0.002 mol / L, 0.004 mol / L, 0.006 mol / L, 0.008 mol / L, 0.01 mol / L). The suspension is ultrasonically dispersed for 20~30 min to break up powder agglomerates, allowing noble metal ions to be uniformly adsorbed on the porous surface and inside the pores of the alloy. Subsequently, a reducing agent is slowly added dropwise to the system. The reducing agent is selected from at least one of sodium borohydride, hydrazine hydrate, and ascorbic acid. The molar ratio of the reducing agent to the precursor is controlled to be 2:1 to 10:1 (e.g., 2:1, 4:1, 6:1, 8:1, 10:1). It should be understood that the amount of reducing agent used in this invention is based on its molar ratio to the precursor. Apart from this molar ratio, this invention does not specifically limit the molar concentration of the reducing agent in the reaction system. Those skilled in the art can conventionally adjust the actual concentration of the reducing agent within the molar ratio range defined by this invention based on the amount of solvent used, the reaction temperature, and the mass transfer efficiency of the reaction system. For example, the molar concentration of the reducing agent in this invention can be 0.002 to 0.05 mol / L (e.g., 0.002 mol / L, 0.01 mol / L, 0.03 mol / L, 0.05 mol / L). The reaction is carried out at room temperature with stirring for 1 to 3 hours (e.g., 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours), during which noble metal ions are reduced in situ to elemental nanoparticles and firmly loaded onto the alloy surface. After the reaction is completed, the solid is separated by centrifugation and the solid product is washed with deionized water to completely remove residual precursors, reaction byproducts and excess reducing agent. After washing, the powder is vacuum dried at 40~70 ℃ to constant weight to obtain the surface modified rare earth hydrogen storage alloy.
[0057] Specifically, step S4 can also employ an impregnation-hydrogen thermal reduction method, which involves completely immersing the rare earth hydrogen storage alloy matrix powder in an ethanol solution containing the precursor. Utilizing the low surface tension and high permeability of ethanol, the precursor is fully impregnated into the porous structure of the alloy. The impregnation is carried out at room temperature for 2–12 h (e.g., 2 h, 4 h, 6 h, 8 h, 10 h, 12 h), thereby achieving uniform adsorption and enrichment of the precursor on the particle surface and within the pores. After impregnation, the ethanol solvent is removed by isothermal evaporation. The powder after ethanol solvent removal is placed in a tube furnace, and a mixed gas of hydrogen and argon is introduced. The volume fraction of hydrogen in the mixed gas is 5-10% (e.g., 5%, 6%, 7%, 8%, 9%, 10%). The furnace is kept at 150-300℃ (e.g., 150℃, 200℃, 250℃, 300℃) for 1-3 h (e.g., 1 h, 1.5 h, 2 h, 2.5 h, 3 h) to completely reduce the adsorbed noble metal precursor to elemental nanoparticles, achieving highly dispersed and uniform loading of the noble metal, and obtaining the surface-modified rare earth hydrogen storage alloy.
[0058] Specifically, step S4 can also employ atomic layer deposition (ALD), using Pt loading as an example: In an ALD apparatus, Pt(acac)₂ is used as the precursor, and O₃ as the co-reactant, deposition is performed at 140–250°C for 5–70 cycles. Each cycle includes: a Pt(acac)₂ pulse of 0.1–1 second, a N₂ purge of 5–20 seconds, an O₃ pulse of 0.1–5 seconds, and a N₂ purge of 5–20 seconds. It should be noted that ALD, as a mature thin film deposition process in the field, allows for parameter adjustments by those skilled in the art depending on the specific noble metal loading.
[0059] This invention provides an application of the above-mentioned surface-modified rare earth hydrogen storage alloy in catalytic hydrogenation and dehydrogenation of organic liquid hydrogen carriers.
[0060] Specifically, the hydrogenation reaction conditions are as follows: the surface-modified rare earth hydrogen storage alloy and the organic liquid hydrogen carrier are reacted in contact at a mass ratio of 1:10~100, the stirring speed is 400~600 r / min (e.g., 400 r / min, 450 r / min, 500 r / min, 550 r / min, 600 r / min), the temperature is heated to 100~180℃ (e.g., 100℃, 110℃, 120℃, 130℃, 140℃, 150℃, 160℃, 170℃, 180℃), the hydrogen pressure is 2~10 MPa (e.g., 2 MPa, 3 MPa, 4 MPa, 5 MPa, 6 MPa, 7 MPa, 8 MPa, 9 MPa, 10 MPa), and the reaction time is 0.5~10 h (0.5 h, 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h, 10 h).
[0061] Specifically, the dehydrogenation reaction conditions are as follows: the surface-modified rare earth hydrogen storage alloy is reacted with the hydrogenated organic liquid hydrogen carrier at a mass ratio of 1:10~100, the stirring speed is 400~600 r / min (e.g., 400 r / min, 450 r / min, 500 r / min, 550 r / min, 600 r / min), the vacuum is drawn to a hydrogen partial pressure of 0~0.1 MPa (e.g., 0 MPa, 0.01 MPa, 0.02 MPa, 0.04 MPa, 0.06 MPa, 0.08 MPa, 0.1 MPa), the temperature is heated to 140~200℃ (e.g., 140℃, 150℃, 160℃, 170℃, 180℃, 190℃, 200℃), and the reaction time is 2~15 h (e.g., 2 h, 4 h, 6 h, 8 h, 10 h, 12 h, 15 h).
[0062] It should be noted that the surface-modified rare-earth hydrogen storage alloy of the present invention possesses a nickel-rich catalytically active shell, providing more catalytically active sites for LOHC hydrogenation and dehydrogenation reactions. The equilibrium hydrogen pressure of the bulk hydride in the core alloy matches the thermodynamic window of the LOHC hydrogenation and dehydrogenation reactions, allowing the reactions to proceed under milder conditions and significantly reducing the reaction temperature. Furthermore, the surface-modified rare-earth hydrogen storage alloy of the present invention can achieve bidirectional catalysis of LOHC hydrogenation and dehydrogenation through simple control of hydrogen partial pressure and reaction temperature, eliminating the need for two different catalysts for the hydrogenation and dehydrogenation reactions, greatly simplifying the equipment and process.
[0063] To more clearly describe the present invention, the following embodiments and comparative examples are provided for further illustration.
[0064] Example 1 A surface-modified rare-earth hydrogen storage alloy, the preparation method of which includes the following steps: S1. Preparation of LaNi using vacuum induction melting method 4.6 Al 0.4 Alloy matrix powder: Raw materials were weighed according to the molar ratio of La:Ni:Al = 1:4.6:0.4 and placed in a vacuum induction melting furnace. The furnace was evacuated to an absolute vacuum of ≤5 Pa. After evacuation, high-purity argon gas was introduced into the chamber. This process of evacuation and argon purging was repeated three times, maintaining a relative vacuum of -0.055 MPa. The furnace was melted at 1400℃ for 15 min. The melt was then poured into a cooled copper rod and rapidly quenched to form alloy sheets. The alloy sheets were annealed at 950℃ under argon protection for 24 h. Finally, the sheets were mechanically crushed and sieved to obtain alloy powder with a particle size of 10~50 μm.
[0065] S2. Take 10 g of alloy powder and place it in 100 mL of 10 mol / L NaOH solution, and immerse it at 80℃ for 10 min. After immersion, perform solid-liquid separation, and wash the solid product with deionized water until the washing solution is neutral. Place the washed powder in a vacuum drying oven and dry it at 60℃ for 4 h.
[0066] S3. The alloy powder obtained in step S2 is placed in a tube furnace and held at 300°C in a mixed atmosphere of oxygen and argon (oxygen volume fraction of 2%) for 1 h. Surface-modified rare earth hydrogen storage alloy is obtained.
[0067] The results show that the alloy core layer prepared in Example 1 has a diameter of approximately 25 μm, a Ni-rich shell thickness of approximately 50 nm, a La2O3 stabilizing layer thickness of approximately 5 nm, and a La2O3 stabilizing layer coverage of approximately 40%. The Ni atom percentage of the alloy core layer is 52%, and the Ni atom percentage of the Ni-rich shell layer is 68%.
[0068] Catalytic performance test: 0.2g of the surface-modified rare-earth hydrogen storage alloy of this embodiment was mixed with 20g of N-ethylcarbazole (NEC) and tested in a high-pressure reactor with a stirring speed of 500 r / min. Hydrogenation reaction conditions: heating to 160℃, hydrogen pressure 6 MPa, reaction time 5 h; dehydrogenation reaction conditions: atmospheric pressure (0.1 MPa), heating to 180℃, reaction time 7 h.
[0069] The test results are as follows: Hydrogenation: NEC conversion > 99%, 12H-NEC selectivity > 98%; Dehydrogenation: Dehydrogenation efficiency > 98%, NEC selectivity > 99%. Activity retention rate after 20 cycles > 88%.
[0070] Example 2 A surface-modified rare-earth hydrogen storage alloy, the preparation method of which includes the following steps: S1. La was prepared using vacuum induction melting method. 0.8 Ce 0.2 Ni5 alloy matrix powder: Raw materials were weighed according to the molar ratio of La:Ce:Ni = 0.8:0.2:5 and placed in a vacuum induction melting furnace. The furnace was evacuated to an absolute vacuum of ≤5 Pa. After evacuation, high-purity argon gas was introduced into the furnace. This process of evacuation and argon purging was repeated three times, maintaining a relative vacuum of -0.055 MPa. The furnace was melted at 1350℃ for 15 min. The melt was then poured into a cooled copper rod and rapidly quenched to form alloy sheets. The alloy sheets were annealed at 875℃ under argon protection for 16 h. Finally, the sheets were mechanically crushed and sieved to obtain alloy powder with a particle size of 10~50 μm.
[0071] S2. Immerse 10 g of alloy powder in 100 mL of 10 mol / L NaOH solution and keep it at 80℃ for 10 min. After immersion, perform solid-liquid separation and wash the solid product with deionized water until the washing solution is neutral. Place the washed powder in a vacuum drying oven and dry it at 60℃ for 4 h.
[0072] S3. The alloy powder obtained in step S2 is placed in a tube furnace and held at 350°C in a mixed atmosphere of oxygen and argon (oxygen volume fraction of 2%) for 1.5 h to form a CeO2 / La2O3 composite oxide stabilizing layer. A surface-modified rare-earth hydrogen storage alloy is thus obtained.
[0073] Catalytic performance test: 0.2g of the surface-modified rare-earth hydrogen storage alloy of this embodiment was mixed with 20g of NEC and tested in a high-pressure reactor with a stirring speed of 500 r / min. Hydrogenation reaction conditions: heating to 160℃, hydrogen pressure 6 MPa, reaction time 4 h; dehydrogenation reaction conditions: atmospheric pressure (0.1MPa), heating to 180℃, reaction time 6 h.
[0074] The test results are as follows: Hydrogenation: NEC conversion rate > 99%, 12H-NEC selectivity > 98%; Dehydrogenation: Dehydrogenation efficiency > 98%. Activity retention rate after 30 cycles > 93%.
[0075] This indicates that the introduction of CeO2 further improves antioxidant capacity and thermal stability.
[0076] Example 3 A surface-modified rare-earth hydrogen storage alloy, the preparation method of which includes the following steps: S1. Preparation of La2Y4Ni by vacuum induction melting method 19.5 Mn 0.5 Al alloy matrix powder: Raw materials were weighed according to the molar ratio of La:Y:Ni:Mn:Al = 2:4:19.5:0.5:1 and placed in a vacuum induction melting furnace. The furnace was evacuated to an absolute vacuum of ≤5 Pa. After evacuation, high-purity argon gas was introduced into the furnace. This process of evacuation and argon purging was repeated three times, maintaining a relative vacuum of -0.055 MPa. The furnace was melted at 1400℃ for 15 min. The melt was then poured into a cooled copper rod and rapidly quenched to form alloy sheets. The alloy sheets were annealed at 950℃ under argon protection for 36 h. Finally, the sheets were mechanically crushed and sieved to obtain alloy powder with a particle size of 10~50 μm.
[0077] S2. Take 10 g of alloy powder and place it in 100 mL of 10 mol / L NaOH solution. Immerse it at 80 °C for 10 min. After immersion, perform solid-liquid separation and wash the solid product with deionized water until the washing solution is neutral. Place the washed powder in a vacuum drying oven and dry it at 60 °C for 4 h.
[0078] S3. The alloy powder obtained in step S2 is placed in a tube furnace and held at 250°C in a mixed atmosphere of oxygen and argon (oxygen volume fraction of 2%) for 2 hours to obtain a surface-modified rare earth hydrogen storage alloy.
[0079] Catalytic performance test: 0.2g of the surface-modified rare-earth hydrogen storage alloy of this embodiment was mixed with 20g of NEC and tested in a high-pressure reactor with a stirring speed of 500 r / min. Hydrogenation reaction conditions: heating to 150℃, hydrogen pressure 6 MPa, reaction time 4 h; dehydrogenation reaction conditions: atmospheric pressure (0.1MPa), heating to 170℃, reaction time 6 h.
[0080] The test results are as follows: Hydrogenation: NEC conversion > 99%, 12H-NEC selectivity > 98%; Dehydrogenation: Dehydrogenation efficiency > 97%, NEC selectivity > 98.5%. Activity retention rate > 90% after 40 cycles.
[0081] Example 4 In this embodiment, after preparing the alloy powder according to the method of Example 3 (steps S1~S3), step S4 is further included: 2.0 g of alloy powder is dispersed in 100 mL of a 0.001 mol / L K2PdCl4 precursor aqueous solution, ultrasonically dispersed for 20 min, and 0.05 mol / L NaBH4 solution is slowly added dropwise, controlling the molar ratio of reducing agent to precursor to be 8:1, and reacted at room temperature for 2 h. After the reaction is completed, the solid is separated by centrifugation and washed three times with deionized water, and vacuum dried at 60℃ to constant weight to obtain a surface-modified rare earth hydrogen storage alloy 0.53 wt% Pd / La2Y4Ni. 19.5 Mn 0.5 Al.
[0082] Catalytic performance test: 0.2g of the surface-modified rare-earth hydrogen storage alloy of this embodiment was mixed with 20g of NEC and tested in a high-pressure reactor with a stirring speed of 500 r / min. The hydrogenation reaction conditions were: heating to 160℃, hydrogen pressure 6 MPa, and reaction time 4.5 h; the dehydrogenation reaction conditions were: atmospheric pressure (0.1MPa), heating to 175℃, and reaction time 6 h.
[0083] The test results were as follows: Hydrogenation: NEC conversion rate > 99%; Dehydrogenation: Dehydrogenation efficiency > 97%. Although the Pd content was only 60% of that in Comparative Example 5 (0.83 wt% Pd / LaNi5), the catalytic activity was similar, indicating that AB... 3-4 The superlattice alloy substrate and trace amounts of Pd exhibit a good synergistic effect. After 20 cycles, the activity retention rate is >92%.
[0084] Example 5 A surface-modified rare-earth hydrogen storage alloy, the preparation method of which includes the following steps: S1. La was prepared using vacuum induction melting method. 1.5 Ce 0.5 Y4Ni 20.6 Mn 1.2 Al alloy matrix powder: Raw materials were weighed according to the molar ratio of La:Ce:Y:Ni:Mn:Al = 1.5:0.5:4:20.6:1.2:1 and placed in a vacuum induction melting furnace. The furnace was evacuated to an absolute vacuum of ≤5 Pa. After evacuation, high-purity argon gas was introduced into the furnace. This process of evacuation and argon purging was repeated three times, maintaining a relative vacuum of -0.055 MPa. The furnace was melted at 1400℃ for 15 min. The melt was then poured into a cooled copper rod and rapidly quenched to form alloy sheets. The alloy sheets were annealed at 900℃ under argon protection for 24 h. Finally, the sheets were mechanically crushed and sieved to obtain alloy powder with a particle size of 10~50 μm.
[0085] S2. Take 10 g of alloy powder and place it in 100 mL of 10 mol / L NaOH solution. Immerse it at 80 °C for 10 min. After immersion, perform solid-liquid separation and wash the solid product with deionized water until the washing solution is neutral. Place the washed powder in a vacuum drying oven and dry it at 60 °C for 4 h.
[0086] S3. Place the alloy powder obtained in step S2 into a tube furnace and heat it at 300°C in a mixed atmosphere of oxygen and argon (oxygen volume fraction of 2%) for 1 h.
[0087] S4. Pt loading using atomic layer deposition (ALD): In an ALD apparatus, Pt(acac)₂ was used as the precursor and O₃ as the co-reactant. Deposition was performed for 10 cycles at 250°C. Each cycle consisted of: a Pt(acac)₂ pulse for 0.5 seconds, a N₂ purge for 10 seconds, an O₃ pulse for 1 second, and a N₂ purge for 10 seconds. Surface-modified rare-earth hydrogen storage alloys were obtained.
[0088] Catalytic performance test: 0.2g of the surface-modified rare-earth hydrogen storage alloy of this embodiment was mixed with 20g of N-propylcarbazole (NPC) and tested in a high-pressure reactor with a stirring speed of 500 r / min. Hydrogenation reaction conditions: heating to 150℃, hydrogen pressure 5 MPa, reaction time 5 h; dehydrogenation reaction conditions: atmospheric pressure (0.1 MPa), heating to 170℃, reaction time 7 h.
[0089] The test results are as follows: Hydrogenation: NPC conversion rate > 98%; Dehydrogenation: Dehydrogenation efficiency > 96%. Activity retention rate > 90% after 25 cycles.
[0090] Comparative Example 1 A rare earth hydrogen storage alloy is prepared by the following steps: preparing LaNi using a vacuum induction melting method. 4.6 Al 0.4 Alloy matrix powder: Raw materials were weighed according to the molar ratio of La:Ni:Al = 1:4.6:0.4 and placed in a vacuum induction melting furnace. The furnace was evacuated to an absolute vacuum of ≤5 Pa. After evacuation, high-purity argon gas was introduced into the furnace. This process of evacuation and argon purging was repeated three times, maintaining a relative vacuum of -0.055 MPa. The furnace was melted at 1400℃ for 15 min. The melt was then poured into a cooled copper rod and rapidly quenched to form alloy sheets. The alloy sheets were annealed at 950℃ under argon protection for 24 h. Finally, the sheets were mechanically crushed and sieved to obtain rare-earth hydrogen storage alloy powder with a particle size of 10~50 μm.
[0091] The results show that the percentage of Ni atoms on the alloy surface is 52%, which is much lower than the 68% percentage of Ni atoms on the surface-modified rare earth hydrogen storage alloy surface in Example 1.
[0092] Compare Figure 2 (Comparative Example 1) and Figure 3 The SEM image of Example 1 shows that the alloy powder of Comparative Example 1, which has not undergone surface modification, has a smooth surface. After surface modification, the surface of the alloy powder in Example 1 becomes rough, and the surface layer is covered with needle-like rare earth oxides.
[0093] Catalytic performance test results showed that, under the same reaction conditions as in Example 1 and with the same stirring speed, the NEC hydrogenation conversion rate in this comparative example was only 85%, and the dehydrogenation efficiency was only 68%, both significantly lower than in Example 1. This indicates that the Ni-rich shell formed after surface modification treatment can significantly improve catalytic activity.
[0094] Comparative Example 2 A surface-modified rare-earth hydrogen storage alloy, the preparation method of which includes the following steps: S1. La was prepared using vacuum induction melting method. 0.8 Ce 0.2Ni5 alloy matrix powder: Raw materials were weighed according to the molar ratio of La:Ce:Ni = 0.8:0.2:5 and placed in a vacuum induction melting furnace. The furnace was evacuated to an absolute vacuum of ≤5 Pa. After evacuation, high-purity argon gas was introduced into the furnace. This process of evacuation and argon purging was repeated three times, maintaining a relative vacuum of -0.055 MPa. The furnace was melted at 1350℃ for 15 min. The melt was then poured into a cooled copper rod and rapidly quenched to form alloy sheets. The alloy sheets were annealed at 875℃ under argon protection for 16 h. Finally, the sheets were mechanically crushed and sieved to obtain alloy powder with a particle size of 10~50 μm.
[0095] S2. Take 10 g of alloy powder and immerse it in 100 mL of 10 mol / L NaOH solution. Immerse at 80℃ for 10 min. After immersion, perform solid-liquid separation and wash the solid product with deionized water until the washing solution is neutral. Place the washed powder in a vacuum drying oven and dry at 60℃ for 4 h to obtain the surface-modified rare earth hydrogen storage alloy.
[0096] Catalytic performance test results show that, under the same reaction conditions and stirring speed as in Example 2, the NEC conversion rate in this comparative example is 95%, and the dehydrogenation efficiency is 93%. After 30 cycles, the activity retention rate is 86%. The alloy particles in this comparative example have a Ni-rich catalytically active shell on their core surface, but this shell is not oxidized, and the shell surface is not covered with a rare earth oxide stabilizing modification layer. Therefore, during high-temperature hydrogenation and dehydrogenation cycles, the active nickel sites are prone to oxidation and deactivation, surface carbon accumulation, and particle agglomeration and detachment. Simultaneously, the alloy matrix is easily oxidized and corroded, significantly reducing the material's catalytic selectivity, hydrogen storage efficiency, and cycle stability. This demonstrates that the shell and modification layer of the core-shell structure of this invention are indispensable and work synergistically to produce a technical effect greater than the sum of its parts (1+1>2).
[0097] Comparative Example 3 Comparative Example 3 used a commercially available 5 wt% Pd / Al2O3 catalyst to replace the surface-modified rare earth hydrogen storage alloy 0.53 wt% Pd / La2Y4Ni in Example 4. 19.5 Mn 0.5 Al alloy. Hydrogenation and dehydrogenation efficiencies were tested under the same reaction conditions as in Example 4. The results showed that the dehydrogenation efficiency of Comparative Example 3 was >99%, but the Pd loading was approximately 10 times that of the catalyst in Example 4 of this invention, resulting in higher catalyst costs. After 30 cycles, the Pd nanoparticles underwent significant sintering, with an activity decrease of approximately 15%. This demonstrates that the core-shell structure catalyst of this invention has significant advantages in reducing the amount of precious metals used, lowering costs, and improving cycle stability.
[0098] Comparative Example 4 A rare earth hydrogen storage alloy is prepared by the following steps: LaNi5 alloy matrix powder is prepared by molten salt-assisted CaH2 reduction method according to existing technology: Lanthanum chloride heptahydrate LaCl3·7H2O and nickel chloride hexahydrate NiCl2·6H2O are dissolved in deionized water at a La:Ni molar ratio of 1:5.5, NaOH is added to form a hydroxide precipitate, the precipitate is dried and mixed with excess KCl and CaH2, and reduced at 973 K under argon atmosphere for 2 h. The precipitate is washed with 0.1 mol / L dilute acetic acid to obtain LaNi5 nanoparticles of about 100 nm.
[0099] The rare-earth hydrogen storage alloy prepared in this comparative example was subjected to hydrogenation and dehydrogenation tests under the same reaction conditions as in Example 1. The results showed that the NEC conversion rate of this comparative example was approximately 85%, and the dehydrogenation efficiency was approximately 78%, both lower than that of Example 1. After three cycles, nano-LaNi5 exhibited significant phase decomposition, while the catalysts in Examples 1-5 of this invention maintained a stable alloy main phase even after 20 cycles. This indicates that the surface modification process of this invention plays a crucial role in improving catalytic performance and stability.
[0100] Comparative Example 5 A method for preparing a Pd-supported surface-modified rare-earth hydrogen storage alloy includes the following steps: S1. LaNi5 alloy matrix powder was prepared by molten salt-assisted CaH2 reduction method according to existing technology: LaCl3·7H2O and NiCl2·6H2O were dissolved in deionized water at a molar ratio of La:Ni = 1:5.5. NaOH was added to form a hydroxide precipitate. After drying, the precipitate was mixed with excess KCl and CaH2 and reduced at 973 K under argon atmosphere for 2 h. The powder was washed with 0.1 mol / L dilute acetic acid to obtain LaNi5 nanoparticles with a size of about 100 nm.
[0101] S2. Disperse 200 mg of LaNi5 nanoparticles in 3.00 mL of deionized water and stir at low speed; slowly add 0.0432 mol / L K2PdCl4 solution and continue stirring until the deep orange color completely disappears. The product is centrifuged, washed with deionized water and ethanol, and vacuum dried at room temperature for 12 h. A 0.83 wt% Pd-supported surface-modified rare earth hydrogen storage alloy is obtained. The particle size range of the Pd nanoparticles supported on the alloy surface is 3–5 nm.
[0102] Catalytic performance testing was conducted: 0.2g of the surface-modified rare-earth hydrogen storage alloy of this embodiment was mixed with 20g of NEC and tested in a high-pressure reactor with a stirring speed of 500 r / min. Hydrogenation reaction conditions: heating to 160℃, hydrogen pressure 6 MPa, reaction time 3 h; dehydrogenation reaction conditions: atmospheric pressure (0.1 MPa), heating to 160℃, reaction time 5 h. Before each catalytic reaction, the alloy catalyst was vacuum heat-treated at 343 K for 4 h to stabilize the Pd / LaNi5 interface.
[0103] Test results: Hydrogenation: NEC conversion > 99%; Dehydrogenation: Dehydrogenation efficiency > 98%, NEC selectivity > 98.5%. Activity retention rate after 20 cycles > 85%. Compared with Example 1, the dehydrogenation temperature was reduced by 20°C and the reaction time was shortened by 1 h, but the activity retention rate dropped to 85% after 20 cycles, and the long-term cycling stability was weaker than that of the core-shell modified catalyst in Example 1.
[0104] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.
Claims
1. A surface-modified rare-earth hydrogen storage alloy, characterized in that, It has a core-shell structure consisting of a core layer, a shell layer, and a modification layer; the core layer has an AB5 type crystal structure or AB 3-4 The superlattice crystal structure is described; the shell is a Ni-rich nanocrystalline shell, and the Ni atom percentage of the shell minus the Ni atom percentage of the core layer is ≥10%; the modification layer is a rare earth oxide stabilizing layer; the modification layer partially covers the surface of the shell. The general chemical formula of the AB5 type crystal structure is R1. z1 La 1-z1 Ni 5-x1-y1 Al x1 M1 y1 Where R1 is a rare earth element other than La, 0≤z1<1; M1 is selected from at least one of Co, Cu, Mn, Fe, Sn, V, Ti, Zr, Cr, Zn, Mo and Si, 0≤x1+y1≤1.5, 0≤x1≤1, 0≤y1≤0.6; The AB 3-4 The general chemical formula for a superlattice crystal structure is Ln x2 R2 1-x2 Ni n-z M2 z Wherein, Ln is selected from one or more of La, Ce, Pr, Nd, Sm, and Gd; R2 is selected from one or more of Y, Mg, Sm, and Gd; M2 is selected from one or more of Al, Co, Mn, Fe, Cu, Sn, Cr, and Zn, 0≤x2≤0.5, 3.0≤n≤4.0, and 0≤z≤1.
5.
2. The surface-modified rare-earth hydrogen storage alloy according to claim 1, characterized in that, The thickness of the shell is 5~200 nm.
3. The surface-modified rare-earth hydrogen storage alloy according to claim 1, characterized in that, The thickness of the modified layer is 1~20 nm.
4. The surface-modified rare-earth hydrogen storage alloy according to claim 1, characterized in that, The coverage of the modified layer is 30-80%.
5. A surface-modified rare-earth hydrogen storage alloy according to claim 1, characterized in that, The surface-modified rare-earth hydrogen storage alloy further includes noble metal particles loaded between the shell layer and the modification layer; the noble metal particles are at least one of Pd, Pt and Ru; the particle size of the noble metal particles is 1~10 nm. The loading of the precious metal particles is 0.5 to 3 wt% of the total mass of the surface-modified rare earth hydrogen storage alloy.
6. A method for preparing a surface-modified rare-earth hydrogen storage alloy according to any one of claims 1 to 5, characterized in that, Includes the following steps: S1. Preparation of rare earth hydrogen storage alloy matrix powder; S2. The rare earth hydrogen storage alloy matrix powder is immersed in a hot alkaline solution, then washed with deionized water until neutral, and then vacuum dried. S3. The rare earth hydrogen storage alloy matrix powder processed in step S2 is subjected to oxidation treatment to obtain the surface-modified rare earth hydrogen storage alloy.
7. The preparation method according to claim 6, characterized in that, Step S2 specifically involves immersing the rare earth hydrogen storage alloy matrix powder in an alkaline solution of 1.0 to 10.0 mol / L at 60°C to 90°C for 1 to 15 minutes, then washing it with deionized water until neutral, and finally vacuum drying it.
8. The preparation method according to claim 6, characterized in that, Step S3 specifically involves placing the rare earth hydrogen storage alloy matrix powder obtained in step S2 in an oxidizing atmosphere and holding it at 200~400℃ for 0.5~3 h.
9. The preparation method according to claim 6, characterized in that, It also includes step S4: loading nanoscale noble metal particles onto the surface of the rare earth hydrogen storage alloy matrix powder after step S3.
10. The application of a surface-modified rare-earth hydrogen storage alloy according to any one of claims 1 to 5 or a surface-modified rare-earth hydrogen storage alloy obtained by the preparation method according to any one of claims 6 to 9 in the catalytic hydrogenation and dehydrogenation of organic liquid hydrogen carriers.