A method for photothermal-driven methane cracking reaction
By using a high-entropy alloy catalyst supported on SrTiO3 and irradiating it with focused sunlight in a mobile phase reactor, CH4 was converted into H2 with high efficiency and selectivity under mild conditions. This solves the problems of high energy consumption at high temperatures and low catalyst selectivity in existing technologies and has good prospects for industrial application.
Patent Information
- Application Number
- CN202611440118.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-16
- Publication Date
- 2026-11-17
AI Technical Summary
Existing methane cracking technologies suffer from high energy consumption, numerous side reactions, and low catalyst selectivity under high-temperature conditions, making it difficult to efficiently produce H2 under mild conditions.
Using a high-entropy alloy catalyst supported on strontium titanate (SrTiO3), CH4 is converted into C+H2 at room temperature in a mobile phase reactor by irradiation with focused sunlight.
It achieves efficient H2 production under mild conditions, with a generation rate of over 1.1 mol g⁻¹ h⁻¹ and a selectivity of over 99%. The catalyst has good stability, can be reused, and reduces energy consumption and production costs.
Smart Images

Figure CN123105550A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of photothermal synergistic catalysis technology, specifically to a method for photothermal-driven methane cracking reaction. Background Technology
[0002] Natural gas is both a high-quality clean energy source and a key chemical raw material. In the face of increasingly severe environmental challenges, its clean and environmentally friendly characteristics are attracting significant attention compared to other fossil fuels such as coal and oil. Methane cracking (MP) technology can efficiently convert natural gas, whose main component is CH4, into high-calorific-value hydrogen. This process not only mitigates the greenhouse effect but also improves energy efficiency. However, the highly symmetrical structure of methane molecules, with an average CH bond energy of 440 kJ / mol, typically requires temperatures above 900℃ to drive the conversion reaction. This not only results in enormous energy consumption but also significant environmental pollution. Furthermore, under these extreme high-temperature conditions, side reactions such as methanation are thermodynamically unavoidable, leading to a decrease in catalyst selectivity. Considering the costs of industrial production, the energy crisis, and environmental pollution, there is an urgent need to develop new methods for MP technology that are greener, more environmentally friendly, have milder reaction conditions, and higher selectivity. Summary of the Invention
[0003] The purpose of this invention is to provide a method for photothermal-driven methane cracking reaction, solving the problem of how to achieve efficient, highly selective, and highly stable H2 preparation under mild conditions.
[0004] To achieve the above objectives, the present invention provides the following technical solution:
[0005] A novel photothermal-driven MP reaction method comprises: using a high-entropy alloy supported on strontium titanate (SrTiO3) as a catalyst, in a mobile phase reactor, under focused sunlight irradiation, converting the greenhouse gas CH4 into C+H2 at room temperature.
[0006] In a preferred embodiment, the feed gas can be derived from pure CH4 gas or from a CH4-containing gas mixture. The term "CH4-containing gas" refers to a gas mixture containing CH4. Alternatively, the feed gas can also be derived directly from methane hydrate, shale gas, and natural gas. Preferably, the gas contains more than 10% CH4 by volume.
[0007] In a preferred embodiment, the flow rate of the CH4 gas is 5-60 mL / min. Preferably, the CH4 gas flow rate is 10 mL / min.
[0008] In a preferred embodiment, the carrier SrTiO3 can be a commercially available, inexpensive SrTiO3, or SrTiO3 with a specific structure can be synthesized according to experimental needs.
[0009] In a preferred embodiment, the catalyst support includes, but is not limited to, SrTiO3. Other commercial oxides may be used instead of SrTiO3, such as TiO2, LaFeO3, MgO, Al2O3, SiO2, BaTiO3, etc. Commercially available SrTiO3 is preferred as the support.
[0010] In a preferred embodiment, the high-entropy alloy of the carrier includes, but is not limited to, Co, Fe, Ni, Cu, Ru, Rh, Pd, Pt, Ir, etc. A preferred composition is a high-entropy alloy of FeNiRhRuPd.
[0011] In a preferred embodiment, the molar ratio of the high-entropy alloy and SrTiO3 supported in the catalyst is 0.005~0.1:1. More preferably, the molar ratio of the high-entropy alloy and SrTiO3 supported in the catalyst is 0.05:1.
[0012] In a preferred embodiment, the illuminance of the illumination conditions is 10–4000 mW / cm². 2 The preferred light intensity is 4000 mW / cm². 2 .
[0013] In a preferred embodiment, the light source used for the illumination conditions is one or more selected from natural light, xenon lamps, LED lamps, tungsten lamps, and mercury lamps. Preferably, the light source for the illumination conditions is natural light.
[0014] In a preferred embodiment, the reaction temperature is 20–400 °C. o C. Preferably, the reaction temperature is 25°C. o C.
[0015] The reaction can run for 0–200 hours. Preferably, the reaction can run for 100 hours.
[0016] In a preferred embodiment, the reactor is a quartz reactor, a glass reactor, a fixed-bed reactor, or a mobile phase reactor. Preferably, the reactor is a mobile phase reactor.
[0017] In a preferred embodiment, the pressure of the CH4 gas in the reactor is 0.1 MPa to 10 MPa. Preferably, the pressure of the CH4 gas in the reactor is 0.1 MPa.
[0018] The beneficial effects of this invention are as follows: This application utilizes a high-entropy alloy supported on SrTiO3 as a catalyst, enabling efficient driving of the MP reaction in a mobile phase reactor using only focused sunlight irradiation. CH4 gas is converted to C+H2 under mild conditions, with a H2 production rate as high as 1.1 mol g. -1 h -1 The selectivity is greater than 99%. The product contains no CO or aromatic hydrocarbons and can be directly used for daily energy consumption. The catalyst has high stability and can operate stably for more than 200 hours.
[0019] The high-entropy alloy catalyst developed in this invention exhibits excellent photothermal conversion efficiency, and the local surface temperature of the catalyst can reach as high as 500°C under focused solar radiation. o C can efficiently drive the MP reaction under mild conditions. This process not only helps mitigate the greenhouse effect but also improves energy efficiency, significantly reducing production costs and energy consumption.
[0020] Furthermore, the method of this invention has advantages such as simple reaction process, short cycle, inexpensive and readily available catalyst that can be reused. It represents a novel synthetic route for the MP reaction and has broad prospects for industrial application.
[0021] The above description is merely an overview of the technical solution of the present invention. In order to better understand the technical means of the present invention and to implement it in accordance with the contents of the specification, the preferred embodiments of the present invention are described in detail below with reference to the accompanying drawings. Attached Figure Description
[0022] Figure 1 This is a schematic diagram illustrating the H2 generation rate and selectivity obtained by the present invention.
[0023] Figure 2 This is a diagram illustrating the effect of reusing the SrTiO3-supported high-entropy alloy catalyst of this invention. Detailed Implementation
[0024] The technical solution of the present invention will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0025] In the description of this invention, it should be noted that the terms "center," "upper," "lower," "left," "right," "vertical," "horizontal," "inner," and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing the invention and for simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the invention. Furthermore, the terms "first," "second," and "third" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.
[0026] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection of two components. Those skilled in the art can understand the specific meaning of the above terms in this invention based on the specific circumstances.
[0027] Furthermore, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0028] This invention screens high-entropy alloy catalysts with strong CH bond dissociation and photothermal conversion capabilities. The components of the high-entropy alloy include, but are not limited to, Co, Fe, Ni, Cu, Ru, Rh, Pd, Pt, and Ir. Using supported high-entropy alloys as catalysts, highly efficient, selective, and stable MP reaction for H2 production was achieved under focused sunlight.
[0029] The photothermal driven MP reaction method of the present invention includes: using a high-entropy alloy supported on SrTiO3 as a catalyst, in a mobile phase reactor, under focused sunlight irradiation, converting greenhouse gas CH4 into H2 at room temperature.
[0030] In the method of this invention, the only product after the reaction is complete is H2. No additional separation step is required, and it can be directly used for daily energy consumption.
[0031] In the method of this invention, after the reaction is complete, the conversion rate of the feed gas CH4 and the generation rate and selectivity of the product H2 can be detected by conventional means, such as, but not limited to, gas chromatography (GC). The stability of the catalyst can be assessed by long-term operation under operating conditions.
[0032] In the method of this invention, commercially available SrTiO3 can be directly purchased as a catalyst support, or a SrTiO3 support can be synthesized as needed. The metal salt used can be one or more of nitrates, chlorides, and acetates. Other commercial oxides can also be used instead of SrTiO3, such as TiO2, LaFeO3, MgO, Al2O3, SiO2, BaTiO3, etc.
[0033] In the method of this invention, the catalyst used is a high-entropy alloy-supported SrTiO3 compound. SrTiO3, as the base material in the catalyst of this invention, is not only widely available and inexpensive, but also possesses excellent optical properties, chemical stability, thermal stability, superhydrophilicity, and non-migratory properties. Furthermore, the inventors have discovered that, during the catalyst preparation process, by simply loading a high-entropy alloy, the obtained high-entropy alloy-supported SrTiO3 compound can serve as a highly efficient catalyst to selectively convert CH4 gas or CH4 containing CH4 into H2 under specific reaction conditions. In addition, the inventors have also found that the high-entropy alloy-supported SrTiO3 catalyst used exhibits excellent stability, capable of stable operation for over 200 hours under operating conditions, thus making the entire process of this invention highly promising for industrial applications.
[0034] In the method of the present invention, preferably, the molar ratio of the high-entropy alloy and SrTiO3 supported in the catalyst is 0.05:1.
[0035] In the method of this invention, the feed gas used can be derived from pure CH4 gas or from a CH4-containing gas. The term "CH4-containing gas" refers to a gas mixture containing CH4. Preferably, the gas contains more than 10% CH4 by volume.
[0036] In the method of the present invention, although there is no particular limitation on the pressure of CH4 gas or CH4-containing gas in the reactor, it is preferred that the pressure of CH4 gas or CH4-containing gas in the reactor is 0.1 MPa to 10 MPa.
[0037] In the method of the present invention, preferably, the light intensity of the illumination conditions used can be 10–4000 mW / cm². 2 The preferred light intensity is 4000 mW / cm². 2 .
[0038] In the method of the present invention, there are no particular limitations on the light source used for illumination conditions, as long as it can emit light radiation. Preferably, the light source used for illumination conditions can be one or more selected from focused sunlight, xenon lamps, LED lamps (i.e., light-emitting diodes), tungsten lamps, and mercury lamps.
[0039] In the method of this invention, the reaction temperature of the reactor is typically 20–500°C; preferably, the reaction temperature used can be 20–500°C, and most preferably, the reaction is carried out at room temperature (i.e., about 25–30°C). If necessary, the reactor can be heated to the desired reaction temperature by conventional means such as heating wires or heating mantles.
[0040] In the method of the present invention, from an efficiency point of view, the reaction can typically run stably for 0-200 h, and more preferably for a continuous running time of 100 h.
[0041] In the method of this invention, there are no particular limitations on the reactor used, as long as it is a container that can withstand a certain pressure and can be sealed. For example, the reactor used can be a quartz reactor, a glass reactor, a fixed-bed reactor, or a flowable reactor. Preferably, the reactor is a mobile phase reactor.
[0042] In the method of this invention, there are no particular limitations on the catalyst support used. The catalyst support may include, but is not limited to, SrTiO3, and may also be TiO2, LaFeO3, MgO, Al2O3, SiO2, BaTiO3, etc. Commercially available SrTiO3 is preferred as the support.
[0043] In the method of this invention, there are no particular limitations on the high-entropy alloy used, and the composition of the high-entropy alloy may include Co, Fe, Ni, Cu, Ru, Rh, Pd, Pt, Ir, etc. Preferably, the high-entropy alloy used is FeNiRhRuPd.
[0044] The present invention will be further described below with reference to specific embodiments. These descriptions are merely preferred embodiments of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention are included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.
[0045] Unless otherwise stated, there are no particular restrictions on the source of all raw materials used in this invention, and all of them are commercially available; at the same time, there are no particular restrictions on their purity, but analytical grade is preferred in this invention.
[0046] This invention does not impose any particular limitations on the reaction or detection equipment or apparatus used; any conventional equipment or apparatus known to those skilled in the art can be used as long as the objective can be achieved.
[0047] Catalyst preparation
[0048] The catalyst used in this invention is prepared as follows, taking SrTiO3 supported by a high-entropy alloy as an example:
[0049] Add 2.3 g SrTiO3 and 200 mL deionized water to a 500 mL glass beaker, stir vigorously for 30 min, then add 5 mL of 10 mM solution of each metal precursor. After stirring at room temperature for 1 hour, transfer the resulting mixture to a 100 mL incubator. o The sample was evaporated overnight at C to completely remove deionized water. Then, the resulting sample was subjected to evaporation at 400°C in a 10% H₂ / 90% Ar atmosphere. o Calcination at C for 2 hours (heating rate 5) o C min -1 Finally, the catalyst was naturally cooled to room temperature to obtain a high-entropy alloy-supported TiO2 catalyst. The molar ratio of the high-entropy alloy and SrTiO3 supported in the catalyst was 0.05:1.
[0050] Based on the same procedure described above, only the amount of metal precursor used is changed accordingly, thereby obtaining a molar ratio of SrTiO3 supported on a high-entropy alloy of 0.005~0.1:1.
[0051] Based on the same procedure described above, only the type of metal precursor used is changed accordingly, thereby obtaining SrTiO3 catalysts with different high-entropy alloy supports, including but not limited to FeNiRhRuPt / SrTiO3, CoNiRhRuPd / SrTiO3, CoNiRhRuPt / SrTiO3, FeNiRhPdPt / SrTiO3, CoNiRhPdPt / SrTiO3, FeNiRhIrPd / SrTiO3, etc.
[0052] Based on the same procedure described above, other high-entropy alloy-supported catalysts with the same metal loading were prepared by using oxide materials such as TiO2, LaFeO3, MgO, Al2O3, SiO2, and BaTiO3 instead of SrTiO3 as the support material.
[0053] Example 1
[0054] In a mobile phase reactor (which is controlled by a stainless steel valve and can apply a maximum pressure of 20 MPa), 100 mg of a high-entropy alloy-supported SrTiO3 catalyst (FeNiRhRuPd / SrTiO3, where the molar ratio of FeNiRhRuPd to SrTiO3 is 0.05:1) was added as a catalyst. A steel cylinder containing 10% CH4 / 90% Ar was introduced into the mobile phase reactor via a pressure reducing valve. The pressure inside the reactor was atmospheric pressure, and the flow rate of CH4 was 10 mL / min. -1 The total flow rate was 10 mL / min. -1 At room temperature (approximately 25°C) oUnder condition C), using focused sunlight as the light source, at 4000 mW / cm²... 2 The reaction was carried out under irradiation with light intensity. The product H2 was evaluated using an online gas chromatograph (GC-2014ATFSPL, Ar carrier, Shimadzu) equipped with two flame ionization detectors (FID) and one thermal conductivity detector (TCD). The product was determined by gas chromatography to be H2, with a formation rate of 1.1 mol g. -1 h -1 above( Figure 1 a) Selectivity is above 99% ( Figure 1 (b) In addition, the catalyst can operate stably continuously for more than 200 hours. Considering the product formation rate, selectivity, and catalyst stability, it clearly has the potential for industrial application.
[0055] Example 2
[0056] The specific reaction process and detection method were the same as in Example 1, except that FeNiRhRuPd / TiO2 was used instead of FeNiRhRuPd / SrTiO3 as the catalyst. The formation rate of the target product H2 was measured to be 0.7 mol g. −1 h −1 The selectivity rate was 96%.
[0057] Example 3
[0058] The specific reaction process and detection method were the same as in Example 1, with FeNiRhRuPd / LaFeO3 replacing FeNiRhRuPd / SrTiO3 as the catalyst. The formation rate of the target product H2 was measured to be 0.8 mol g. −1 h −1 The selectivity rate was 94%.
[0059] Example 4
[0060] The specific reaction process and detection method were the same as in Example 1, with FeNiRhRuPd / MgO replacing FeNiRhRuPd / SrTiO3 as the catalyst. The generation rate of the target product H2 was measured to be 0.5 mol g. −1 h −1 The selectivity rate was 91%.
[0061] Example 5
[0062] The specific reaction process and detection method were the same as in Example 1, with FeNiRhRuPd / Al2O3 replacing FeNiRhRuPd / SrTiO3 as the catalyst. The generation rate of the target product H2 was measured to be 0.6 mol g. −1 h−1 The selectivity rate is 98%.
[0063] Example 6
[0064] The specific reaction process and detection method were the same as in Example 1, with FeNiRhRuPd / BaTiO3 replacing FeNiRhRuPd / SrTiO3 as the catalyst. The formation rate of the target product H2 was measured to be 0.9 mol g. −1 h −1 The selectivity is 99%.
[0065] Example 7
[0066] The specific reaction process and detection method were the same as in Example 1, with FeNiRhRuPd / SiO2 replacing FeNiRhRuPd / SrTiO3 as the catalyst. The generation rate of the target product H2 was measured to be 0.2 mol g. −1 h −1 The selectivity rate was 97%.
[0067] Example 8
[0068] The specific reaction process and detection method were the same as in Example 1, using a 300W xenon lamp instead of natural sunlight as the light source. The generation rate of the target product H2 was measured to be 1.2 mol g. −1 h −1 The selectivity is 99%.
[0069] Example 9
[0070] The specific reaction process and detection method are the same as in Example 1, using a light intensity of 3000 mW / cm². 2 Light intensity replacing 4000 mW / cm 2 The light intensity was measured. The generation rate of the target product H2 was determined to be 0.8 mol g. −1 h −1 The selectivity is 99%.
[0071] Example 10
[0072] The specific reaction process and detection method were the same as in Example 1, except that 100% CH4 was used instead of 10% CH4 / 90% Ar as the feed gas. The generation rate of the target product H2 was measured to be 1.8 mol g. −1 h −1 The selectivity is 99%.
[0073] Example 11
[0074] The specific reaction process and detection method are the same as in Example 1, except that the flow rate of CH4 is 30 mL / min.-1 Instead of 10 mL min -1 The flow rate was measured, and the formation rate of the target product H2 was found to be 1.0 mol g. −1 h −1 The selectivity is 99%.
[0075] Example 12
[0076] The specific reaction process and detection method are the same as in Example 1, except that the flow rate of CH4 is 5 mL / min. -1 Instead of 10 mL min -1 The flow rate was measured, and the formation rate of the target product H2 was found to be 0.9 mol g. −1 h −1 The selectivity is 99%.
[0077] Examples 13-23
[0078] The specific reaction process and detection method are the same as in Example 1, but a batch reactor is used instead of a mobile phase reactor for the experiment. The recovered catalyst is used 1, 2, 3 times, up to 11 times (i.e., reused 10 times). After 10 reuses, the catalytic efficiency (i.e., the activity and selectivity of the target product) of the catalyst of the present invention does not decrease significantly. Figure 2 ).
[0079] In summary, this invention provides a photothermal-driven methane cracking reaction method. This method utilizes a high-entropy alloy supported on SrTiO3 as a catalyst, and in a mobile phase reactor, the MP reaction can be efficiently driven solely by focused sunlight irradiation. CH4 gas is converted to C+H2 under mild conditions, with a H2 production rate as high as 1.1 mol g. -1 h -1 The selectivity is greater than 99%. The product contains no CO or aromatic hydrocarbons and can be directly used for daily energy consumption. The catalyst exhibits high stability, capable of stable operation for over 200 hours; its high-entropy alloy catalyst demonstrates excellent photothermal conversion efficiency, with localized surface temperatures reaching up to 500°C under focused solar radiation. o C can efficiently drive the MP reaction under mild conditions. This process not only helps mitigate the greenhouse effect but also improves energy efficiency, significantly reducing production costs and energy consumption. It also boasts advantages such as a simple reaction process, short cycle time, and readily available and reusable inexpensive catalysts. This represents a novel synthetic route for the MP reaction and has broad prospects for industrial application.
[0080] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0081] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.
Claims
1. A method for photothermal-driven methane cracking reaction, characterized in that, A catalyst support containing a high-entropy alloy is added to the reactor. The high-entropy alloy on the catalyst support serves as the catalyst, and the reaction occurs under focused illumination. The molar ratio of the high-entropy alloy to the catalyst support is 0.005–0.1:1, and the illumination intensity is 10–4000 mW / cm². 2 The reaction temperature is 20–500℃, the reaction time is 0–200 h, CH4 is converted into C+H2, and the pressure of CH4 gas in the reactor is 0.1 MPa~10 MPa.
2. The method for photothermal-driven methane cracking reaction as described in claim 1, characterized in that, The raw gas used can be derived from pure CH4 gas or combustible ice, shale gas, or natural gas containing CH4 gas.
3. The method for photothermal-driven methane cracking reaction as described in claim 1, characterized in that, Catalyst supports include, but are not limited to, SrTiO3, TiO2, LaFeO3, MgO, Al2O3, SiO2, and BaTiO3.
4. The method according to claim 1, characterized in that, The components of high-entropy alloys include, but are not limited to, Co, Fe, Ni, Cu, Ru, Rh, Pd, Pt, and Ir.
5. The method according to claim 1, characterized in that, The preferred molar ratio of high-entropy alloy to catalyst support is 0.05:
1.
6. The method according to claim 1, characterized in that, The optimal light intensity under illumination conditions is 4000 mW / cm². 2 .
7. The method according to claim 5, characterized in that, The light source for the illumination conditions is one or any combination of natural light, xenon lamps, LED lamps, tungsten lamps, and mercury lamps.
8. The method according to claim 1, characterized in that, The preferred reaction temperature is 25℃, and the preferred reaction duration is 100 h.
9. The method according to claim 1, characterized in that, The reactor is one of the following: quartz reactor, glass reactor, fixed-bed reactor, or mobile phase reactor.