A double heterojunction sodium vanadium fluoride phosphate material, its preparation method and application

By coating the surface of Na3V2(PO4)2F3 cathode material with a carbon layer and a V2O3 phase layer in a double heterojunction structure, the problems of low electronic conductivity and poor cycle stability are solved, realizing a sodium-ion battery cathode material with high specific capacity and long cycle life, which is suitable for industrial production.

CN123105589APending Publication Date: 2026-11-17XUCHANG UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611482456.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-22
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing Na3V2(PO4)2F3 cathode materials have low electronic conductivity and poor cycle stability. The preparation process of the dual heterostructure is complicated, and the matrix crystal form is singular, which limits the improvement of performance.

Method used

A double heterojunction structure with Na3V2(PO4)2F3 as the matrix and a carbon layer and a V2O3 phase layer coated on the surface is prepared by one-step three-stage inert atmosphere calcination to form a V2O3/Na3V2(PO4)2F3/C interface, constructing a continuous conductive network and buffering lattice stress.

Benefits of technology

It improves electronic conductivity and sodium ion diffusion rate, enhances the rate performance and cycle stability of the material, achieves high specific capacity and long cycle life, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105589A_ABST
    Figure CN123105589A_ABST
Patent Text Reader

Abstract

This application provides a double heterojunction sodium vanadium fluoride phosphate material, its preparation method, and its application. The material is a V₂O₃ / Na₃V₂(PO₄)₂F₃ / C ternary composite structure, with Na₃V₂(PO₄)₂F₃ (C₂ / c space group) as the matrix phase. A double heterojunction interface of V₂O₃ / Na₃V₂(PO₄)₂F₃ and Na₃V₂(PO₄)₂F₃ / C is simultaneously constructed on the surface. A continuous conductive network is built through the carbon layer to improve electronic conductivity. The lattice defects of the V₂O₃ phase provide additional sodium storage active sites, buffering lattice stress during sodium insertion / extraction and suppressing material structure collapse, thus synergistically improving the material's specific capacity, rate performance, and cycle stability. The preparation method uses hydrothermally synthesized vanadium dioxide powder as a precursor. The target product can be generated in situ through raw material mixing and a one-step, three-stage inert atmosphere calcination process, eliminating the need for multi-step post-deposition processes. This method is low-cost, simple to operate, provides controllable phase composition, and exhibits good batch stability, making it suitable for industrial-scale production. This material can be directly used in sodium-ion batteries, and the batteries made from it have high reversible specific capacity and long cycle life under high current, showing good prospects for energy storage applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of sodium-ion battery materials technology, and in particular to a double heterojunction sodium vanadium fluoride phosphate material, its preparation method and application. Background Technology

[0002] With the large-scale application of renewable energy and the upgrading of energy storage technology, sodium-ion batteries have become an important alternative to lithium-ion batteries due to their abundant sodium resources and low cost. Among cathode materials, Na3V2(PO4)2F3 (NVPF) has a typical NASICON-type three-dimensional open framework structure, which can construct continuous sodium-ion transport channels. It also has high operating voltage and excellent structural stability, making it a research hotspot for sodium-ion battery cathode materials.

[0003] However, the practical application of Na3V2(PO4)2F3 is limited by three core issues: First, its intrinsic electronic conductivity is poor, resulting in insufficient battery rate performance; second, the repeated insertion and extraction of sodium ions easily generates structural stress, leading to capacity decay; and third, existing mainstream preparation processes, such as high-temperature solid-state methods and conventional hydrothermal methods, generally produce products with uneven particle size distribution and poor product repeatability, making it difficult to meet the requirements of industrial production.

[0004] Existing modification strategies such as carbon coating and element doping can improve individual properties, but they cannot simultaneously solve the problem of synergistic optimization of conductivity and structural stability. In recent years, heterojunction interface engineering, by constructing an embedded electric field at the interface between two phases, can simultaneously regulate electron and ion transport dynamics, becoming an important direction for optimizing the performance of cathode materials. However, most existing sodium vanadium fluorophosphate-based heterojunction materials are single heterojunction designs, which can only solve the shortcomings of a single property; a few double heterojunction materials require multi-step post-deposition processes to prepare, which have defects such as weak interfacial bonding, complex processes, and difficulty in crystal form control. Moreover, the matrix is ​​conventional R3c or tetragonal NVPF, and the performance improvement has reached the theoretical bottleneck, making it impossible to achieve a breakthrough improvement.

[0005] Therefore, developing a novel crystalline structure that can synergistically improve electron / ion transport efficiency and structural stability, as well as a simple, structurally controllable preparation method suitable for large-scale production, is a core technical problem that urgently needs to be solved in this field. Summary of the Invention

[0006] In view of this, this application provides a double heterojunction sodium vanadium fluoride phosphate material, its preparation method and application, to solve the technical problems of low electronic conductivity, poor cycle stability, complicated preparation process of double heterostructure, single matrix crystal form and limited performance improvement of existing Na3V2(PO4)2F3 cathode material.

[0007] This application provides a double heterojunction sodium vanadium fluoride phosphate material, comprising Na3V2(PO4)2F3 and a carbon layer and a V2O3 phase layer coated on the surface of Na3V2(PO4)2F3; The Na3V2(PO4)2F3 has a Na3Fe(PO4)2 type structure and a crystal space group of C2 / c. The crystal space group of the V2O3 phase layer is R3c.

[0008] In some specific implementations, the mass of the V2O3 phase layer accounts for 0.01% to 0.05% of the total mass of the double heterojunction sodium vanadium fluoride phosphate material; The carbon layer accounts for 3.01% to 10.01% of the total mass of the double heterojunction sodium vanadium fluoride phosphate material.

[0009] This application also provides a method for preparing a double heterojunction sodium vanadium fluoride phosphate material, comprising the following steps: (1) A soluble vanadium salt solution was subjected to a hydrothermal reaction under acidic conditions to obtain vanadium dioxide powder; (2) The vanadium dioxide powder, fluorine source, phosphate source, carbon source and sodium source are mixed in sequence to obtain a precursor mixture; (3) The precursor mixture is calcined in an inert atmosphere to obtain a double heterojunction sodium vanadium fluoride phosphate material V2O3 / Na3V2(PO4)2F3 / C.

[0010] In some specific implementations, in step (1), the soluble vanadium salt is one or more of the following: vanadium oxalate, vanadium sulfate, vanadium isonicate, vanadium oxychloride, ammonium metavanadate, sodium vanadate, lithium vanadate, and vanadic acid. The concentration of the soluble vanadium salt solution is 0.1 mol / L to 0.12 mol / L; The pH value of the acidic conditions is 1 to 4.

[0011] In some specific implementations, step (2) specifically involves: mixing the vanadium dioxide powder, fluorine source, phosphate source, carbon source and sodium source in sequence, then adding deionized water for ultrasonic dispersion and stirring to evaporate to dryness, thereby obtaining a precursor mixture; The ultrasonic dispersion time is 10 min to 1 h.

[0012] In some specific implementations, in step (2), the molar ratio of vanadium in the vanadium dioxide powder, fluorine in the fluorine source, phosphorus in the phosphate source, and sodium in the sodium source is 2:2:3:(3.04~3.12); The mass of the added carbon source is 3% to 10% of the theoretical yield of Na3V2(PO4)2F3.

[0013] In some specific implementations, the fluorine source is selected from one or more of ammonium fluoride, sodium fluoride, and ammonium bifluoride; The phosphate source is selected from one or more of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, and sodium phosphate; The carbon source is one or more of glucose, sucrose, and citric acid; The sodium source is selected from one or more of sodium carbonate, sodium bicarbonate, and sodium oxalate.

[0014] In some specific implementations, step (3) specifically includes: a first stage, a second stage and a third stage; The temperature of the first stage is 350℃~400℃, and the time is 3h~8h; The second stage is conducted at a temperature of 700℃~750℃ for 8h~12h. The temperature of the third stage is 800℃~850℃, and the time is 1h~3h.

[0015] In some specific implementations, in step (3), the inert gas is an argon atmosphere with a flow rate of 10 mL / min to 40 mL / min.

[0016] This application also provides a sodium-ion battery, including the double heterojunction sodium vanadium fluoride phosphate material described in the above technical solution, or the double heterojunction sodium vanadium fluoride phosphate material prepared by the preparation method described in the above technical solution.

[0017] This application provides a double heterojunction sodium vanadium fluoride phosphate material, its preparation method, and its application. The material includes Na3V2(PO4)2F3 and a carbon layer and a V2O3 phase layer coated on the surface of Na3V2(PO4)2F3. That is, with Na3V2(PO4)2F3 of space group C2 / c as the matrix phase, a double heterojunction interface of V2O3 / Na3V2(PO4)2F3 and Na3V2(PO4)2F3 / C is simultaneously constructed on the surface. The carbon layer constructs a continuous conductive network to improve electronic conductivity, and the lattice defects of the V2O3 phase provide additional sodium storage active sites and buffer the lattice stress during sodium insertion and extraction, suppressing the collapse of the material structure and synergistically improving the specific capacity, rate performance, and cycle stability of the material. The preparation method uses hydrothermally synthesized vanadium dioxide powder as a precursor. The target product can be generated in situ through raw material mixing and a one-step, three-stage inert atmosphere calcination process, eliminating the need for multi-step post-deposition processes. This method is low-cost, simple to operate, provides controllable phase composition, and exhibits good batch stability, making it suitable for industrial-scale production. This material can be directly used as the positive electrode active material for sodium-ion batteries, producing batteries with high reversible specific capacity and long high-current cycle life, demonstrating promising prospects for electrochemical energy storage applications. Attached Figure Description

[0018] Figure 1 The image shows the crystal structure and microstructure of the vanadium dioxide nanopowder prepared in Example 1. Figure 1 In Figure 'a', the X-ray diffraction (XRD) pattern of vanadium dioxide powder is shown. Figure 1 Image b in the image is a scanning electron microscope (SEM) image of vanadium dioxide powder. Figure 1 Image c is a transmission electron microscope (TEM) image of vanadium dioxide powder; Figure 2 The X-ray diffraction patterns of V2O3 / Na3V2(PO4)2F3 / C prepared in Examples 1, 3, 4 and 5 are shown. Figure 2 In Figure a, the X-ray diffraction pattern of V2O3 / Na3V2(PO4)2F3 / C prepared in Example 1 is shown. Figure 2 In Figure b, the X-ray diffraction pattern of V2O3 / Na3V2(PO4)2F3 / C prepared in Comparative Example 3 is shown. Figure 2 In Figure c, the X-ray diffraction pattern of V2O3 / Na3V2(PO4)2F3 / C prepared in Comparative Example 4 is shown. Figure 2 In the image, d is the X-ray diffraction pattern of V2O3 / Na3V2(PO4)2F3 / C prepared in Comparative Example 5; Figure 3 These are transmission electron microscope (TEM) images of V₂O₃ / Na₃V₂(PO₄)₂F₃ / C prepared in Example 1 at different magnifications. Figure 3 Image a is a bright-field transmission electron microscopy (TEM) image of V₂O₃ / Na₃V₂(PO₄)₂F₃ / C prepared in Example 1. Figure 3 b is a high-resolution transmission electron microscope image of V2O3 / Na3V2(PO4)2F3 / C prepared in Example 1; Figure 4 Scanning electron microscope image of V2O3 / Na3V2(PO4)2F3 / C prepared in Comparative Example 5; Figure 5 The first cycle cyclic voltammetry curve of V2O3 / Na3V2(PO4)2F3 / C prepared in Example 1; Figure 6 The above are charge-discharge curves of the materials prepared in Example 1, Comparative Example 1, Comparative Example 2, Comparative Example 4, and Comparative Example 5. Figure 6 In Figure 'a', the charge-discharge curve of V2O3 / Na3V2(PO4)2F3 prepared in Example 1 is shown. Figure 6 Figure b shows the charge-discharge curves of Na3V2(PO4)2F3 / C prepared in Comparative Example 1. Figure 6 In Figure c, the charge-discharge curve of V2O3 / Na3V2(PO4)2F3 prepared in Comparative Example 2 is shown. Figure 6 In Figure d, the charge-discharge curve of V2O3 / Na3V2(PO4)2F3 / C prepared in Comparative Example 4 is shown. Figure 6 In Figure e, the charge-discharge curve of V2O3 / Na3V2(PO4)2F3 / C prepared in Comparative Example 5 is shown. Figure 7 The above figures show the rate performance of the materials prepared in Example 1, Comparative Example 1, Comparative Example 2, Comparative Example 4, and Comparative Example 5. Figure 7 In Figure 'a', the rate performance diagram of V2O3 / Na3V2(PO4)2F3 / C prepared in Example 1 is shown. Figure 7 Figure b shows the rate performance of Na3V2(PO4)2F3 / C prepared in Comparative Example 1. Figure 7 In Figure c, the rate performance diagram of V2O3 / Na3V2(PO4)2F3 prepared in Comparative Example 2 is shown. Figure 7 In the diagram, d represents the rate performance of V2O3 / Na3V2(PO4)2F3 / C prepared in Comparative Example 4. Figure 7 In Figure e, the rate performance diagram of V2O3 / Na3V2(PO4)2F3 / C prepared in Comparative Example 5 is shown. Figure 8 The cycling curve of V2O3 / Na3V2(PO4)2F3 / C prepared in Example 1 is shown. Detailed Implementation

[0019] It should be understood that the expression “one or more of…” individually includes each of the objects described after the expression, as well as various different combinations of two or more of the described objects, unless otherwise understood from the context and usage. The expression “and / or” combined with three or more described objects should be understood to have the same meaning, unless otherwise understood from the context.

[0020] The terms “including,” “having,” or “containing,” including the use of their grammatical synonyms, should generally be understood as open-ended and non-restrictive, for example, not excluding other unstated elements or steps, unless otherwise specifically stated or understood from the context.

[0021] It should be understood that the order of steps or the sequence of actions is not important as long as this application remains operational. Furthermore, two or more steps or actions can be performed simultaneously.

[0022] The use of any and all instances or exemplary language such as “e.g.” or “including” herein is merely intended to better illustrate the application and does not constitute a limitation on the scope of the application unless the claims are made. No language in this specification should be construed as indicating that any unclaimed element is essential to the practice of this application.

[0023] Furthermore, the numerical ranges and parameters used to define this application are approximate values, and the relevant values ​​in the specific embodiments have been presented as precisely as possible. However, any numerical value inevitably contains standard deviations due to individual test methods. Therefore, unless otherwise explicitly stated, it should be understood that all ranges, quantities, values, and percentages used in this disclosure are modified with the word "approximately." Here, "approximately" generally means that the actual value is within plus or minus 10%, 5%, 1%, or 0.5% of a specific value or range.

[0024] This application provides a double heterojunction sodium vanadium fluoride phosphate material, comprising Na3V2(PO4)2F3 and a carbon layer and a V2O3 phase layer coated on the surface of Na3V2(PO4)2F3; The Na3V2(PO4)2F3 has a Na3Fe(PO4)2 type structure and a crystal space group of C2 / c. The crystal space group of the V2O3 phase layer is R3c.

[0025] In some specific implementations, the mass of the V2O3 phase layer accounts for 0.01% to 0.05% of the total mass of the double heterojunction sodium vanadium fluoride phosphate material; The carbon layer accounts for 3.01% to 10.01% of the total mass of the double heterojunction sodium vanadium fluoride phosphate material.

[0026] The double heterojunction sodium vanadium fluoride phosphate material provided in this application includes Na3V2(PO4)2F3 and a carbon layer and a V2O3 phase layer coated on the surface of Na3V2(PO4)2F3. The main phase Na3V2(PO4)2F3 belongs to the Na3Fe(PO4)2 type structure with a crystal space group of C2 / c, corresponding to JCPDS standard card No. 54-0061. Its surface is simultaneously and in situ coated with a continuous carbon layer and a V2O3 phase layer. The crystal space group of the V2O3 phase is R3c, corresponding to JCPDS standard card No. 85-1403. The two form a V2O3 / Na3V2(PO4)2F3 and a Na3V2(PO4)2F3 / C double heterojunction structure at the interface, respectively. The V₂O₃ phase contains controllable concentrations of oxygen vacancies and lattice defects within its crystal lattice, effectively optimizing the material's electronic structure, providing additional interfacial reactive sites, and buffering lattice stress during charge and discharge. Combined with the continuous conductive network on the particle surface constructed by the outer carbon layer, the dual heterojunction can synergistically form an all-path electron transport channel, simultaneously improving the material's electronic conductivity and sodium ion diffusion rate, giving the material both excellent rate performance and long-cycle stability. Within the charge / discharge voltage range of 1.0V to 3.8V, V₂O₃ (theoretical specific capacity 695 mAh·g⁻¹) exhibits... -1 ) and carbon phase (theoretical specific capacity 350 mAh·g) -1Both exhibit sodium storage activity, and their theoretical specific capacities are higher than those of the main phase Na3V2(PO4)2F3 (128.3 mAh·g). -1 The double heterojunction structure can contribute capacity in synergy with the main phase; the formation of the double heterojunction structure can further regulate the concentration and distribution of oxygen vacancies and defects in the crystal, and enhance the charge transport efficiency and structural stability effect.

[0027] This application also provides a method for preparing a double heterojunction sodium vanadium fluoride phosphate material, comprising the following steps: (1) A soluble vanadium salt solution was subjected to a hydrothermal reaction under acidic conditions to obtain vanadium dioxide powder; (2) The vanadium dioxide powder, fluorine source, phosphate source, carbon source and sodium source are mixed in sequence to obtain a precursor mixture; (3) The precursor mixture is calcined in an inert atmosphere to obtain a double heterojunction sodium vanadium fluoride phosphate material V2O3 / Na3V2(PO4)2F3 / C.

[0028] First, a soluble vanadium salt solution is subjected to a hydrothermal reaction under acidic conditions to obtain vanadium dioxide powder.

[0029] Specifically, a soluble vanadium salt is prepared into an aqueous solution, the pH of the system is adjusted to acidic, and a hydrothermal reaction is carried out. After filtration, washing, and drying, vanadium dioxide powder is obtained. This application does not restrict the source of the soluble vanadium salt. In some specific implementations, the soluble vanadium salt is one or more of vanadium oxalate, vanadium sulfate, vanadium isonicate, vanadium oxychloride, ammonium metavanadate, sodium vanadate, lithium vanadate, and vanadic acid, preferably ammonium metavanadate; the concentration of the soluble vanadium salt solution is 0.1 mol / L to 0.12 mol / L; the pH of the acidic condition is 1 to 4, preferably 1 to 2. In some specific implementations, the reaction temperature is 160℃ to 200℃, preferably 180℃, and the reaction time is 13h to 17h, preferably 14h to 16h, more preferably 15h.

[0030] After obtaining vanadium dioxide powder, the vanadium dioxide powder, fluorine source, phosphate source, carbon source and sodium source are mixed in sequence to obtain a precursor mixture.

[0031] Specifically, vanadium dioxide powder, a fluorine source, a phosphate source, a carbon source, and a sodium source are weighed and mixed sequentially, then deionized water is added for ultrasonic dispersion and stirring followed by evaporation to obtain a precursor mixture. This application does not restrict the sources of the vanadium dioxide powder, fluorine source, phosphate source, carbon source, and sodium source. In some specific implementations, the fluorine source is selected from one or more of ammonium fluoride, sodium fluoride, and ammonium bifluoride, preferably ammonium fluoride. In some specific implementations, the phosphate source is selected from one or more of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, and sodium phosphate, preferably ammonium dihydrogen phosphate. In some specific implementations, the carbon source is one or more of glucose, sucrose, and citric acid, preferably glucose. In some specific implementations, the sodium source is selected from one or more of sodium carbonate, sodium bicarbonate, and sodium oxalate, preferably sodium carbonate. In some specific implementations, the ultrasonic dispersion time is 10 min to 1 h, preferably 10 min to 45 min. In some specific implementations, the molar ratio of vanadium in the vanadium dioxide powder, fluorine in the fluorine source, phosphorus in the phosphate source, and sodium in the sodium source is 2:2:3:(3.04~3.12). In some specific implementations, the added mass of the carbon source is 3%~10% of the theoretical yield of Na3V2(PO4)2F3. Those skilled in the art will understand that when the vanadium source (vanadium dioxide), phosphorus source, and fluorine source are added according to the molar ratio of V:P:F = 2:2:3 in the target product Na3V2(PO4)2F3, the sodium source should be controlled to be 1.33mol%~4mol% excess (in terms of the amount of sodium) relative to the theoretically required amount of sodium to compensate for the loss of sodium through volatilization during high-temperature roasting. For example, when the vanadium feed amount corresponds to 2 mol and the theoretical reaction amount of sodium is 3 mol, the actual sodium feed amount is controlled at 3.04 mol to 3.12 mol; when the vanadium feed amount corresponds to 5 mol and the theoretical reaction amount of sodium is 7.5 mol, the actual sodium feed amount is controlled at 7.6 mol to 7.8 mol.

[0032] A precursor mixture was obtained, and the precursor mixture was calcined in an inert atmosphere to obtain a double heterojunction sodium vanadium fluoride phosphate material V2O3 / Na3V2(PO4)2F3 / C. Those skilled in the art will understand that Na3V2(PO4)2F3 is also written as NVPF; consequently, V2O3 / Na3V2(PO4)2F3 / C is written as V2O3 / NVPF / C in the following text and figures.

[0033] In some specific implementations, the inert gas is an argon atmosphere with a flow rate of 10 mL / min to 40 mL / min, preferably 10 mL / min to 30 mL / min. In some specific implementations, step (3) specifically includes: a first stage, a second stage, and a third stage; the temperature of the first stage is 350℃ to 400℃, preferably 350℃, and the time is 3h to 8h, preferably 5h to 7h; the temperature of the second stage is 700℃ to 750℃, preferably 700℃, and the time is 8h to 12h, preferably 9h to 11h; the temperature of the third stage is 800℃ to 850℃, preferably 800℃, and the time is 1h to 3h, preferably 1h to 2h.

[0034] This application first prepares a vanadium dioxide powder precursor with excellent crystallinity via hydrothermal reaction; the precursor is then ground and mixed with sodium, phosphate, fluorine and carbon sources that can decompose and generate gas, and deionized water is added for ultrasonic dispersion and then stirred and evaporated to dryness. Sodium ions, carbonate ions, ammonium ions, fluorine ions and phosphate ions are uniformly loaded onto the surface and pores of the vanadium dioxide powder by means of ultrasonic action; then a one-step three-stage calcination is carried out in an inert atmosphere to finally obtain the double heterojunction sodium vanadium fluoride phosphate material V2O3 / Na3V2(PO4)2F3 / C. The process involves three stages: the first stage is a low-temperature stage, which decomposes raw materials and pretreats precursors; the second stage is a medium-temperature stage, which completes the nucleation and initial crystallization of the Na3V2(PO4)2F3 matrix; and the third stage is a high-temperature stage, which promotes crystal growth and interface reconstruction, while simultaneously completing carbothermic reduction and carbon layer coating in situ. During this process, the carbon source is pyrolyzed to generate derived carbon, and vanadium dioxide powder is reduced to vanadium trioxide. At the same time, gases such as carbon dioxide and ammonia released by the pyrolysis of decomposable raw materials such as sodium source diffuse from the inside of vanadium dioxide powder to the outside, driving the pyrolyzed carbon and the reduced vanadium trioxide to be simultaneously enriched on the surface of the in-situ generated sodium vanadium fluoride phosphate product. In addition, the preparation process does not require additional multi-step post-deposition or surface modification processes, the raw material cost is low, the process flow is simple, the phase composition and microstructure are highly controllable, the batch product performance is consistent, and it is easy to scale up to achieve industrial-scale production.

[0035] This application also provides a sodium-ion battery, including the double heterojunction sodium vanadium fluoride phosphate material described in the above technical solution, or the double heterojunction sodium vanadium fluoride phosphate material prepared by the preparation method described in the above technical solution.

[0036] The sodium vanadium fluoride fluoride material provided in this application comprises Na3V2(PO4)2F3 and a carbon layer and a V2O3 phase layer coated on the surface of Na3V2(PO4)2F3. Specifically, Na3V2(PO4)2F3 with C2 / c space groups is the main active phase. A V2O3 phase layer and a carbon coating layer are sequentially constructed in situ from the inside out on the surface of the matrix particles, simultaneously forming V2O3 / Na3V2(PO4)2F3 and Na3V2(PO4)2F3 / C dual heterojunction interfaces. The carbon coating layer can construct a high-speed electronic conductive network that runs through the entire material, significantly reducing the interfacial charge transfer resistance. The process enhances electron transport efficiency and rate performance. The V2O3 phase layer possesses a higher theoretical sodium storage capacity than the matrix, and its lattice is rich in oxygen holes and intrinsic defects. This provides additional active sites for sodium ion storage, thereby increasing the overall specific capacity of the material. Furthermore, it buffers lattice volume changes caused by sodium ion insertion / extraction during charge / discharge, inhibiting the pulverization and collapse of the active material structure and enhancing the long-term cycling stability of the material. The synergistic effect of the two heterojunctions modifies the performance of the Na3V2(PO4)2F3 matrix from multiple dimensions, including electronic conductivity, ion diffusion, and structural stability, improving the specific capacity, rate performance, and cycling stability of the material. The preparation method uses hydrothermally synthesized vanadium dioxide powder as a vanadium source precursor. This precursor has a high specific surface area and a well-developed mesoporous structure, enabling uniform loading and confined reactions of sodium, phosphorus, fluorine, and carbon sources. The target dual heterojunction material can be generated in situ through a single three-step inert atmosphere calcination. The obtained materials can be directly used as positive electrode active materials for sodium-ion batteries. The sodium-ion batteries produced exhibit high reversible specific capacity, excellent high current rate performance and long cycle life. They have good applicability in wide temperature range and high power energy storage scenarios, and can provide core material support for the development of new low-cost and long-life sodium-ion energy storage batteries.

[0037] The present application is further illustrated below with reference to embodiments. The scope of protection of the present application is not limited to the following embodiments.

[0038] Example 1

[0039] 0.25g of ammonium metavanadate was dissolved in a polytetrafluoroethylene liner containing 30mL of deionized hot water. Concentrated hydrochloric acid was added dropwise to adjust the pH of the system to 1. The mixture was then placed in a stainless steel reactor and placed in an oven at 180℃ for 15 hours. After filtration, washing, and drying, vanadium dioxide powder was obtained.

[0040] Weigh 0.33g of the above-mentioned vanadium dioxide powder, 0.13g of ammonium fluoride, 0.23g of ammonium dihydrogen phosphate, 0.12g of glucose monohydrate and 0.17g of sodium carbonate, grind and mix them thoroughly, add 10mL of deionized water, ultrasonically disperse them evenly, stir and evaporate the solvent, transfer them to a magnetic boat, and place them in a tube furnace. Under an argon atmosphere, first keep at 350℃ for 6h, then raise the temperature to 700℃ for 10h, and then raise the temperature to 800℃ for 1h. After that, wash the obtained product until neutral and dry it to obtain the double heterojunction sodium vanadium fluoride phosphate material V2O3 / Na3V2(PO4)2F3 / C.

[0041] Comparative Example 1

[0042] Weigh out 0.234g ammonium metavanadate, 0.13g ammonium fluoride, 0.23g ammonium dihydrogen phosphate, 0.12g glucose monohydrate and 0.16g sodium carbonate, grind and mix them thoroughly, add 10mL deionized water, ultrasonically disperse and stir to evaporate the solvent, transfer to a magnetic boat and place in a tube furnace. Under an argon atmosphere, first keep at 350℃ for 6h, then raise the temperature to 700℃ for 10h, and then raise the temperature to 800℃ for 1h. After that, wash the product until neutral and dry to obtain carbon composite sodium vanadium fluoride phosphate material Na3V2(PO4)2F3 / C.

[0043] Comparative Example 2

[0044] 0.25g of ammonium metavanadate was dissolved in a polytetrafluoroethylene liner containing 30mL of deionized hot water. Concentrated hydrochloric acid was added dropwise to adjust the pH of the system to 1. The mixture was then placed in a stainless steel reactor and placed in an oven at 180℃ for 15 hours. After filtration, washing, and drying, vanadium dioxide powder was obtained.

[0045] Weigh 0.33g of the above-mentioned vanadium dioxide powder, 0.13g of ammonium fluoride, 0.23g of ammonium dihydrogen phosphate and 0.16g of sodium carbonate, grind and mix them thoroughly, add 10mL of deionized water, ultrasonically disperse them evenly, stir and evaporate the solvent, transfer them to a magnetic boat, and place them in a tube furnace. Under an argon atmosphere, first keep at 350℃ for 6h, then raise the temperature to 700℃ for 10h, and then raise the temperature to 800℃ for 1h. After that, wash the obtained product until neutral and dry it to obtain the V2O3 composite sodium vanadium fluoride phosphate material V2O3 / Na3V2(PO4)2F3.

[0046] Comparative Example 3

[0047] 0.25g of ammonium metavanadate was dissolved in a polytetrafluoroethylene liner containing 30mL of deionized hot water. Concentrated hydrochloric acid was added dropwise to adjust the pH of the system to 2. The mixture was then placed in a stainless steel reactor and placed in an oven at 180℃ for 15 hours. After filtration, washing, and drying, vanadium dioxide powder was obtained.

[0048] Weigh 0.33g of the above-mentioned vanadium dioxide powder, 0.13g of ammonium fluoride, 0.23g of ammonium dihydrogen phosphate, 0.10g of glucose monohydrate and 0.17g of sodium carbonate, grind and mix them thoroughly, add 10mL of deionized water, ultrasonically disperse them evenly, stir and evaporate the solvent, transfer them to a magnetic boat, and place them in a tube furnace. Under an argon atmosphere, first keep at 350℃ for 6h, then raise the temperature to 700℃ and react for 10h. After washing the obtained product until neutral, dry it to obtain the double heterojunction sodium vanadium fluoride phosphate material V2O3 / Na3V2(PO4)2F3 / C.

[0049] Comparative Example 4

[0050] Weigh 0.33g of commercial vanadium dioxide powder, 0.13g of ammonium fluoride, 0.23g of ammonium dihydrogen phosphate, 0.12g of glucose monohydrate and 0.17g of sodium carbonate, grind and mix them thoroughly, add 10mL of deionized water, ultrasonically disperse and stir to evaporate the solvent, transfer to a magnetic boat and place in a tube furnace. Under an argon atmosphere, first keep at 350℃ for 6h, then raise the temperature to 700℃ for 10h, and then raise the temperature to 800℃ for 1h. After that, wash the product until neutral and dry to obtain the double heterojunction sodium vanadium fluoride phosphate material V2O3 / Na3V2(PO4)2F3 / C.

[0051] Comparative Example 5

[0052] The only difference between this comparative example and Example 1 is the order in which the raw materials are added, as detailed below: 0.25g of ammonium metavanadate was dissolved in a polytetrafluoroethylene liner containing 30mL of deionized hot water. Concentrated hydrochloric acid was added dropwise to adjust the pH of the system to 1. The mixture was then placed in a stainless steel reactor and placed in an oven at 180℃ for 15 hours. After filtration, washing, and drying, vanadium dioxide powder was obtained.

[0053] Weigh out 0.13g ammonium fluoride, 0.17g sodium carbonate, 0.23g ammonium dihydrogen phosphate, 0.33g vanadium dioxide powder and 0.12g glucose monohydrate, grind and mix them thoroughly, add 10mL deionized water, ultrasonically disperse and stir to evaporate the solvent, transfer to a magnetic boat and place in a tube furnace. Under an argon atmosphere, first keep at 350℃ for 6h, then raise the temperature to 700℃ for 10h, and then raise the temperature to 800℃ for 1h. After that, wash the obtained product until neutral and dry it to obtain the double heterojunction sodium vanadium fluoride phosphate material V2O3 / Na3V2(PO4)2F3 / C.

[0054] Experimental Example 1

[0055] The phase structure and microstructure of the vanadium dioxide powder prepared in Example 1 were tested using X-ray diffraction, field emission scanning electron microscopy, and transmission electron microscopy. The results are shown in [reference needed]. Figure 1 , Figure 1 The image shows the crystal structure and microstructure of the vanadium dioxide powder prepared in Example 1; wherein, Figure 1 In Figure 'a', the X-ray diffraction (XRD) pattern of vanadium dioxide powder is shown. Figure 1 Image b in the image is a scanning electron microscope (SEM) image of vanadium dioxide powder. Figure 1 Image c is a transmission electron microscope (TEM) image of vanadium dioxide powder.

[0056] Depend on Figure 1 As shown in section a, the diffraction peaks in the spectrum correspond well with the characteristic peaks of the VO2 material (JCPDS No. 812392) with space group c2 / m(12), indicating that the obtained vanadium dioxide powder has a pure phase and excellent crystallinity. Figure 1 b and Figure 1 As can be seen from c, the obtained VO2 exhibits a uniform porous nanosphere structure with a particle size of 20nm~50nm.

[0057] Experimental Example 2

[0058] The phase structure of the V₂O₃ / Na₃V₂(PO₄)₂F₃ / C samples prepared in Example 1, Comparative Example 3, Comparative Example 4, and Comparative Example 5 was characterized using X-ray diffraction. The results are shown in [reference needed]. Figure 2 , Figure 2 The X-ray diffraction patterns of V2O3 / Na3V2(PO4)2F3 / C prepared in Example 1, Comparative Example 3, Comparative Example 4, and Comparative Example 5 are shown below; Figure 2 In Figure a, the X-ray diffraction pattern of V2O3 / Na3V2(PO4)2F3 / C prepared in Example 1 is shown. Figure 2 In Figure b, the X-ray diffraction pattern of V2O3 / Na3V2(PO4)2F3 / C prepared in Comparative Example 3 is shown. Figure 2 In Figure c, the X-ray diffraction pattern of V2O3 / Na3V2(PO4)2F3 / C prepared in Comparative Example 4 is shown. Figure 2 In the diagram, d is the X-ray diffraction pattern of V2O3 / Na3V2(PO4)2F3 / C prepared in Comparative Example 5.

[0059] Experimental results show that, by Figure 2As can be seen from a, in the V2O3 / Na3V2(PO4)2F3 / C prepared in Example 1, the space group of Na3V2(PO4)2F3 is C2 / c

[15] , Na3Fe(PO4)2 type, corresponding to JCPDS standard card No. 54-0061; the space group of V2O3 is R3c

[167] , corresponding to JCPDS standard card No. 85-1403; at the same time, Na3V2(PO4)3 of the Na3Fe2(PO4)3 type with the space group R3c

[167] appears, corresponding to JCPDS standard card No. 70-361. Figure 2 As can be seen in Figure b, the crystallinity of V2O3 / Na3V2(PO4)2F3 / C prepared in Comparative Example 3 is lower than that in Example 1. Figure 2 As can be seen from c, Comparative Example 4, using commercially available vanadium dioxide, can also synthesize the double heterojunction sodium vanadium fluoride phosphate material V2O3 / Na3V2(PO4)2F3 / C. Figure 2 As shown in Figure d, in the V2O3 / Na3V2(PO4)2F3 / C prepared in Comparative Example 5, the space group of Na3V2(PO4)2F3 is C2 / c

[15] , which is of the Na3Fe(PO4)2 type and corresponds to JCPDS standard card No. 54-0061.

[0060] Experimental Example 3

[0061] The V₂O₃ / Na₃V₂(PO₄)₂F₃ / C prepared in Example 1 and Comparative Example 5 were characterized using transmission electron microscopy. The results are shown in [link to documentation]. Figure 3 and Figure 4 , Figure 3 Transmission electron microscopy (TEM) images of V₂O₃ / Na₃V₂(PO₄)₂F₃ / C prepared in Example 1 at different magnifications; wherein, Figure 3 Image a is a bright-field transmission electron microscopy (TEM) image of V₂O₃ / Na₃V₂(PO₄)₂F₃ / C prepared in Example 1. Figure 3 Image b is a high-resolution transmission electron microscope image of V2O3 / Na3V2(PO4)2F3 / C prepared in Example 1. Figure 4 Scanning electron microscope image of V2O3 / Na3V2(PO4)2F3 / C prepared for Comparative Example 5.

[0062] Experimental results show that, by Figure 3 a and Figure 3 As shown in section b, the V2O3 / Na3V2(PO4)2F3 / C prepared in Example 1 exhibits a double heterojunction structure of V2O3 / Na3V2(PO4)2F3 and Na3V2(PO4)2F3 / C, and the V2O3 phase layer generates abundant holes and defects in its lattice, which is beneficial for increasing the active sites of sodium ions. Figure 4It can be seen that the V2O3 / Na3V2(PO4)2F3 / C prepared in Comparative Example 5 are all large particles with a diameter of over 5 μm, which is not conducive to improving specific capacity.

[0063] Test Example 4

[0064] The V2O3 / Na3V2(PO4)2F3 / C prepared in Example 1 was used as the positive electrode to assemble a sodium-ion battery. The performance of the sodium-ion battery was tested at a voltage of 1.0V~3.8V and a scan rate of 0.6mV / s. The results are shown in [reference needed]. Figure 5 , Figure 5 The first cycle voltammetry curve of V2O3 / Na3V2(PO4)2F3 / C prepared in Example 1.

[0065] Experimental results show that V2O3 / Na3V2(PO4)2F3 / C exhibits two oxidation peaks and a reduction peak during charge and discharge, consistent with its high specific capacity. This indicates that the V2O3 / Na3V2(PO4)2F3 / C prepared in Example 1, when used as a cathode material in a sodium-ion battery, demonstrates excellent electrochemical performance.

[0066] Experimental Example 5

[0067] The V2O3 / Na3V2(PO4)2F3 / C prepared in Example 1, the Na3V2(PO4)2F3 / C prepared in Comparative Example 1, the V2O3 / Na3V2(PO4)2F3 prepared in Comparative Example 2, the V2O3 / Na3V2(PO4)2F3 / C prepared using commercial VO2 in Comparative Example 4, and the V2O3 / Na3V2(PO4)2F3 / C prepared in Comparative Example 5 were each independently used as positive electrodes to assemble sodium-ion batteries for their first charge-discharge tests. The results are shown in [link to relevant documentation]. Figure 6 , Figure 6 The charge-discharge curves of the materials prepared in Example 1, Comparative Example 1, Comparative Example 2, Comparative Example 4, and Comparative Example 5 are shown; wherein, Figure 6 In Figure 'a', the charge-discharge curve of V2O3 / Na3V2(PO4)2F3 / C prepared in Example 1 is shown. Figure 6 Figure b shows the charge-discharge curves of Na3V2(PO4)2F3 / C prepared in Comparative Example 1. Figure 6 In Figure c, the charge-discharge curve of V2O3 / Na3V2(PO4)2F3 prepared in Comparative Example 2 is shown. Figure 6 In Figure d, the charge-discharge curve of V2O3 / Na3V2(PO4)2F3 / C prepared in Comparative Example 4 is shown. Figure 6 In Figure e, the charge-discharge curve of V2O3 / Na3V2(PO4)2F3 / C prepared in Comparative Example 5 is shown.

[0068] Experimental results show that the V2O3 / Na3V2(PO4)2F3 / C prepared in Example 1 exhibits a high discharge specific capacity of 160 mAh / g, which is significantly better than the 136 mAh / g specific capacity of carbon-composite sodium vanadium fluoride phosphate (Na3V2(PO4)2F3 / C); the Na3V2(PO4)2F3 / C prepared in Comparative Example 1 exhibits a moderate specific capacity of 139 mAh / g, which is lower than the 160 mAh / g of V2O3 / Na3V2(PO4)2F3 / C when used as a positive electrode; the V2O3 / Na3V2(PO4)2F3 / C prepared in Comparative Example 2... The V2O3 / Na3V2(PO4)2F3 / C prepared using commercial VO2 showed a high specific capacity of 220 mAh / g, but its specific capacity decreased to 127 mAh / g in the second cycle, which was significantly lower than that of Example 1. Furthermore, as the current density increased to 5 A / g (24C), the specific capacity decreased to 27 mAh / g. The V2O3 / Na3V2(PO4)2F3 / C prepared in Comparative Example 4 showed the lowest specific capacity of 104 mAh / g. The V2O3 / Na3V2(PO4)2F3 / C prepared in Comparative Example 5 had a specific capacity of 150 mAh / g during the first charge and a specific capacity of 140 mAh / g during the discharge.

[0069] Experimental Example 6

[0070] The V2O3 / Na3V2(PO4)2F3 / C prepared in Example 1, the Na3V2(PO4)2F3 / C prepared in Comparative Example 1, the V2O3 / Na3V2(PO4)2F3 prepared in Comparative Example 2, the V2O3 / Na3V2(PO4)2F3 / C prepared using commercial VO2 in Comparative Example 4, and the V2O3 / Na3V2(PO4)2F3 / C prepared in Comparative Example 5 were each independently used as positive electrodes to assemble sodium-ion batteries for rate performance testing. The results are shown in [link to relevant documentation]. Figure 7 , Figure 7 The following are rate performance diagrams of the materials prepared in Example 1, Comparative Example 1, Comparative Example 2, Comparative Example 4, and Comparative Example 5; wherein, Figure 7 In Figure 'a', the rate performance diagram of V2O3 / Na3V2(PO4)2F3 / C prepared in Example 1 is shown. Figure 7 Figure b shows the rate performance of Na3V2(PO4)2F3 / C prepared in Comparative Example 1. Figure 7 In Figure c, the rate performance diagram of V2O3 / Na3V2(PO4)2F3 prepared in Comparative Example 2 is shown. Figure 7 In the diagram, d represents the rate performance of V2O3 / Na3V2(PO4)2F3 / C prepared in Comparative Example 4. Figure 7 In Figure e, the rate performance diagram of V2O3 / Na3V2(PO4)2F3 / C prepared in Comparative Example 5 is shown.

[0071] Experimental results show that the V2O3 / Na3V2(PO4)2F3 / C prepared in Example 1 still maintains a specific capacity of 105 mAh / g after 70 cycles, exhibiting good cycling stability. This is mainly attributed to the fact that the abundant vacancies and defects in the unique double heterojunction structure of V2O3 / Na3V2(PO4)2F3 / C provide a buffer space to alleviate the collapse of the composite material structure and extend the cycle life. The specific capacity of Na3V2(PO4)2F3 / C obtained in Comparative Example 1 was only 80 mAh / g after 70 cycles; the specific capacity of V2O3 / Na3V2(PO4)2F3 obtained in Comparative Example 2 was 52 mAh / g after 70 cycles; the specific capacity of V2O3 / Na3V2(PO4)2F3 / C prepared using commercial VO2 in Comparative Example 4 was 74 mAh / g after 70 cycles; and the specific capacity of V2O3 / Na3V2(PO4)2F3 / C prepared in Comparative Example 5 was the lowest, at only 67 mAh / g, after 70 cycles.

[0072] Experimental Example 7

[0073] After assembling a sodium-ion battery using the V2O3 / Na3V2(PO4)2F3 / C prepared in Example 1 as the positive electrode, a cycle test was conducted at a current density of 5A / g. The results are shown in [reference]. Figure 8 , Figure 8 The figure shows the cycling curve of V2O3 / Na3V2(PO4)2F3 / C prepared in Example 1. As can be seen from the figure, the specific capacity of V2O3 / Na3V2(PO4)2F3 / C remains at 50 mAh / g after 1400 cycles.

[0074] The above description is merely a preferred embodiment of this application, but the scope of protection of this application is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in this application, based on the technical solution and inventive concept of this application, should be included within the scope of protection of this application.

Claims

1. A double heterojunction sodium vanadium phosphate fluoride material, characterized in that, It includes Na3V2(PO4)2F3 and a carbon layer and a V2O3 phase layer coated on the surface of Na3V2(PO4)2F3; The Na3V2(PO4)2F3 has a Na3Fe(PO4)2 type structure and a crystal space group of C2 / c. The space group of the V2O3 phase layer crystal is R3c.

2. The double heterojunction sodium vanadium fluorophosphate material of claim 1, wherein, The mass of the V2O3 phase layer accounts for 0.01% to 0.05% of the total mass of the double heterojunction sodium vanadium fluoride phosphate material; The carbon layer accounts for 3.01% to 10.01% of the total mass of the double heterojunction sodium vanadium fluoride phosphate material.

3. A method for producing the double heterojunction sodium vanadium fluorophosphate material according to claim 1 or 2, characterized in that, Includes the following steps: (1) A soluble vanadium salt solution was subjected to a hydrothermal reaction under acidic conditions to obtain vanadium dioxide powder; (2) The vanadium dioxide powder, fluorine source, phosphate source, carbon source and sodium source are mixed in sequence to obtain a precursor mixture; (3) The precursor mixture is calcined in an inert atmosphere to obtain a double heterojunction sodium vanadium fluoride phosphate material V2O3 / Na3V2(PO4)2F3 / C.

4. The production method according to claim 3, characterized by, In step (1), the soluble vanadium salt is one or more of the following: vanadium oxalate, vanadium sulfate, vanadium isonicate, vanadium oxychloride, ammonium metavanadate, sodium vanadate, lithium vanadate, and vanadic acid. The concentration of the soluble vanadium salt solution is 0.1 mol / L to 0.12 mol / L; The pH value of the acidic conditions is 1 to 4.

5. The preparation method according to claim 3, characterized in that, Step (2) specifically involves: mixing the vanadium dioxide powder, fluorine source, phosphate source, carbon source and sodium source in sequence, then adding deionized water for ultrasonic dispersion and stirring to evaporate to dryness, thereby obtaining a precursor mixture; The ultrasonic dispersion time is 10 min to 1 h.

6. The production method according to claim 3 or 5, characterized by, In step (2), the molar ratio of vanadium in the vanadium dioxide powder, fluorine in the fluorine source, phosphorus in the phosphate source and sodium in the sodium source is 2:2:3:(3.04~3.12); The mass of the added carbon source is 3% to 10% of the theoretical yield of Na3V2(PO4)2F3.

7. The preparation method according to claim 3, characterized in that, The fluorine source is selected from one or more of ammonium fluoride, sodium fluoride, and ammonium bifluoride; The phosphate source is selected from one or more of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, and sodium phosphate; The carbon source is one or more of glucose, sucrose, and citric acid; The sodium source is selected from one or more of sodium carbonate, sodium bicarbonate, and sodium oxalate.

8. The preparation method according to claim 3, characterized in that, In step (3), the roasting specifically includes: a first stage, a second stage, and a third stage; The temperature of the first stage is 350℃~400℃, and the time is 3h~8h; The second stage is conducted at a temperature of 700℃~750℃ for 8h~12h. The temperature of the third stage is 800℃~850℃, and the time is 1h~3h.

9. The production method according to claim 3, wherein In step (3), the inert gas is an argon atmosphere with a flow rate of 10 mL / min to 40 mL / min.

10. A sodium-ion battery, characterized in that, Includes the sodium vanadium fluoride phosphate material with double heterojunction as described in claim 1 or 2, or the sodium vanadium fluoride phosphate material with double heterojunction prepared by the preparation method according to any one of claims 3 to 9.