Phosphorus-doped high-capacity sodium-ion battery hard carbon anode material and its preparation method

By combining phosphorus doping and acidic catalysts, the problems of low sodium storage capacity of hard carbon materials and high energy consumption of traditional activation processes have been solved, realizing the preparation of efficient and environmentally friendly sodium-ion battery anode materials and improving sodium storage capacity and electrochemical performance.

CN123105609APending Publication Date: 2026-11-17SHENZHEN JANAENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611507605.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-28
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing hard carbon materials have low sodium storage capacity in sodium-ion batteries. Traditional activation processes are energy-intensive, costly, and environmentally unfriendly, and their uneven pore structure makes it difficult to meet the requirements for high energy density.

Method used

The preparation method using phosphorus doping involves constructing interconnected channels through low-temperature pre-carbonization with phosphorus-containing additives, combined with gas-phase activation with acidic catalysts and surface coating modification, to achieve efficient and uniform micropore construction and widening of carbon layer spacing. High-temperature sintering is then used to control the microstructure.

Benefits of technology

It significantly improves the sodium storage capacity and electrochemical performance of hard carbon anode materials for sodium-ion batteries, reduces production energy consumption and costs, and enhances the environmental friendliness and stability of the materials.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a phosphorus-doped high-capacity sodium-ion battery hard carbon anode material and its preparation method. The preparation method includes the following steps: S1, precursor mixing treatment: uniformly mixing carbon-containing raw materials and phosphorus-containing additives to obtain a uniformly dispersed mixed precursor; S2, pre-carbonization treatment: performing low-temperature pre-carbonization to obtain a pre-carbonized precursor; S3, activation treatment: uniformly mixing the pre-carbonized precursor with a catalyst and performing activation treatment to obtain a precursor rich in micropores; S4, surface coating modification treatment: uniformly mixing the microporous precursor with a coating agent and performing surface modification coating treatment to obtain a surface-coated precursor; S5, high-temperature sintering: subjecting the surface-coated precursor from step S4 to high-temperature sintering treatment to finally obtain a high-performance hard carbon anode material. The phosphorus-doped high-capacity sodium-ion battery hard carbon anode material and its preparation method of this invention have the characteristics of excellent electrochemical performance, green and environmentally friendly process, and low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of sodium-ion battery technology, specifically to a phosphorus-doped high-capacity sodium-ion battery hard carbon anode material and its preparation method. Background Technology

[0002] With the rapid development of the new energy storage field, low-cost, long-life, and highly safe energy storage battery technology has become a core research and development direction for the industry. Compared with lithium-ion batteries, sodium-ion batteries have outstanding advantages such as abundant and widely distributed sodium resources, low cost, and excellent low-temperature performance, making them one of the most industrially promising technologies in the field of large-scale electrochemical energy storage. As the core material of sodium-ion batteries, the sodium storage performance of the anode material directly determines the battery's capacity, rate performance, cycle stability, and industrialization cost, and is one of the core bottlenecks restricting the large-scale promotion of sodium-ion batteries.

[0003] Hard carbon materials have become the mainstream research and industrialization direction in the sodium-ion battery industry due to their advantages such as wide availability of raw materials, controllable preparation costs, high sodium storage capacity, and low operating potential.

[0004] Currently, hard carbon materials are mostly prepared by direct high-temperature pyrolysis of raw materials such as biomass, coal, and resin. However, extensive research and industrial application have shown that hard carbon materials prepared by direct high-temperature pyrolysis have low sodium storage capacity, which is insufficient to meet the application requirements of high-energy-density sodium-ion batteries. To improve the sodium storage capacity of hard carbon materials, current mainstream modification technologies focus on activating and creating pores in the carbon precursor. By constructing a rich microporous structure within the hard carbon precursor, the active sites for sodium storage are increased, thereby significantly improving the sodium storage capacity of hard carbon materials.

[0005] Currently, the most widely used methods are chemical activation and physical activation. Chemical activation uses highly corrosive activators such as KOH and NaOH to etch pores in hard carbon precursors. However, this method requires several times the mass of the precursor as a strong alkaline activator, resulting in high raw material consumption and low product yield. Furthermore, the process is highly corrosive and places stringent requirements on equipment. In addition, it necessitates extensive acid washing and pure water washing, generating massive amounts of difficult-to-treat waste liquid, leading to poor environmental performance. Physical activation involves introducing an activating atmosphere as an activator into the carbonized material at high temperatures (typically 700℃~1100℃), causing a redox reaction between the carbon atoms and the pores to be burned off. However, the pore-forming effect relies solely on surface diffusion etching, resulting in slow gas penetration into the precursor, weak reaction kinetics, and a low overall activation rate. It requires extremely high temperatures and long holding times to achieve the desired pore-forming effect, leading to high industrial costs and extremely high energy consumption. It also easily results in uneven activation, with over-activation of the surface layer and insufficient activation of the interior. To increase porosity, the carbon matrix needs to be excessively etched, resulting in severe carbon skeleton loss and high carbon burn-off rate. The overall yield is usually between 15-30%, which is relatively low. Summary of the Invention

[0006] The purpose of this invention is to provide a method for preparing phosphorus-doped high-capacity sodium-ion battery hard carbon anode material, which has the characteristics of excellent electrochemical performance, green and environmentally friendly process and low cost.

[0007] This invention can be achieved through the following technical solutions:

[0008] The present invention discloses a method for preparing phosphorus-doped high-capacity sodium-ion battery hard carbon anode material, comprising the following steps:

[0009] S1. Precursor mixing treatment: Carbon-containing raw materials and phosphorus-containing additives are uniformly mixed to obtain a uniformly dispersed mixed precursor.

[0010] S2. Pre-carbonization treatment: The mixed precursor obtained in step S1 is subjected to low-temperature pre-carbonization to obtain a pre-carbonized precursor.

[0011] S3. Activation treatment: The pre-carbonized precursor prepared in step S2 is uniformly mixed with the catalyst and activated to obtain a precursor rich in micropores.

[0012] S4. Surface coating modification treatment: The precursor rich in micropores after activation and pore formation in step S3 is uniformly mixed with the coating agent and subjected to surface modification coating treatment to obtain a surface-coated precursor.

[0013] S5. High-temperature sintering: The precursor coated on the surface in step S4 is subjected to high-temperature sintering to control the degree of graphitization of the carbon matrix and reconstruct the microstructure, ultimately obtaining a high-performance hard carbon anode material.

[0014] Specifically, in step S2, the carbon-containing raw material is initially carbonized to remove moisture, small molecule impurities, and various volatile components, resulting in a structurally stable carbonized precursor. Simultaneously, relying on the low-temperature activation etching effect of the phosphorus-containing additive, a permeable primary hard pore structure is pre-constructed within the carbon matrix, providing a structural basis for subsequent gas-phase activation. In step S3, during activation, the activation atmosphere rapidly and fully penetrates into the material through the permeable primary pores constructed in step S2. At the same time, the acidic catalyst effectively reduces the activation energy and temperature of gas-phase activation, efficiently catalyzing a controllable etching reaction between the carbon matrix and the activation atmosphere, promoting the activation reaction to proceed fully within the material's pores. Compared to traditional pure physical gas-phase activation, this invention achieves a deeper and more uniform internal pore-forming effect through an acidic catalytic-assisted mechanism, significantly increasing the micropore content within the material while achieving precise control of pore size, effectively avoiding the defects of excessive surface etching and insufficient internal activation inherent in traditional physical activation. This step allows for precise control of the material's pore structure ratio, significantly reducing the proportion of ineffective mesopores and macropores. It constructs a large number of uniformly distributed, structurally stable, high-density effective sodium-storage micropores within the carbon matrix, further optimizing the number of sodium ion transport channels and sodium-storage active sites, and significantly improving the material's sodium storage capacity and electrochemical kinetics performance. In step S4, surface coating effectively reduces the specific surface area of ​​the hard carbon material, passivates surface defects, and thus significantly reduces irreversible side reactions between the electrolyte and the material surface during battery charging and discharging, inhibiting excessive SEI film growth and significantly improving the first-cycle coulombic efficiency and interface stability of the hard carbon anode material. In step S5, during high-temperature sintering, the precursor material undergoes final graphitization control and microstructure reconstruction under high temperature. The phosphorus element introduced into the precursor can achieve in-situ self-doping modification, effectively controlling the bulk microstructure of the hard carbon material and significantly widening the interlayer spacing. Compared to undoped pure hard carbon materials, phosphorus doping effectively disrupts the locally regular stacked structure of the carbon layers and significantly increases the interlayer spacing, providing ample interlayer transport space for the rapid insertion and extraction of large-radius sodium ions. This greatly improves the material's kinetic properties and thus enhances its rate performance. Simultaneously, the high-temperature sintering process in step S5, while fully preserving the rich microporous structure constructed earlier, achieves deep carbonization and moderate graphitization of the surface carbon coating layer, effectively reducing the material's specific surface area and passivating surface activity defects. After high-temperature structural reconstruction according to this invention, a high-performance hard carbon anode material with high micropore content, uniform pore size distribution, unobstructed ion transport channels, wide interlayer spacing, and dual stability in both bulk and interfacial structures is ultimately obtained, achieving a synergistic breakthrough in high capacity and high rate performance for sodium-ion battery hard carbon materials.

[0015] Further, in step S1, the phosphorus-containing additive is one or more of phosphoric acid, pyrophosphoric acid, polyphosphoric acid, metaphosphoric acid, sodium dihydrogen phosphate, and potassium dihydrogen phosphate. In this invention, various phosphorus-containing additives can achieve low-temperature activation. During the subsequent pre-carbonization step S2, the hard carbon precursor can be gently etched from the inside out, constructing a three-dimensional interconnected primary pore structure throughout the material in situ, providing a smooth transport pathway for the subsequent deep penetration of the activation atmosphere into the material for deep oxidation. This fundamentally solves the technical shortcomings of traditional physical vapor phase activation, which can only create pores on the material surface and cannot allow the activation atmosphere to penetrate deep into the material's interior.

[0016] Furthermore, in step S1, the amount of phosphorus-containing additive added is 0.5–5 wt% of the amount of carbon source added; this range is a key parameter for achieving the excellent technical effect of this invention. If the amount of phosphorus-containing additive added is too low, the etching active component is insufficient, and a continuous and interconnected primary pore structure cannot be constructed inside the hard carbon precursor. The subsequent activation atmosphere will still have difficulty penetrating the material, and the pore-forming effect will be greatly limited. If the amount of phosphorus-containing additive added is too high, the carbon matrix will be over-etched, resulting in a large number of ineffective mesopores and macropores inside the material, destroying the advantages of the microporous structure, and reducing the sodium storage capacity and first coulombic efficiency of the material.

[0017] Furthermore, in step S2, the conditions for low-temperature pre-carbonization are: a protective atmosphere of nitrogen and / or argon, a pre-carbonization temperature of 400-700℃, and a holding time of 1-5 hours. If the pre-carbonization temperature is too high or the holding time is too long, it is easy to cause over-activation, resulting in ineffective mesopores and macropores; if the pre-carbonization temperature is too low or the holding time is too short, the precursor will not be sufficiently solidified, the activation etching force will be insufficient, and a stable carbon skeleton and a complete through-hole primary pore structure cannot be achieved.

[0018] Further, in step S3, the catalyst is one or more of hydrochloric acid, sulfuric acid, nitric acid, oxalic acid, citric acid, benzoic acid, p-benzenesulfonic acid, and phosphoric acid, and the amount of the catalyst added is 0.5 to 2 wt.% of the carbonization precursor.

[0019] Further, in step S3, the activation conditions are: activation temperature of 500-800℃, activation time of 2-5h; and activation atmosphere of one or more of oxygen, air, water vapor, CO2, and CO.

[0020] If the amount of acidic catalyst added is too high, the activation temperature is too high, or the activation time is too long, it is easy to cause over-etching of the carbon matrix, which will induce pore collapse, the generation of a large number of ineffective mesopores and macropores, and destroy the advantages of the microporous structure. Conversely, if the amount of catalyst added is too low, the activation temperature is insufficient, or the activation time is too short, the degree of etching reaction will be insufficient, the number of pores will be small, the pore connectivity will be poor, and the efficient micropore formation effect cannot be achieved.

[0021] Further, in step S5, the conditions for high-temperature sintering are: a protective atmosphere of nitrogen and / or argon, a sintering temperature of 1100-1600℃, and a sintering holding time of 2-5 hours. The sintering temperature and holding time in this step are the core parameters of this invention, directly determining the degree of graphitization of the hard carbon and the quality of the sodium storage microstructure. If the sintering temperature is too high or the holding time is too long, the degree of graphitization of the hard carbon material will be too high, resulting in overly dense carbon layer stacking. This will significantly narrow the carbon layer spacing, hindering the rapid insertion / extraction diffusion of large-radius sodium ions and drastically weakening the material's rate performance and sodium storage capacity. If the sintering temperature is too low or the holding time is insufficient, the degree of graphitization of the hard carbon material will be too low, resulting in incomplete carbon layer framework development, disordered microstructure, and high defect levels. This will prevent the formation of an optimal carbon layer structure suitable for sodium ion storage, leading to a significant decrease in sodium storage capacity and first-week coulombic efficiency.

[0022] Further, in step S4, the coating agent is one or more of asphalt, phenolic resin, glucose, and polyacrylonitrile. The amount of coating agent added is 0.5–3 wt.% of the precursor mass, and this addition range represents the optimal process window that balances interfacial stability and ion transport performance. If too much coating agent is added, an excessively thick coating layer will form on the surface of the hard carbon material, increasing the diffusion resistance of sodium ions and impairing the rate performance of the material. If too little coating agent is added, the carbon content on the material surface will be insufficient, failing to effectively cover surface defects and reduce the specific surface area, thus failing to achieve excellent coating modification effects.

[0023] Furthermore, in step S1, the carbon-containing raw material is one or more of the following: coconut shell, walnut shell, wood chips, straw, bamboo, macadamia nut shell, corn cob, anthracite, lignite, bituminous coal, phenolic resin, and epoxy resin.

[0024] Another aspect of the present invention is to protect a hard carbon anode material for sodium-ion batteries, which is prepared by the above-described preparation method.

[0025] This invention discloses a phosphorus-doped high-capacity hard carbon anode material for sodium-ion batteries and its preparation method, which has the following beneficial effects:

[0026] First, it exhibits excellent electrochemical performance. This invention combines high sodium storage capacity with excellent kinetic performance: By constructing three-dimensional interconnected primary channels from the inside out using phosphorus-containing additives, and combined with acidic catalysis for controllable gas-phase activation, a large number of uniform and effective sodium storage microporous structures can be built within the carbon matrix, significantly increasing the number of active sodium storage sites and substantially improving the material's reversible sodium storage capacity. Simultaneously, in-situ phosphorus doping effectively widens the carbon interlayer spacing, and the interconnected multi-level pore structure significantly reduces sodium ion diffusion resistance. Combined with the passivation effect of surface coating modification on interface defects, it effectively inhibits excessive SEI film growth, improves first-cycle coulombic efficiency and interface stability, enabling the material to possess excellent comprehensive electrochemical performance with high capacity, high rate capability, and long cycling duration.

[0027] Secondly, the process is green and environmentally friendly. This invention completely eliminates the use of traditional strong alkalis and avoids the use of strong corrosive activators such as KOH and NaOH, thus preventing problems such as strong alkali corrosion at the source. The process eliminates the need for complex post-treatment steps such as acid washing and multi-stage water washing, significantly reducing the discharge of high-salt, high-alkali wastewater and waste residue during production, resulting in extremely low pressure on waste treatment. Simultaneously, it effectively reduces the corrosive wear and tear on production equipment under high-temperature, strong-alkali conditions, extending equipment lifespan. The production process is safe, clean, green, and low-carbon, meeting the industrialization requirements of green manufacturing for new energy materials.

[0028] Third, low cost. This invention features low raw material costs, low energy consumption, and significantly improved raw material utilization and product yield: Compared to traditional pure physical gas-phase activation processes, this invention leverages the activation energy reduction effect of acidic catalysts to significantly lower the activation reaction temperature and shorten the activation time, thereby greatly reducing production energy consumption and temperature control costs. Simultaneously, phosphorus-containing pre-pores achieve uniform and gentle etching of the entire material, avoiding the problems of excessive surface ablation, carbon skeleton collapse, and raw material waste associated with traditional physical activation. This effectively reduces raw material loss, improves carbon source utilization, and significantly increases product yield. While ensuring excellent electrochemical performance, it significantly reduces material and energy costs, demonstrating significant economic advantages for industrialization. Detailed Implementation

[0029] To enable those skilled in the art to better understand the technical solution of the present invention, the product of the present invention will be further described in detail below with reference to embodiments.

[0030] This invention relates to a method for preparing a phosphorus-doped high-capacity sodium-ion battery hard carbon anode material, comprising the following steps:

[0031] S1. Precursor mixing treatment: Carbon-containing raw materials and phosphorus-containing additives are uniformly mixed to obtain a uniformly dispersed mixed precursor.

[0032] S2. Pre-carbonization treatment: The mixed precursor obtained in step S1 is subjected to low-temperature pre-carbonization to obtain a pre-carbonized precursor.

[0033] S3. Activation treatment: The pre-carbonized precursor prepared in step S2 is uniformly mixed with the catalyst and activated to obtain a precursor rich in micropores.

[0034] S4. Surface coating modification treatment: The precursor rich in micropores after activation and pore formation in step S3 is uniformly mixed with the coating agent and subjected to surface modification coating treatment to obtain a surface-coated precursor.

[0035] S5. High-temperature sintering: The precursor coated on the surface in step S4 is subjected to high-temperature sintering treatment to finally obtain a high-performance hard carbon anode material.

[0036] Further, in step S1, the phosphorus-containing additive is one or more of phosphoric acid, pyrophosphoric acid, polyphosphoric acid, metaphosphoric acid, sodium dihydrogen phosphate, and potassium dihydrogen phosphate.

[0037] Further, in step S1, the amount of phosphorus-containing additive added is 0.5 to 5 wt% of the amount of carbon source added.

[0038] Furthermore, in step S2, the conditions for low-temperature pre-carbonization are: the protective atmosphere is nitrogen and / or argon, the pre-carbonization temperature is 400-700℃, and the holding time is 1-5h.

[0039] Further, in step S3, the catalyst is one or more of hydrochloric acid, sulfuric acid, nitric acid, oxalic acid, citric acid, benzoic acid, p-benzenesulfonic acid, and phosphoric acid, and the amount of the catalyst added is 0.5 to 2 wt.% of the carbonization precursor.

[0040] Further, in step S3, the activation conditions are: activation temperature of 500-800℃, activation time of 2-5h; and activation atmosphere of one or more of oxygen, air, water vapor, CO2, and CO.

[0041] Furthermore, in step S5, the conditions for high-temperature sintering are: a protective atmosphere of nitrogen and / or argon, a sintering temperature of 1100-1600℃, and a sintering holding time of 2-5h.

[0042] Further, in step S4, the coating agent is one or more of asphalt, phenolic resin, glucose, and polyacrylonitrile, and the amount of the coating agent added is 0.5 to 3 wt. of the precursor mass.

[0043] Furthermore, in step S1, the carbon-containing raw material is one or more of the following: coconut shell, walnut shell, wood chips, straw, bamboo, macadamia nut shell, corn cob, anthracite, lignite, bituminous coal, phenolic resin, and epoxy resin.

[0044] Another aspect of the present invention is to protect a hard carbon anode material for sodium-ion batteries, which is prepared by the above-described preparation method.

[0045] Example 1

[0046] This embodiment relates to a phosphorus-doped high-capacity sodium-ion battery hard carbon anode material, the preparation method of which includes the following steps:

[0047] S1. Precursor Mixing Treatment: The carbon-containing raw material and the phosphorus-containing additive are uniformly mixed to obtain a uniformly dispersed mixed precursor. Specifically, the phosphorus-containing additive is phosphoric acid or pyrophosphoric acid; the amount of phosphorus-containing additive added is 5 wt% of the amount of carbon source added; the carbon-containing raw material is coconut shell, walnut shell, wood chips, or epoxy resin.

[0048] S2. Pre-carbonization treatment: The mixed precursor obtained in step S1 is subjected to low-temperature pre-carbonization to obtain a pre-carbonized precursor. Specifically, the conditions for low-temperature pre-carbonization are: a protective atmosphere of nitrogen and argon, a pre-carbonization temperature of 700℃, and a holding time of 3 hours.

[0049] S3. Activation Treatment: The pre-carbonized precursor prepared in step S2 is uniformly mixed with the catalyst and activated to obtain a precursor rich in micropores. Specifically, the catalyst is hydrochloric acid, sulfuric acid, or phosphoric acid, and the amount of catalyst added is 2 wt.% of the mass of the carbonized precursor; the activation conditions are: activation temperature of 800℃, activation time of 3.5 h; and activation atmosphere of oxygen and air.

[0050] S4. Surface Coating Modification Treatment: The microporous precursor obtained after activation and pore-forming in step S3 is uniformly mixed with a coating agent, and surface modification coating treatment is performed to obtain a surface-coated precursor. Specifically, the coating agent is asphalt, phenolic resin, or glucose, and the amount of the coating agent added is 3 wt.% of the precursor mass.

[0051] S5. High-temperature sintering: The precursor coated in step S4 is subjected to high-temperature sintering to obtain a high-performance hard carbon anode material. Specifically, the high-temperature sintering conditions are: a protective atmosphere of nitrogen and argon, a sintering temperature of 1600℃, and a sintering holding time of 3.5h.

[0052] Example 2

[0053] This embodiment relates to a phosphorus-doped high-capacity sodium-ion battery hard carbon anode material, the preparation method of which includes the following steps:

[0054] S1. Precursor Mixing Treatment: The carbon-containing raw material and the phosphorus-containing additive are uniformly mixed to obtain a uniformly dispersed mixed precursor. Specifically, the phosphorus-containing additive is metaphosphoric acid, sodium dihydrogen phosphate, or potassium dihydrogen phosphate; the amount of phosphorus-containing additive added is 3 wt% of the carbon source; the carbon-containing raw material is corn cob, anthracite, lignite, bituminous coal, phenolic resin, or epoxy resin.

[0055] S2. Pre-carbonization treatment: The mixed precursor obtained in step S1 is subjected to low-temperature pre-carbonization to obtain a pre-carbonized precursor. Specifically, the conditions for low-temperature pre-carbonization are: nitrogen atmosphere, pre-carbonization temperature of 550℃, and holding time of 1 hour.

[0056] S3. Activation Treatment: The pre-carbonized precursor prepared in step S2 is uniformly mixed with the catalyst and activated to obtain a precursor rich in micropores. Specifically, the catalyst is oxalic acid and citric acid, and the amount of the catalyst added is 1 wt.% of the mass of the carbonized precursor; the activation conditions are: activation temperature of 500℃, activation time of h; and activation atmosphere of air.

[0057] S4. Surface Coating Modification Treatment: The microporous precursor obtained after activation and pore-forming in step S3 is uniformly mixed with a coating agent, and surface modification coating treatment is performed to obtain a surface-coated precursor. Specifically, the coating agent is asphalt or polyacrylonitrile, and the amount of the coating agent added is 2 wt.% of the precursor mass.

[0058] S5. High-temperature sintering: The precursor coated in step S4 is subjected to high-temperature sintering to obtain a high-performance hard carbon anode material. Specifically, the high-temperature sintering conditions are: nitrogen atmosphere, sintering temperature of 1300℃, and sintering holding time of 2 hours.

[0059] Example 3

[0060] This embodiment relates to a phosphorus-doped high-capacity sodium-ion battery hard carbon anode material, the preparation method of which includes the following steps:

[0061] S1. Precursor Mixing Treatment: The carbon-containing raw material and the phosphorus-containing additive are uniformly mixed to obtain a uniformly dispersed mixed precursor. Specifically, the phosphorus-containing additive is metaphosphoric acid or sodium dihydrogen phosphate; the amount of phosphorus-containing additive added is 0.5 wt% of the carbon source; the carbon-containing raw material is coconut shell, walnut shell, sawdust, corn cob, phenolic resin, or epoxy resin.

[0062] S2. Pre-carbonization treatment: The mixed precursor obtained in step S1 is subjected to low-temperature pre-carbonization to obtain a pre-carbonized precursor. Specifically, the conditions for low-temperature pre-carbonization are: argon atmosphere, pre-carbonization temperature of 400℃, and holding time of 5h.

[0063] S3. Activation Treatment: The pre-carbonized precursor prepared in step S2 is uniformly mixed with the catalyst and activated to obtain a precursor rich in micropores. Specifically, the catalyst is benzoic acid, p-benzenesulfonic acid, and phosphoric acid, and the amount of the catalyst added is 0.5 wt.% of the mass of the carbonized precursor; the activation conditions are: activation temperature of 800℃, activation time of 3.5 h; and activation atmosphere of water vapor.

[0064] S4. Surface Coating Modification Treatment: The microporous precursor obtained after activation and pore-forming in step S3 is uniformly mixed with a coating agent, and surface modification coating treatment is performed to obtain a surface-coated precursor. Specifically, the coating agent is asphalt, phenolic resin, or glucose, and the amount of the coating agent added is 0.5 wt.% of the precursor mass.

[0065] S5. High-temperature sintering: The precursor coated in step S4 is subjected to high-temperature sintering to obtain a high-performance hard carbon anode material. Specifically, the high-temperature sintering conditions are: argon atmosphere, sintering temperature of 1100℃, and sintering holding time of 5h.

[0066] Example 4

[0067] This embodiment relates to a phosphorus-doped high-capacity sodium-ion battery hard carbon anode material, the preparation method of which includes the following steps:

[0068] S1. Precursor Mixing Treatment: The carbon-containing raw material and the phosphorus-containing additive are uniformly mixed to obtain a uniformly dispersed mixed precursor. Specifically, the phosphorus-containing additive is phosphoric acid, pyrophosphoric acid, or polyphosphoric acid; the amount of phosphorus-containing additive added is 2 wt% of the amount of carbon source added; the carbon-containing raw material is coconut shell, walnut shell, wood chips, or epoxy resin.

[0069] S2. Pre-carbonization treatment: The mixed precursor obtained in step S1 is subjected to low-temperature pre-carbonization to obtain a pre-carbonized precursor. Specifically, the conditions for low-temperature pre-carbonization are: a protective atmosphere of nitrogen and argon, a pre-carbonization temperature of 500℃, and a holding time of 4 hours.

[0070] S3. Activation Treatment: The pre-carbonized precursor prepared in step S2 is uniformly mixed with the catalyst and activated to obtain a precursor rich in micropores. Specifically, the catalyst is oxalic acid, citric acid, and phosphoric acid, and the amount of the catalyst added is 1 wt.% of the mass of the carbonized precursor; the activation conditions are: activation temperature of 600℃, activation time of 3h; and activation atmosphere of CO2 and CO.

[0071] S4. Surface Coating Modification Treatment: The microporous precursor obtained after activation and pore-forming in step S3 is uniformly mixed with a coating agent, and surface modification coating treatment is performed to obtain a surface-coated precursor. Specifically, the coating agent is asphalt, phenolic resin, or glucose, and the amount of the coating agent added is 1 wt.% of the precursor mass.

[0072] S5. High-temperature sintering: The precursor coated in step S4 is subjected to high-temperature sintering to obtain a high-performance hard carbon anode material. Specifically, the high-temperature sintering conditions are: a protective atmosphere of nitrogen and argon, a sintering temperature of 1400℃, and a sintering holding time of 3 hours.

[0073] Example 5

[0074] This embodiment relates to a phosphorus-doped high-capacity sodium-ion battery hard carbon anode material, the preparation method of which includes the following steps:

[0075] S1. Precursor Mixing Treatment: The carbon-containing raw material and the phosphorus-containing additive are uniformly mixed to obtain a uniformly dispersed mixed precursor. Specifically, the phosphorus-containing additive is phosphoric acid, pyrophosphoric acid, or polyphosphoric acid; the amount of the phosphorus-containing additive is 0.5-5 wt% of the carbon source; the carbon-containing raw material is coconut shell, walnut shell, sawdust, straw, or bamboo.

[0076] S2. Pre-carbonization treatment: The mixed precursor obtained in step S1 is subjected to low-temperature pre-carbonization to obtain a pre-carbonized precursor. Specifically, the conditions for low-temperature pre-carbonization are: a protective atmosphere of nitrogen and argon, a pre-carbonization temperature of 600℃, and a holding time of 2 hours.

[0077] S3. Activation Treatment: The pre-carbonized precursor prepared in step S2 is uniformly mixed with the catalyst and activated to obtain a precursor rich in micropores. Specifically, the catalyst is hydrochloric acid or sulfuric acid, and the amount of catalyst added is 1.5 wt.% of the mass of the carbonized precursor; the activation conditions are: activation temperature of 600℃, activation time of 3h; and activation atmosphere of oxygen or air.

[0078] S4. Surface Coating Modification Treatment: The microporous precursor obtained after activation and pore-forming in step S3 is uniformly mixed with a coating agent, and surface modification coating treatment is performed to obtain a surface-coated precursor. Specifically, the coating agent is asphalt, phenolic resin, or glucose, and the amount of the coating agent added is 1 wt.% of the precursor mass.

[0079] S5. High-temperature sintering: The precursor coated in step S4 is subjected to high-temperature sintering to obtain a high-performance hard carbon anode material. Specifically, the high-temperature sintering conditions are: a protective atmosphere of nitrogen and argon, a sintering temperature of 1500℃, and a sintering holding time of 3 hours.

[0080] Application Example 1

[0081] This embodiment relates to a phosphorus-doped high-capacity sodium-ion battery hard carbon anode material, the preparation method of which includes the following steps:

[0082] S1. Precursor mixing treatment: Coconut shell powder is selected as the carbon-containing raw material. The coconut shell powder and phosphate additive are thoroughly and evenly mixed to obtain a composite mixed precursor. The mass of the phosphate additive is 3 wt. of the mass of the carbon-containing raw material.

[0083] S2. Pre-carbonization treatment: The mixed precursor obtained in step S1 is placed in a nitrogen atmosphere and heat-treated at a constant temperature of 500℃ for 2 hours to obtain the pre-carbonized precursor.

[0084] S3. Activation treatment: The pre-carbonized precursor prepared in step S2 is uniformly mixed with sulfuric acid catalyst, and then the composite material is placed in an air oxidizing atmosphere for activation treatment. The activation temperature is 600℃ and the activation time is 3h to obtain a precursor rich in micropores.

[0085] S4. Surface coating modification treatment: The porous carbon precursor prepared in step S3 is uniformly blended with a phenolic resin coating agent to obtain a coated modified carbon precursor; wherein, the mass of the added phenolic resin coating agent is 2% of the mass of the porous carbon precursor.

[0086] S5. High-temperature sintering: The coated modified material obtained in step S4 is placed in a nitrogen inert atmosphere for high-temperature sintering treatment. The sintering temperature is 1300℃ and the constant temperature sintering time is 3h to obtain the high-performance sodium-ion battery hard carbon anode material of Application Example 1.

[0087] Comparative Example 1

[0088] This embodiment relates to a hard carbon anode material for sodium-ion batteries, the preparation method of which includes the following steps:

[0089] S1. Pre-carbonization treatment: Coconut shell powder is selected as the carbon-containing raw material, and it is placed in a nitrogen atmosphere and heat-treated at a constant temperature of 500℃ for 2 hours to obtain the pre-carbonized precursor.

[0090] S2. Activation treatment: The pre-carbonized precursor prepared in step S2 is uniformly mixed with sulfuric acid catalyst, and then the composite material is placed in an air oxidizing atmosphere for activation treatment. The activation temperature is 600℃ and the activation time is 3h to obtain a precursor rich in micropores.

[0091] S3. Surface coating modification treatment: The porous carbon precursor prepared in step S2 is uniformly blended with a phenolic resin coating agent to obtain a coated modified carbon precursor; wherein, the mass of the added phenolic resin coating agent is 2% of the mass of the porous carbon precursor.

[0092] S4. High-temperature sintering: The coated modified material obtained in step S3 is placed in a nitrogen inert atmosphere for high-temperature sintering treatment. The sintering temperature is 1300℃ and the constant temperature sintering time is 3h to obtain the sodium-ion battery hard carbon anode material of Comparative Example 1.

[0093] Comparative Example 2

[0094] This embodiment relates to a hard carbon anode material for sodium-ion batteries, the preparation method of which includes the following steps:

[0095] S1. Precursor mixing treatment: Coconut shell powder is selected as the carbon-containing raw material. The coconut shell powder and phosphate additive are thoroughly and evenly mixed to obtain a composite mixed precursor. The mass of the phosphate additive is 3 wt. of the mass of the carbon-containing raw material.

[0096] S2. Pre-carbonization treatment: The mixed precursor obtained in step S1 is placed in a nitrogen atmosphere and heat-treated at a constant temperature of 500℃ for 2 hours to obtain the pre-carbonized precursor.

[0097] S3. Activation treatment: The pre-carbonized precursor prepared in step S2 is placed in an oxidizing atmosphere for activation treatment at an activation temperature of 600℃ for 3 hours to obtain a precursor rich in micropores.

[0098] S4. Surface coating modification treatment: The porous carbon precursor prepared in step S3 is uniformly blended with a phenolic resin coating agent to obtain a coated modified carbon precursor; wherein, the mass of the added phenolic resin coating agent is 2% of the mass of the porous carbon precursor.

[0099] S5. High-temperature sintering: The coated modified material obtained in step S4 is placed in a nitrogen inert atmosphere for high-temperature sintering treatment. The sintering temperature is 1300℃ and the constant temperature sintering time is 3h to obtain the sodium-ion battery hard carbon anode material of Comparative Example 2.

[0100] To fully verify the structural advantages and electrochemical performance gains brought about by the preparation method of this invention, systematic structural characterization and electrochemical performance testing were conducted on Application Example 1, Comparative Example 1, and Comparative Example 2 of this invention. The specific test results and mechanism analysis are as follows:

[0101] The specific surface area of ​​the uncoated porous carbon precursor after S3 activation treatment was tested. The specific surface areas of Application Example 1, Comparative Example 1, and Comparative Example 2 were 1062, 1380, and 950 m² / g, respectively. The precursor activated in Application Example 1 of this invention has a suitable and higher effective specific surface area, demonstrating that the dual activation system of phosphoric acid pre-opening and sulfuric acid acid catalysis can achieve efficient and uniform deep pore formation, constructing a rich microporous structure inside the carbon matrix, providing sufficient sodium storage sites, and avoiding the problems of disordered pores and excessive skeletal defects caused by traditional over-activation.

[0102] The true density test indirectly characterized the closed-pore content of the material. The test results showed that the true densities of Application Example 1, Comparative Example 1, and Comparative Example 2 were 1.80, 1.92, and 1.93 g / cm³, respectively. Application Example 1 showed a significantly lower true density, indicating a higher closed-pore content. This is because the present invention achieves a high proportion of open-pore structures through controllable activation via S3, and subsequent surface coating modification via S4 effectively transforms the open micropores into closed-pore structures. The closed-pore structure not only serves as an efficient sodium storage space, further increasing the sodium storage capacity of the material, but also effectively isolates the internal channels from direct contact with the electrolyte, greatly suppressing electrolyte side reactions during charging and discharging, reducing irreversible capacity loss, and further improving electrode interface stability and cycle life.

[0103] The specific surface area of ​​the final prepared hard carbon anode material was tested. The specific surface areas of Example 1, Comparative Example 1, and Comparative Example 2 were 4.6, 4.4, and 5.1 m² / g, respectively. The specific surface area of ​​the three groups of samples remained at a low level, demonstrating that the S4 carbon-based surface coating modification process of this invention has excellent interface control effect.

[0104] Constant current charge-discharge tests revealed that the first-week charging specific capacities of Application Example 1, Comparative Example 1, and Comparative Example 2 were 365, 320, and 316 mAh / g, respectively, and the first-week coulombic efficiencies were 92.5%, 91.4%, and 91.2%, respectively. It can be seen that the first-week reversible sodium storage capacity and first-week coulombic efficiency of Application Example 1 are significantly better than those of the two comparative examples.

[0105] The core mechanism of this performance advantage is as follows: This invention uses phosphorus-containing additives to etch the carbon matrix from the inside out during the pre-carbonization stage, constructing a three-dimensional through mass transfer channel, which completely solves the defect that traditional activation can only create pores on the surface; combined with subsequent acidic catalyst-assisted controllable gas-phase activation, a large number of uniformly distributed and reasonably sized effective sodium storage micropores can be constructed in situ inside the carbon matrix, while inhibiting the formation of ineffective mesopores and macropores, greatly increasing the number of effective sodium storage active sites, and significantly improving the reversible sodium storage capacity of hard carbon materials.

[0106] Meanwhile, the first-week coulombic efficiency of the three groups of finished products was relatively high. This is because the surface coating layer can effectively passivate the surface defects of the hard carbon material, cover the surface openings, significantly reduce the overall specific surface area of ​​the material, reduce the contact area between the electrolyte and the material surface, inhibit the disordered excessive growth of the SEI film, and greatly reduce the irreversible side reactions of charging and discharging, so that the final hard carbon anode material has a high first-week coulombic efficiency.

[0107] The 5C high current density rate performance of the three groups of samples was tested. The results showed that the 5C capacity retention rates of Application Example 1, Comparative Example 1, and Comparative Example 2 were 89.2%, 82.4%, and 80.6%, respectively. Application Example 1 of the present invention has superior high-rate discharge performance.

[0108] The reason for this is that the phosphorus element introduced into the precursor in the system of this invention achieves in-situ self-doping modification through high-temperature sintering, which can effectively break the regular stacking structure of the carbon layers and widen the interlayer spacing of hard carbon, providing sufficient space for the rapid insertion and extraction of large-radius sodium ions; at the same time, the constructed interconnected multi-level pore structure significantly shortens the sodium ion diffusion path and reduces ion transport resistance. Under the dual synergistic effect of phosphorus doping layer expansion and interconnected pore mass transfer, the electrochemical kinetic characteristics of the material are significantly optimized, the sodium ion migration rate is greatly improved, and ultimately it exhibits excellent rate performance.

[0109] In summary, this invention achieves multi-dimensional optimization of the pore structure, bulk lattice structure, and electrode interface structure of hard carbon materials through a synergistic process of phosphorus-containing pre-pore opening, acidic catalytic controllable activation, surface coating modification, and high-temperature phosphorus doping layer expansion. This completely breaks through the technical bottlenecks of traditional hard carbon materials, such as low capacity, poor kinetics, and unstable interfaces. While taking into account high capacity and high rate performance, it ensures excellent cycle stability and industrialization feasibility of the material.

[0110] The above embodiments are merely specific examples of the present invention, and their descriptions are quite specific and detailed, but they should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these obvious substitutions all fall within the protection scope of the present invention.

Claims

1. A method for preparing a phosphorus-doped high-capacity sodium-ion battery hard carbon anode material, characterized in that... Includes the following steps: S1. Precursor mixing treatment: Carbon-containing raw materials and phosphorus-containing additives are uniformly mixed to obtain a uniformly dispersed mixed precursor. S2. Pre-carbonization treatment: The mixed precursor obtained in step S1 is subjected to low-temperature pre-carbonization to obtain a pre-carbonized precursor. S3. Activation treatment: The pre-carbonized precursor prepared in step S2 is uniformly mixed with the catalyst and activated to obtain a precursor rich in micropores. S4. Surface coating modification treatment: The precursor rich in micropores after activation and pore formation in step S3 is uniformly mixed with the coating agent and subjected to surface modification coating treatment to obtain a surface-coated precursor. S5. High-temperature sintering: The precursor coated on the surface in step S4 is subjected to high-temperature sintering treatment to finally obtain a high-performance hard carbon anode material.

2. The method for preparing phosphorus-doped high-capacity sodium-ion battery hard carbon anode material according to claim 1, characterized in that: In step S1, the phosphorus-containing additive is one or more of phosphoric acid, pyrophosphoric acid, polyphosphoric acid, metaphosphoric acid, sodium dihydrogen phosphate, and potassium dihydrogen phosphate.

3. The method for preparing phosphorus-doped high-capacity sodium-ion battery hard carbon anode material according to claim 1, characterized in that: In step S1, the amount of phosphorus-containing additive added is 0.5 to 5 wt% of the amount of carbon source added.

4. The method for preparing phosphorus-doped high-capacity sodium-ion battery hard carbon anode material according to claim 1, characterized in that: In step S2, the conditions for low-temperature pre-carbonization are: the protective atmosphere is nitrogen and / or argon, the pre-carbonization temperature is 400-700℃, and the holding time is 1-5h.

5. The method for preparing phosphorus-doped high-capacity sodium-ion battery hard carbon anode material according to claim 1, characterized in that: In step S3, the catalyst is one or more of hydrochloric acid, sulfuric acid, nitric acid, oxalic acid, citric acid, benzoic acid, p-benzenesulfonic acid, and phosphoric acid, and the amount of the catalyst added is 0.5 to 2 wt. of the carbonization precursor.

6. The method for preparing phosphorus-doped high-capacity sodium-ion battery hard carbon anode material according to claim 1, characterized in that: In step S3, the activation conditions are: activation temperature of 500-800℃, activation time of 2-5h; and activation atmosphere of one or more of oxygen, air, water vapor, CO2, and CO.

7. The method for preparing phosphorus-doped high-capacity sodium-ion battery hard carbon anode material according to claim 1, characterized in that: In step S5, the conditions for high-temperature sintering are: the protective atmosphere is nitrogen and / or argon, the sintering temperature is 1100-1600℃, and the sintering holding time is 2-5h.

8. The method for preparing phosphorus-doped high-capacity sodium-ion battery hard carbon anode material according to claim 1, characterized in that: In step S4, the coating agent is one or more of asphalt, phenolic resin, glucose, and polyacrylonitrile, and the amount of the coating agent added is 0.5 to 3 wt. of the precursor mass.

9. The method for preparing phosphorus-doped high-capacity sodium-ion battery hard carbon anode material according to claim 1, characterized in that: In step S1, the carbon-containing raw material is one or more of the following: coconut shell, walnut shell, wood chips, straw, bamboo, macadamia nut shell, corn cob, anthracite, lignite, bituminous coal, phenolic resin, and epoxy resin.

10. A hard carbon anode material for sodium-ion batteries, characterized in that: It is prepared by any one of the preparation methods described in claims 1-9.