A graphene modification method based on gas-solid interface activation
By using 2-methyleneglutarate preloading and pulsed plasma gas-solid interface activation, the problem of maintaining hydrophilicity, dispersion stability, and sp2 conjugated structure in graphene modification was solved, thus improving the stability and conductivity of graphene surface functionalization.
Patent Information
- Application Number
- CN202611627230.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-21
- Publication Date
- 2026-11-17
AI Technical Summary
Existing graphene modification methods struggle to simultaneously improve hydrophilicity and dispersion stability while maintaining the integrity of the sp2 conjugated structure. Furthermore, organic capping layers can increase interfacial resistance and lead to homopolymerization of free monomers.
After preloading graphene with a low dose of 2-methyleneglutarate, the unsaturated double bonds are directionally grafted onto the active sites on the graphene surface through pulsed plasma gas-solid interface activation in a weakly oxidizing atmosphere of argon, carbon dioxide, and water vapor, thus avoiding monomer homopolymerization and excessive oxidation.
This improved the hydrophilicity and dispersion stability of graphene while maintaining the integrity of the sp2 conjugated structure, reducing the formation of organic capping layers, and enhancing the application effect of modified graphene in composite materials.
Smart Images

Figure CN123105622A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of surface functionalization of carbon nanomaterials and graphene modification technology, and particularly to a graphene modification method based on gas-solid interface activation. Background Technology
[0002] Graphene is composed of carbon atoms arranged in sp... 2 Two-dimensional layered carbon materials with hybrid structures have high carrier mobility, good electrical conductivity, high specific surface area and excellent mechanical properties, and have great application potential in fields such as conductive composite materials, energy storage materials, functional coatings and inorganic composite materials.
[0003] However, graphene sheets exhibit strong π-π interactions and van der Waals interactions, and unmodified graphene surfaces have low polarity and poor hydrophilicity, making them prone to re-stacking and aggregation in aqueous or other polar media. Aggregation reduces the effective specific surface area of graphene and affects its uniform distribution and interfacial contact within the composite system, thus hindering the full utilization of graphene's conductivity, reinforcing properties, and interfacial modulation capabilities. Therefore, appropriately functionalizing the graphene surface to improve its wettability and liquid-phase dispersion stability is a crucial technical approach for achieving efficient graphene utilization.
[0004] Existing methods for hydrophilicating graphene mainly include strong oxidation treatment, graphene oxide reduction treatment, surfactant adsorption, coupling agent modification, polymer coating, and free radical grafting. Strong acid or strong oxidant treatment can introduce oxygen-containing functional groups such as hydroxyl, carboxyl, and epoxy groups onto the graphene surface, thereby improving its hydrophilicity. However, strong oxidation processes easily disrupt the continuous spline structure of graphene. 2 Conjugated structures can lead to more structural defects and may reduce the electrical conductivity of materials.
[0005] Coating or adsorbing graphene with polymers, surfactants, or coupling agents can improve its dispersion in the liquid phase. However, when high levels of organic modifiers are added, a continuous or thick organic coating layer can easily form on the graphene surface. On the one hand, this organic coating layer may increase the interfacial resistance between graphene sheets; on the other hand, a large amount of organic matter may also act as a bridging agent between sheets during drying, leading to re-aggregation of graphene. Furthermore, modifiers that rely solely on physical adsorption may desorb during subsequent washing, dispersion, or use, affecting the stability of the modification effect.
[0006] Radical grafting using organic monomers containing unsaturated bonds is another method to improve the functionalization stability of graphene surfaces. This type of method typically requires the use of thermal initiators, redox initiators, or other chemical initiation systems to generate free radicals, causing the organic monomers to graft onto the carbon material. However, during the free radical reaction, the homopolymerization of the organic monomers and the interfacial grafting reaction usually occur simultaneously. When the monomer concentration is high or free radicals are continuously generated, monomer oligomers or polymers are easily formed, leading to a continuous organic layer on the graphene surface. This creates a conflict between surface functionalization and maintaining the conductive structure.
[0007] Low-temperature plasma offers advantages such as rapid reaction speed, low processing temperature, and no need for large amounts of chemical initiators. It can activate the graphene surface through active species such as electrons, free radicals, and excited-state particles. Oxygen-containing atmospheres such as oxygen, air, water vapor, and carbon dioxide can all generate oxygen-containing active particles under plasma conditions, forming active sites or oxygen-containing functional groups on the graphene surface. However, when graphene is directly treated with continuous oxidizing plasma, the active particles continuously bombard the graphene surface, which can easily increase surface etching and carbon framework defects while improving hydrophilicity. At higher oxidation levels, the sp... 2 Disruption of the conjugated structure can lead to a decrease in electrical conductivity. Therefore, current plasma treatment methods still face the challenge of simultaneously achieving a high degree of surface functionalization and maintaining the carbon framework structure.
[0008] Furthermore, if organic monomers are directly mixed with graphene and the entire liquid system is evaporated to dryness, the free monomers that are not adsorbed by graphene in the liquid phase will also precipitate and deposit on the graphene surface or between the sheets during solvent evaporation. Under subsequent plasma action, a large number of free monomers are prone to continuous homopolymerization, thus forming a thick organic layer, making it difficult to obtain a low-coverage, stable and uniform interfacial functionalized structure.
[0009] Therefore, it is necessary to develop a novel graphene modification method that, while controlling the loading of organic precursors, reduces free monomer deposition and achieves interfacial activation between graphene and organic precursors through mild, intermittent plasma energy input. This allows for preferential interfacial grafting reactions while minimizing homopolymerization of organic monomers and excessive oxidation of the graphene matrix, thus balancing the hydrophilicity, dispersion stability, and sp. 2 Preservation of conjugate structure. Summary of the Invention
[0010] The purpose of this invention is to address the shortcomings of existing technologies by proposing a graphene modification method based on gas-solid interface activation.
[0011] This invention employs low-dose 2-methyleneglutarate to preload graphene in the liquid phase. After adsorption, unadsorbed free monomers are removed by solid-liquid separation. Then, pulsed plasma gas-solid interface activation is performed in a weakly oxidizing atmosphere of argon / carbon dioxide / water vapor, causing the unsaturated double bonds of 2-methyleneglutarate to undergo a directional grafting reaction with the active sites on the graphene surface. Through the synergistic effect of four steps—low-coverage preloading, free monomer removal, pulsed intermittent energy input, and a weakly oxidizing two-component atmosphere—the hydrophilicity and dispersion stability of graphene are improved, while the degree of monomer homopolymerization and graphene over-oxidation is reduced.
[0012] To achieve the above objectives, the present invention adopts the following technical solution:
[0013] This invention first proposes a graphene modification method based on gas-solid interface activation, comprising the following steps:
[0014] (1) Graphene is added to a liquid medium for dispersion to depolymerize the aggregated graphene and obtain a graphene dispersion system.
[0015] (2) Add 2-methyleneglutaric acid to the graphene dispersion system to allow 2-methyleneglutaric acid to fully contact with the graphene and adsorb onto the graphene surface, wherein the amount of 2-methyleneglutaric acid added is 0.05% to 5% of the graphene mass;
[0016] 2-Methyleneglutarate (2-MGA) has a structure containing one unsaturated double bond and two carboxyl groups. During liquid-phase dispersion, graphene aggregates are mechanically stirred, subjected to high shear, or ultrasonically depolymerized; 2-MGA depolymerizes through hydrogen bonding between the carboxyl groups and graphene edges / defects, and through the double bond and sp... 2 π-π interactions within the domain adsorb onto the graphene surface. Since the amount added is less than 5% of the graphene mass, 2-MGA mainly exists as discrete molecules, small molecule aggregates, or discontinuous low-coverage states, avoiding the formation of a continuous organic coating layer.
[0017] (3) After adsorption is completed, the system obtained in step (2) is subjected to solid-liquid separation to remove at least part of the unadsorbed free 2-methyleneglutaric acid in the liquid phase, and then the residual liquid phase medium in the solid phase is removed to obtain graphene with 2-methyleneglutaric acid preloaded on the surface.
[0018] If the entire liquid system is directly evaporated, free 2-MGA will precipitate and deposit on the graphene surface or between the sheets during solvent evaporation. Subsequent plasma treatment can easily lead to continuous homopolymerization, forming a thick organic layer and causing bridging between the sheets. After solid-liquid separation, residual liquid phase is removed by vacuum drying, reduced pressure drying, freeze drying, low-temperature airflow drying, or spray drying, allowing 2-MGA to be pre-loaded onto the graphene surface in a discrete distribution.
[0019] (4) The graphene with 2-methylene glutaric acid preloaded on the surface obtained in step (3) is placed in a weak oxidizing atmosphere composed of argon, carbon dioxide and water vapor for pulsed plasma treatment, wherein argon is the working gas, carbon dioxide and water vapor are oxygen-containing active components, and the active particles generated by the pulsed plasma activate the gas-solid interface of the graphene surface and the preloaded 2-methylene glutaric acid, so that the unsaturated double bond of 2-methylene glutaric acid reacts with the active sites on the graphene surface, and the organic structure containing dicarboxyl groups is grafted and fixed on the graphene surface.
[0020] Graphene pre-loaded with 2-MGA was subjected to pulsed plasma treatment in a weakly oxidizing atmosphere of Ar / CO2 / H2O. Electrons, Ar*, and Ar2O were generated in the gas phase. + Active species such as OH, O, CO, and H are present. These active particles simultaneously interact with graphene and pre-loaded 2-MGA at the gas-solid interface.
[0021] For graphene: at edges, defects, and local sp. 2 The domain generates a controlled number of active sites, such as carbon free radicals and oxygen-containing groups, but avoids deep etching caused by continuous strong oxidation;
[0022] For 2-MGA: activate its unsaturated double bond, allowing the double bond to enter a free radical or excited state;
[0023] Interfacial reaction: The activated 2-MGA double bond undergoes free radical addition, free radical coupling, hydrogen transfer and other reactions with the active sites on the graphene surface, fixing 2-MGA to the graphene surface through double bond grafting, while the two carboxyl groups are retained on the outside of the grafted structure.
[0024] This results in an organic graft structure containing dicarboxyl groups. This structure remains on the graphene surface after being washed with a liquid medium capable of dissolving 2-MGA, indicating that it is not a simple physical adsorption.
[0025] Pulsed plasma employs an intermittent discharge mode with periodic on / off cycles. The ON phase generates plasma-active particles, forming active sites on the graphene surface and the 2-MGA double bonds. The OFF phase ceases continuous bombardment, providing time for interfacial radical addition, migration, and termination reactions. Compared to continuous plasma, the pulsed mode reduces the probability of continuous homopolymerization of 2-MGA and excessive graphene oxidation, making the reaction more likely to occur at the "graphene surface-preloaded 2-MGA" interface, rather than between gaseous phase or free monomers.
[0026] (5) The product obtained in step (4) is washed to remove the unstable 2-methyleneglutarate and soluble oligomers, and then dried to obtain modified graphene.
[0027] Removes physically adsorbed 2-MGA and unstable soluble oligomers, while retaining the stable grafted dicarboxyl-containing organic structure after interfacial activation.
[0028] Preferably, the liquid medium in step (1) is at least one of water, ethanol, and isopropanol; the dispersion is performed by mechanical stirring with a shear rate of 10,000–45,000 s. -1 At least one of the following methods: high-shear dispersion and ultrasonic dispersion.
[0029] Preferably, in step (2), the amount of 2-methyleneglutarate added is 0.1% to 2% of the mass of graphene.
[0030] Preferably, in step (2), 2-methyleneglutaric acid is pre-dissolved in a liquid medium to form a 2-methyleneglutaric acid solution, and then the 2-methyleneglutaric acid solution is continuously, batch-wise, or dropwise added to the graphene dispersion system. Under stirring or ultrasonic conditions, 2-methyleneglutaric acid is adsorbed onto the graphene surface to form sp... 3 2-Methyleneglutarate preloaded state with low coverage and discontinuous distribution of carbon content less than 5%.
[0031] Preferably, the solid-liquid separation in step (3) employs at least one of filtration, vacuum filtration, centrifugation, and membrane separation to remove free 2-methyleneglutarate that is not adsorbed onto the graphene surface in the liquid phase before removing the liquid phase medium; the removal of the residual liquid phase medium employs at least one of vacuum drying, reduced pressure drying, freeze drying, low temperature airflow drying at 50-90°C, or spray drying.
[0032] Preferably, in step (4), the weak oxidizing atmosphere is argon as the balance gas, the volume fraction of carbon dioxide is 0.5% to 5%, the volume fraction of water vapor is 0.01% to 1%, and the balance is argon.
[0033] Ar is the primary working gas and carrier gas, while CO2 and H2O are oxygen-containing active components. Under plasma irradiation, CO2 and H2O generate appropriate amounts of oxygen-containing active particles such as O, OH, and CO, which can synergistically activate the graphene surface and 2-MGA double bonds, and introduce appropriate polar groups. Compared to the strong oxidizing atmosphere of O2, the Ar / CO2 / H2O system is milder, improving hydrophilicity and dispersion stability while reducing defects and resistivity increases in the graphene carbon framework. The synergistic effect of either CO2 or H2O alone is less effective than that of the two.
[0034] Preferably, the pulsed plasma in step (4) is one of dielectric barrier discharge plasma, pulsed glow discharge plasma, pulsed radio frequency plasma or pulsed microwave plasma; the pulsed plasma adopts an intermittent discharge mode of periodic on and off, with a duty cycle of 5% to 80% and a cumulative effective processing time of 0.1 to 60s.
[0035] The present invention also proposes a modified graphene, which is prepared by the aforementioned graphene modification method. The surface of the modified graphene has a dicarboxyl-containing organic graft structure formed by the interfacial activation reaction of the unsaturated double bond of 2-methyleneglutarate. The dicarboxyl-containing organic graft structure is stably bonded to the graphene surface and remains on the graphene surface after washing with a liquid medium capable of dissolving 2-methyleneglutarate.
[0036] Preferably, the modified graphene maintains the sp(s) content of the graphene matrix while introducing a dicarboxyl-containing organic graft structure. 2 Conjugated carbon structure.
[0037] Compared with the prior art, the beneficial effects of the present invention are:
[0038] 1. This invention utilizes a pre-process involving low-dose liquid-phase adsorption, solid-liquid separation to remove free monomers, and drying to obtain discrete pre-loaded powders. This process alters the morphology of the organic precursor, inhibiting homopolymerization and sheet bridging of organic monomers. In existing technologies, if unsaturated monomers are directly mixed with graphene in a liquid phase and then evaporated, a large number of unadsorbed free monomers in the liquid phase will evaporate with the solvent and precipitate, depositing on the surface and interlayer spaces of the graphene sheets. Under subsequent activation conditions, these monomers readily undergo intermolecular homopolymerization, forming a continuous organic coating layer on the graphene surface. This increases the interfacial resistance of the sheets and also causes secondary agglomeration due to sheet bridging. This invention first removes most of the free 2-methyleneglutarate through solid-liquid separation, retaining only the monomers already adsorbed on the graphene surface, so that the monomers are distributed on the graphene surface in a discrete, discontinuous, low-coverage state. In the subsequent plasma activation process, the interfacial grafting reaction between graphene and monomers occurs preferentially, rather than the homopolymerization reaction between monomer molecules. While introducing carboxyl groups to improve hydrophilicity, it avoids the formation of a thick organic coating layer and takes into account the conductivity of the modified graphene.
[0039] 2. This invention employs a weakly oxidizing atmosphere composed of argon-carbon dioxide-water vapor combined with pulsed intermittent plasma discharge. Through time-dimensional energy control, it decouples the generation of active sites from oxidation etching and monomer homopolymerization side reactions, thereby achieving interface activation grafting while reducing the sp. 2 Structural damage to the carbon framework. Traditional continuous discharge plasma or strong oxygen oxidizing plasma, with active particles continuously bombarding the graphene surface, not only continuously etches the carbon framework but also significantly damages spline structure. 2The conjugated structure leads to a surge in defect density and a significant increase in resistivity; on the other hand, the continuously generated free radicals drive the rapid intermolecular homopolymerization of the pre-loaded monomers. This invention employs a pulsed discharge system with alternating discharge and rest phases: during the discharge phase, plasma generates active particles, creating a limited number of active sites on the graphene surface, while simultaneously activating the carbon-carbon double bonds of the pre-loaded 2-methyleneglutarate; during the rest phase, high-energy particle input is stopped, providing a reaction window for interfacial free radical addition and coupling reactions between the double bonds and the graphene active sites, preventing continuous energy accumulation. Simultaneously, a weakly oxidizing atmosphere composed of CO2 and water vapor replaces the strong oxidizing system of pure oxygen, providing only moderately oxygen-containing active species for interfacial activation, avoiding excessive oxidation and etching, and achieving the technical effect of "moderate surface functionalization and minimal damage to the carbon skeleton."
[0040] 3. This invention relies on the gas-solid interface activation grafting mechanism to achieve chemical bonding and fixation of organic structures containing dicarboxyl groups, overcoming the inherent defect of easy desorption of functional groups in simple physical adsorption modification, and significantly improving the dispersion stability of modified graphene in aqueous phase, especially in complex alkaline calcium-containing aqueous environments. Existing physical adsorption modification methods rely on van der Waals forces and weak intermolecular forces to attach organic molecules to the graphene surface. During washing and liquid-phase dispersion, the modified organic molecules are easily re-desorbed back into the liquid phase system, and the modification effect rapidly diminishes. Traditional liquid-phase initiation grafting processes are accompanied by a large amount of homopolymer impurities, and the physically encapsulated polymer will also gradually dissolve and fall off after solvent immersion. This invention, under gas-solid plasma activation conditions, causes the unsaturated double bonds of 2-methyleneglutarate to undergo a covalent grafting reaction with the active sites on the graphene surface, anchoring the organic structure carrying dicarboxyl groups to the graphene surface in the form of chemical bonds. The subsequent washing process can completely remove the physically adsorbed free monomers and soluble oligomers, and the remaining carboxyl grafted structure has excellent elution resistance. The stable presence of dicarboxyl functional groups enhances the surface polarity of graphene and can resist the shielding effect of cations on negatively charged groups in alkaline calcium ion systems. This allows modified graphene to maintain good dispersion in the typical high-calcium alkaline environment of cement-based materials, expanding the application scenarios of graphene in inorganic cementitious composite materials. Attached Figure Description
[0041] Figure 1 This is a schematic diagram of the graphene modification method proposed in this invention;
[0042] Figure 2 This is a schematic diagram of the 2-methyleneglutarate preloading and pulsed plasma gas-solid interface activation and grafting mechanism proposed in this invention;
[0043] Figure 3 This is a schematic diagram showing the pulsed plasma discharge timing and the comparison of the effects of pulsed discharge and continuous discharge in this invention;
[0044] Figure 4This is a SEM image of the graphene after plasma modification in Example 2;
[0045] Figure 5 for Figure 4 A magnified view of a portion of the image;
[0046] Figure 6 A comparison of the Raman spectra of the original graphene sample and the graphene-modified sample obtained in Example 1;
[0047] Figure 7 The image shows a comparison of the infrared spectra of the original graphene sample and the graphene-modified sample obtained in Example 1. Detailed Implementation
[0048] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with existing known technologies. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments.
[0049] Basic process conditions:
[0050] The graphene modification method of the present invention is as follows: Figure 1 As shown, the process includes steps such as liquid phase dispersion, monomer adsorption preloading, solid-liquid separation and drying, pulsed plasma gas-solid interface activation, washing and drying.
[0051] 10g of graphene was weighed and added to a mixture of 500mL of ethanol and water, with a volume ratio of ethanol to water of 7:3. The graphene was depolymerized by mechanical stirring combined with ultrasonic dispersion. The ultrasonic dispersion time was 20min, followed by mechanical stirring for another 30min to obtain a graphene dispersion system.
[0052] The specified mass of 2-methyleneglutarate was pre-dissolved in 50 mL of ethanol / water mixture and slowly added to the graphene dispersion system under continuous stirring. After the addition was completed, stirring was continued for 60 min to allow 2-methyleneglutarate to fully contact with the graphene and adsorb onto the graphene surface.
[0053] Its mechanism is as follows Figure 2 As shown in the figure, (A) is the liquid-phase preloading stage, where 2-methylene glutaric acid molecules are weakly adsorbed on the graphene surface; (B) is the Ar / CO2 / H2O pulsed plasma activation stage, where active particles are generated at the gas-solid interface, and the graphene surface and preloaded monomers are activated at the same time, and the double bonds undergo interfacial grafting reaction; (C) is after washing, where free monomers and soluble oligomers are removed, and only the covalently stable grafted dicarboxyl structure is retained.
[0054] After adsorption, solid-liquid separation was performed by vacuum filtration to remove unadsorbed free 2-methyleneglutarate from the liquid phase. The resulting solid phase was not washed with a large amount of solvent to avoid excessive desorption of 2-methyleneglutarate already adsorbed on the graphene surface. The resulting wet graphene was vacuum dried at 40°C for 12 h to obtain graphene pre-loaded with 2-methyleneglutarate on its surface.
[0055] Unless otherwise specified, pulsed plasma treatment is performed using a dielectric barrier discharge device under normal pressure conditions.
[0056] 2-Methyleneglutarate, pre-loaded on the graphene surface, undergoes interfacial activation under the action of pulsed plasma active particles. Its unsaturated double bonds react with active sites on the graphene surface to form an organic graft structure containing dicarboxyl groups. The working atmosphere consists of Ar, CO2, and H2O, with a total gas flow rate of 2.0 L / min, of which CO2 volume fraction is 3.0%, H2O volume fraction is 0.3%, and the balance is Ar. Water vapor is introduced through a controlled water vapor generation unit.
[0057] The pulsed plasma employs an intermittent discharge method with periodic on and off cycles, alternating between discharge and non-discharge phases. The peak voltage of the pulsed discharge is 12 kV, and the pulse frequency is 1 kHz. Except for the embodiment studying the effect of duty cycle, the pulse duty cycle is set to 30%, and the total processing time is 30 seconds.
[0058] During plasma treatment, the graphene powder is intermittently agitated so that graphene at different locations can be exposed more evenly to the plasma active region.
[0059] Its mechanism is as follows Figure 3 As shown, (a) represents the intermittent discharge sequence of pulsed plasma, divided into an ON discharge phase and an OFF rest phase; (b) compares the reaction pathways of continuous plasma and pulsed plasma: continuous plasma easily induces monomer homopolymerization and excessive oxidation of graphene; pulsed plasma achieves preferential grafting at the interface, suppresses homopolymerization side reactions, and protects graphene sp. 2 Conjugate skeleton.
[0060] After processing, the obtained graphene was thoroughly washed with an ethanol / water mixture to remove unstable 2-methyleneglutarate and soluble oligomers, and then vacuum dried at 40°C to obtain modified graphene.
[0061] Example 1:
[0062] The graphene was processed according to the basic process described above, with 2-methyleneglutaric acid added at 0.25% of the graphene mass. For 10g of graphene, 25mg of 2-methyleneglutaric acid was added. After liquid-phase adsorption, solid-liquid separation, and vacuum drying, the graphene was treated with pulsed dielectric barrier discharge plasma in a weak oxidizing atmosphere of Ar / 3.0%CO2 / 0.3%H2O, with a pulse duty cycle of 30% and a total treatment time of 30s. The treated sample was washed and dried to obtain the modified graphene of Example 1.
[0063] Example 2:
[0064] This embodiment is basically the same as Example 1, except that the amount of 2-methyleneglutaric acid added is 0.50% of the graphene mass. For 10g of graphene, 50mg of 2-methyleneglutaric acid is added. The plasma working atmosphere is Ar / 3.0%CO2 / 0.3%H2O, the pulse duty cycle is 30%, and the total processing time is 30s. This embodiment is one of the preferred embodiments of the present invention.
[0065] Example 3:
[0066] This embodiment is basically the same as Example 2, except that the amount of 2-methyleneglutaric acid added is 1.00% of the graphene mass. For 10g of graphene, 100mg of 2-methyleneglutaric acid is added. The remaining liquid phase preloading, solid-liquid separation, drying, pulsed plasma treatment, washing, and secondary drying conditions are the same as in Example 2.
[0067] Example 4:
[0068] This embodiment is basically the same as Example 2, except that the amount of 2-methyleneglutaric acid added is 2.00% of the graphene mass. For 10g of graphene, 200mg of 2-methyleneglutaric acid is added. The other conditions are the same as in Example 2.
[0069] Example 5:
[0070] This example was used to investigate the modification effect under low pulse duty cycle conditions. The amount of 2-methyleneglutarate added was 0.50% of the graphene mass, the plasma working atmosphere was Ar / 3.0%CO2 / 0.3%H2O, the pulse frequency was 1kHz, and the total processing time was 30s. Unlike Example 2, the pulse duty cycle was set to 10%. All other process conditions were the same as in Example 2.
[0071] Example 6:
[0072] This embodiment is basically the same as Example 5, except that the amount of 2-methyleneglutarate added is 0.50%, the plasma atmosphere is Ar / 3.0%CO2 / 0.3%H2O, and the total processing time is 30s. The pulse duty cycle is set to 20%. The remaining conditions are the same as in Example 2.
[0073] Example 7:
[0074] This embodiment is basically the same as Example 2, except that the amount of 2-methyleneglutarate added is 0.50%, the plasma atmosphere is Ar / 3.0%CO2 / 0.3%H2O, and the total processing time is 30s. The pulse duty cycle is set to 50%. All other conditions are the same as in Example 2.
[0075] Example 8:
[0076] This embodiment is basically the same as Example 2, except that the amount of 2-methyleneglutarate added is 0.50%, the plasma atmosphere is Ar / 3.0%CO2 / 0.3%H2O, and the total processing time is 30s. The pulse duty cycle is set to 70%. All other conditions are the same as in Example 2.
[0077] The following comparison model was also set:
[0078] Comparative Example 1:
[0079] Untreated raw graphene was used as Comparative Example 1. This sample was used to determine the raw Raman spectrum ID / IG, resistivity, water contact angle, and 24-hour liquid phase dispersion retention of the graphene.
[0080] Comparative Example 2:
[0081] Liquid-phase treatment was performed according to Example 2, wherein the amount of 2-methyleneglutaric acid added was 0.50% of the graphene mass. After 2-methyleneglutaric acid adsorption and solid-liquid separation, the sample was vacuum dried, but without plasma treatment. The resulting sample was directly washed thoroughly with the same ethanol / water mixture as in Example 2, and then dried. This comparative example was used to evaluate the effect of simple 2-methyleneglutaric acid liquid-phase pretreatment on graphene properties and to determine the stability of 2-methyleneglutaric acid physisorption without plasma activation.
[0082] Comparative Example 3:
[0083] This comparative example does not include 2-methyleneglutarate. Graphene, after undergoing the same liquid-phase dispersion and vacuum drying, was directly subjected to pulsed plasma treatment in a weak oxidizing atmosphere of Ar / 3.0%CO2 / 0.3%H2O. The pulse duty cycle was 30%, and the total treatment time was 30 s. This comparative example was used to evaluate the effect of the weak oxidizing pulsed plasma itself on the hydrophilicity, structure, and conductivity of graphene.
[0084] Comparative Example 4:
[0085] Preloading, solid-liquid separation, and drying of 2-methyleneglutarate were performed according to Example 2. The plasma working atmosphere remained Ar / 3.0%CO2 / 0.3%H2O, but the pulsed discharge was changed to continuous discharge, and the total treatment time was maintained at 30 s. The treated samples were washed and dried according to the method of Example 2. This comparative example was used to evaluate the differences between continuous plasma and pulsed plasma in terms of graphene structural damage, conductivity, hydrophilicity, and liquid phase dispersion stability.
[0086] Comparative Example 5:
[0087] Preloading, solid-liquid separation, and drying of 2-methyleneglutarate were performed according to Example 2. Pure Ar was used as the working gas during the plasma treatment stage, without the addition of CO2 or H2O. A pulsed discharge mode was used with a duty cycle of 30%, and the total treatment time was 30 s. All other conditions were the same as in Example 2. This comparative example was used to evaluate the activation effect of pure Ar plasma on the 2-methyleneglutarate / graphene interface.
[0088] Comparative Example 6:
[0089] 2-Methyleneglutarate preloading, solid-liquid separation, and drying were performed according to Example 2. The plasma working atmosphere was a mixture of Ar and CO2, with CO2 volume fraction of 3.0% and the balance being Ar; no water vapor was added. The pulse duty cycle was 30%, and the total processing time was 30 s. All other conditions were the same as in Example 2. This comparative example was used to evaluate the role of CO2 as a single oxygen-containing active component.
[0090] Comparative Example 7:
[0091] 2-Methyleneglutarate preloading, solid-liquid separation, and drying were performed according to Example 2. The plasma working atmosphere was a mixture of Ar and H2O, with H2O volume fraction of 0.3% and the balance being Ar; no CO2 was added. The pulse duty cycle was 30%, and the total processing time was 30 s. All other conditions were the same as in Example 2. This comparative example was used to evaluate the role of water vapor as a single oxygen-containing active component.
[0092] Comparative Example 8:
[0093] Preloading, solid-liquid separation, and drying of 2-methyleneglutarate were performed according to Example 2. The plasma working atmosphere was a mixture of Ar and O2, with O2 volume fraction of 3.0% and the remainder being Ar. The pulse duty cycle was 30%, and the total processing time was 30 s. The remaining processing, washing, and drying conditions were the same as in Example 2. This comparative example was used to evaluate the effect of a strong oxidizing plasma atmosphere on the hydrophilic modification of graphene, as well as the carbon framework structure and electrical conductivity.
[0094] Characterization and evaluation methods:
[0095] To evaluate the structural integrity, electrical conductivity, surface wettability, and liquid-phase dispersion stability of the modified graphene prepared in this invention, the original graphene, the modified graphene obtained from different embodiments, and the comparative sample were characterized and compared under the same test conditions.
[0096] The symbols used in this section are explained below:
[0097] ID / IG is the ratio of the peak intensities of the D peak to the G peak in the Raman spectrum; Δ(ID / IG) is the change in ID / IG before and after modification;
[0098] ρ is resistivity, with units of Ω·cm; Rρ is the rate of change of resistivity;
[0099] θ is the water contact angle, in degrees; Δθ is the decrease in water contact angle before and after modification.
[0100] A0 is the absorbance at the initial dispersion; At is the absorbance after a settling time t, where t is the settling time in hours.
[0101] St represents the dispersion retention rate after a settling time t, expressed as % .
[0102] Ar is the chemical symbol for argon; C is the symbol for carbon; H is the symbol for hydrogen; O is the symbol for oxygen.
[0103] sp is a prefix indicating the hybridization mode of carbon atoms, used with the superscript 2 to represent sp. 2 Hybridization;
[0104] Vis is an abbreviation for ultraviolet-visible spectrum.
[0105] 1. Raman spectroscopy characterization:
[0106] The structural changes of graphene before and after modification were characterized by Raman spectroscopy. The D peak, G peak and 2D peak of the sample were obtained, and the peak intensity ratio of D peak to G peak, ID / IG, was calculated.
[0107] Among them, the D peak is mainly related to structural defects, edges, and sp in graphene. 2 The degree of disorder in the carbon skeleton is related to the G peak, which mainly reflects sp. 2 In-plane vibrations of hybrid carbon atoms. Therefore, ID / IG is used as an indicator to evaluate the degree of change in carbon framework defects during graphene modification.
[0108] Each sample was measured under the same laser wavelength, laser power, integration time, and testing method, and the average value of the test results from multiple locations was taken to reduce the impact of local differences in graphene powder.
[0109] By comparing the ID / IG values of pristine graphene, graphene treated only with pulsed plasma, graphene preloaded with 2-methyleneglutarate and then treated with continuous plasma, and the modified graphene of this invention, the effects of different modification methods on the sp of graphene were evaluated. 2 The influence of conjugated carbon structure.
[0110] The following formula is preferred to represent the change in defects before and after modification:
[0111] ;
[0112] In the formula, (ID / IG) modified The ratio of the D peak to the G peak intensity of the modified graphene is shown in (ID / IG). raw The ratio of the D peak to the G peak intensity of the original graphene.
[0113] Under conditions where similar wettability or liquid-phase dispersion properties are achieved, a smaller Δ(ID / IG) indicates a greater impact of the modification process on the graphene bulk sp. 2 The less damage caused by the conjugated structure.
[0114] 2. Resistivity test:
[0115] A standardized method was used to prepare raw graphene and various modified graphene samples into compressed tablets. Electrical performance tests were conducted under identical sample mass, compression pressure, holding time, sample diameter, sample thickness, and environmental conditions to minimize the impact of variations in sample packing states on the test results. The resistivity ρ of the samples was determined using the four-probe method or other suitable resistivity testing methods for graphene compressed tablets, with units expressed as Ω·cm.
[0116] The rate of change of resistivity can be further calculated using the following formula:
[0117] ;
[0118] In the formula, ρ modified To modify the resistivity of graphene, ρ raw The resistivity represents that of the original graphene. Under the condition of achieving similar hydrophilicity and dispersion stability, the smaller the increase in resistivity after modification, the better the modification method is for the graphene conductive network and sp2pF2. 2 The better the conjugate structure is preserved.
[0119] 3. Water contact angle test:
[0120] The surface wetting properties of graphene before and after modification were evaluated using a water contact angle test. Raw graphene and each modified graphene were prepared into flat, compressed tablets under identical conditions, with uniform control over sample quality, compression pressure, sample size, and surface treatment. A specified volume of deionized water droplets was dropped onto the sample surface, and the static contact angle between the droplets and the graphene tablet surface was recorded using a contact angle meter. Multiple locations were selected for testing on each sample, and the average value was taken as the water contact angle for that sample.
[0121] The degree of reduction in contact angle after graphene modification is expressed by the following formula:
[0122] ;
[0123] In the formula, θ raw θ represents the original water contact angle of graphene. modified The water contact angle of the modified graphene is Δθ. The larger the Δθ, the more significant the improvement in the water wettability of the modified graphene surface.
[0124] 4. Evaluation of liquid phase dispersion stability by ultraviolet-visible spectrophotometry:
[0125] The dispersion stability of graphene in the liquid phase was quantitatively evaluated using ultraviolet-visible spectrophotometry. Original graphene and each modified graphene were added to the same volume of liquid medium to prepare graphene dispersions with the same initial mass concentration, and treated with the same ultrasonic time, ultrasonic power, temperature, and other dispersion conditions. After dispersion, each sample was allowed to stand under the same environmental conditions, and ultraviolet-visible absorbance measurements were performed on dispersions taken from the same location at predetermined time points.
[0126] The absorbance At is measured at a predetermined characteristic wavelength or a test wavelength that can stably reflect the graphene dispersion concentration, and the dispersion retention rate is calculated according to the following formula, using the absorbance A0 immediately after dispersion as a reference:
[0127] ;
[0128] In the formula, St represents the dispersion retention rate after standing time t, At represents the absorbance after standing time t, and A0 represents the initial absorbance. A higher S_t indicates a lower degree of sedimentation of graphene in the liquid phase and better dispersion stability. The dispersion retention rate after 24 hours was used as the main comparison index between different samples.
[0129] Example and comparative test results:
[0130] 1. Effect of different amounts of 2-methyleneglutarate added:
[0131] Examples 1-4 correspond to the addition of 0.25%, 0.50%, 1.00%, and 2.00% of 2-methyleneglutarate, respectively, with all other treatment conditions remaining consistent. The test results are shown in Table 1.
[0132] Table 1. Modification effect of graphene with different amounts of 2-methyleneglutaric acid
[0133]
[0134] For Table 1, the water contact angle of the unmodified original graphene is 118°, and the dispersion retention rate after 24 hours is only 18%, which shows strong hydrophobicity and poor liquid phase dispersion stability.
[0135] As the amount of 2-methyleneglutarate added increased from 0.25% to 1.00%, the water contact angle of graphene gradually decreased, and the dispersion retention rate after 24 hours significantly improved. This indicates that the pre-loading of 2-methyleneglutarate combined with pulsed weak oxidation plasma can effectively improve the wettability of graphene surface and the dispersion stability of aqueous phase.
[0136] When the amount of 2-methyleneglutarate added was further increased from 1.00% to 2.00%, the water contact angle only decreased from 39° to 36%, and the 24-hour dispersion retention rate increased from 89% to 91%, indicating a relatively small improvement. Meanwhile, the ID / IG ratio increased from 0.34 to 0.41, and the resistivity increased from 3.7 × 10⁻⁶. -3 Ω·cm increased to 5.1×10 -3 Ω·cm.
[0137] This indicates that while adding excessive amounts of 2-methyleneglutarate can further improve the hydrophilicity of graphene, it may also increase the coverage of organic structures and the probability of free radical polymerization, thereby increasing the interfacial resistance between graphene sheets.
[0138] Taking into account the hydrophilicity, 24-hour dispersion stability, structural integrity and conductivity of graphene, the optimal addition amount of 2-methyleneglutaric acid is 0.25% to 1.00%, with about 0.50% showing better overall performance.
[0139] Synergistic effect of 2,2-methyleneglutarate and pulsed plasma:
[0140] Comparative Examples 1-4 were compared with Example 2 to evaluate the synergistic effect between 2-methyleneglutarate, weakly oxidizing pulsed plasma, and pulsed discharge mode.
[0141] The test results are shown in Table 2:
[0142] Table 2. Properties of graphene under different modification methods
[0143]
[0144] As shown in Table 2, in Comparative Example 2, which only underwent liquid phase treatment with 2-methyleneglutarate, the contact angle decreased from 118° to 92°, and the dispersion retention rate increased to 37% after 24 hours. This indicates that the physical adsorption of 2-methyleneglutarate can have a certain impact on the surface properties of graphene, but the degree of improvement is limited after thorough washing.
[0145] Comparative Example 3 was treated with only weak oxidizing pulsed plasma, with a contact angle of 71° and a dispersion retention rate of 58% after 24 hours. This indicates that pulsed plasma itself can improve the surface activity of graphene, but its degree of hydrophilic modification is still significantly lower than that of synergistic treatment with 2-methylene glutaric acid and pulsed plasma.
[0146] Comparative Example 4, after continuous plasma treatment, showed a decrease in contact angle to 38° and an increase in 24-hour dispersion retention to 88%, but also an increase in ID / IG to 0.46 and resistivity to 4.9 × 10⁻⁶. -3 Ω·cm.
[0147] Example 2, after pulsed plasma treatment, showed a contact angle of 47° and a dispersion retention rate of 85% after 24 hours, exhibiting similar hydrophilicity and dispersion stability to the continuous plasma sample; however, its ID / IG ratio was only 0.30 and its resistivity was only 3.2 × 10⁻⁶. -3 Ω·cm.
[0148] Compared to the original graphene, the ID / IG ratio of Example 2 increased by only 0.06, while that of the continuous plasma-treated sample increased by 0.22; the resistivity of Example 2 increased by approximately 14.3%, while that of the continuous plasma-treated sample increased by approximately 75.0%.
[0149] This demonstrates that using pulsed plasma can significantly reduce the structural defects and conductivity loss in graphene caused by continuous discharge, while achieving high hydrophilicity and dispersion stability.
[0150] 3. The influence of different plasma atmospheres:
[0151] The effects of different plasma atmospheres on the graphene modification were compared using Comparative Examples 5-8 and Example 2.
[0152] All samples were prepared using 0.50% 2-methyleneglutarate and a 30% pulse duty cycle.
[0153] The test results are shown in Table 3:
[0154] Table 3. Modification effects of the examples and comparative examples under different plasma atmospheres
[0155]
[0156] Under a pure Ar atmosphere, the water contact angle of the sample was 78° and the dispersion retention rate was 51% after 24 hours, indicating that it is difficult to obtain a high degree of hydrophilic modification by relying solely on the physical activation effect of Ar plasma.
[0157] After adding 3.0% CO2, the water contact angle decreased to 59°, and the dispersion retention rate increased to 70% after 24 hours; after adding 0.3% H2O, the water contact angle decreased to 63°, and the dispersion retention rate increased to 66% after 24 hours.
[0158] When CO2 and H2O are used simultaneously as oxygen-containing active components, the water contact angle in Example 2 decreases to 47°, the 24-hour dispersion retention rate increases to 85%, while ID / IG and resistivity remain at 0.30 and 3.2 × 10⁻⁶, respectively. -3 Ω·cm.
[0159] This indicates that when CO2 and H2O coexist, a significantly better surface modification effect than CO2 or H2O alone can be achieved under conditions of lower structural damage.
[0160] When 3.0% O2 was used as the oxygen-containing component, the water contact angle of Comparative Example 8 could be further reduced to 35%, and the 24-hour dispersion retention rate reached 89%, but its ID / IG ratio increased to 0.43, and its resistivity increased to 4.6 × 10⁻⁶. -3 Ω·cm.
[0161] This indicates that while stronger oxidizing plasma can achieve higher hydrophilicity, it also significantly increases the degree of structural defects in graphene and reduces its conductivity.
[0162] Therefore, the purpose of using the weakly oxidizing composite atmosphere of Ar / CO2 / H2O in this invention is not to obtain the lowest contact angle for graphene, but to achieve a better balance between hydrophilicity, liquid phase dispersion stability and carbon skeleton structure preservation.
[0163] 4. The effect of pulse duty cycle:
[0164] Examples 5, 6, 2, 7 and 8 use pulse duty cycles of 10%, 20%, 30%, 50% and 70% respectively, while keeping the other processing conditions the same.
[0165] The test results are shown in Table 4:
[0166] Table 4. Graphene modification effects of different pulse duty cycles in the examples
[0167]
[0168] As shown in Table 4, when the pulse duty cycle increases from 10% to 30%, the water contact angle of graphene decreases from 65° to 47°, and the 24-hour dispersion retention rate increases from 64% to 85%, while the increase in ID / IG and resistivity is relatively small. This indicates that appropriately increasing the pulse energy input can significantly promote the interfacial activation between graphene and 2-methyleneglutarate.
[0169] When the pulse duty cycle was further increased from 30% to 50% and 70%, the contact angle decreased to 42° and 39°, respectively, and the 24-hour dispersion retention rate only increased to 87% and 88%; meanwhile, the ID / IG ratio increased to 0.35 and 0.41, respectively, and the resistivity increased to 3.6 × 10⁻⁶. -3 Ω·cm and 4.2×10 -3 Ω·cm.
[0170] It can be seen that when the duty cycle is high, further increasing the plasma energy input gradually leads to saturation in improving hydrophilicity and dispersion stability, while the structural defects and resistivity of graphene continue to increase.
[0171] Taking all performance factors into account, the pulse duty cycle is preferably 10% to 50%, and more preferably 20% to 40%, with about 30% showing a better overall modification effect.
[0172] 5. Overall Evaluation:
[0173] The results in Tables 1 to 4 show that the present invention uses low-dose 2-methyleneglutarate liquid-phase preloading, and removes the unadsorbed free 2-methyleneglutarate after adsorption, followed by pulsed plasma treatment in a weak oxidizing atmosphere of Ar / CO2 / H2O, which can significantly improve the hydrophilicity and aqueous dispersion stability of graphene.
[0174] Among them, under the conditions of adding 0.50% of the graphene mass of 2-methyleneglutarate, plasma working atmosphere of Ar+3.0%CO2+0.3%H2O, and pulse duty cycle of 30%, the water contact angle of the modified graphene was reduced from 118° of the original graphene to 47°, and the 24h UV-vis dispersion retention rate was increased from 18% to 85%.
[0175] Meanwhile, RamanID / IG increased only from 0.24 to 0.30, and resistivity increased from 2.8 × 10⁻⁶. -3 Ω·cm increased to 3.2×10 -3 The resistivity increases by approximately 14.3% in Ω·cm.
[0176] Compared with continuous plasma treatment, the pulsed plasma treatment of the present invention can significantly reduce the increase in ID / IG and resistivity while achieving similar dispersion performance. Compared with a strong oxidizing atmosphere containing 3.0% O2, the weak oxidizing composite atmosphere of Ar / CO2 / H2O of the present invention, although resulting in a slightly higher contact angle, can significantly reduce defects in the graphene carbon skeleton and the loss of conductivity.
[0177] The above results indicate that this invention does not simply aim to maximize the hydrophilicity of graphene by increasing the degree of oxidation or forming a large amount of organic coating. Instead, it achieves this by leveraging the synergistic effect of low-coverage preloading with 2-methyleneglutarate, removal of free monomers, a weakly oxidizing composite atmosphere, and pulsed energy input. This improves the surface wettability and liquid-phase dispersion stability of graphene while simultaneously reducing the sp. 2 Damage to the conjugated carbon structure is mitigated, thereby achieving synergistic regulation between the graphene's dispersion properties and the maintenance of its conductive structure.
[0178] for Figure 4 and Figure 5 It can be observed that the graphene sample modified by pulsed plasma activation at the gas-solid interface of the present invention retains the two-dimensional sheet-like skeleton structure of the graphene sheets completely, without sheet breakage, large-area etched holes, or continuous polymer coating film.
[0179] At low magnification (15000×), graphene exhibits a typical sheet-like stacked morphology with clear edges and gaps between sheets, without severe sheet bridging or agglomeration; the surface has only a few scattered microparticles, and there is no large-area continuous organic coating layer. This confirms the effectiveness of the pre-treatment process for removing free monomers, successfully preventing the homopolymerization of monomers to form a thick polymer film encapsulating the graphene.
[0180] High-magnification (35000×) observation of the sheet surface reveals: the graphene substrate is smooth, without deep pits or numerous nanopores caused by strong plasma etching; the sheet surface exhibits fine, uniform textures, which are discrete grafting sites formed by the introduction of a small number of active sites and grafting of dicarboxyl monomers into the surface through weak pulsed plasma activation, rather than a continuously covered polymer film. This morphological characteristic indicates that the pulsed weak oxidation atmosphere of this invention only causes localized interfacial grafting reactions on the graphene surface and does not affect the graphene sp. 2 The carbon skeleton caused severe etching damage, but the main lamellar structure was preserved.
[0181] Compared to traditional liquid-phase grafted or continuous plasma modified samples: liquid-phase grafted samples are usually covered with a thick polymer film, with the layers agglomerated and adhered together by the polymer; graphene treated with continuous oxygen plasma shows a large number of etching pits on the surface, and the layers are severely damaged. In contrast, the modified sample of this invention has an intact layer structure, no continuous coating, and no heavy etching. Morphologically, this proves that the present invention has achieved surface functionalization grafting, while preserving the original two-dimensional layer structure and conductive framework of graphene to the greatest extent, which is consistent with the previous mechanism analysis.
[0182] To further verify the structural characteristics and surface chemical environment changes of the modified graphene of the present invention, Raman spectroscopy and Fourier transform infrared spectroscopy were performed on the original graphene and the modified graphene treated by the method of the present invention.
[0183] for Figure 6 Raman spectroscopy results showed that the sample in Example 1, before and after modification, exhibited similar performance at approximately 1350 cm⁻¹. -1 1580cm -1 and 2680cm -1 All samples exhibited D, G, and 2D peaks. Using the same Lorentz peak fitting method, the peak height ratios (ID / IG) of the D and G peaks in the original and modified samples were 0.927 and 0.963, respectively, with an increase of only 0.036 after modification (recorded as ΔID / IG = +0.04 in Table 1). Simultaneously, the G and 2D peaks remained clearly distinguishable, indicating that the modified material retained the sp² carbon structure characteristics of graphene. These results are consistent with the trend in Table 1 where ID / IG increased from 0.24 to 0.30 in Example 2.
[0184] for Figure 7 Infrared spectroscopy results showed that the modified sample was at approximately 3200–3600 cm⁻¹ -1 The broad absorption band within the range is more pronounced than that of the original sample. This absorption band is related to the stretching vibration of OH and may also include the contribution of adsorbed water; in addition, at approximately 1600 cm⁻¹... -1 Nearby and 1000-1300cm -1 The change in the absorption band shape of the region indicates that the chemical environment of the sample surface has changed before and after treatment. The above infrared test sample is modified graphene that has been thoroughly washed and dried with the ethanol / water mixture in step (5). After washing, it still retains obvious OH-related absorption bands. Compared with Comparative Example 2 (only physical adsorption, and the contact angle only dropped to 92° after washing), it shows that after activation by the gas-solid interface pulsed plasma of the present invention, an oxygen-containing / carboxyl-related polar structure that is still stably retained after washing is formed on the graphene surface.
[0185] The above Raman and infrared characterization results are consistent with the present invention's method of regulating graphene surface properties through mild gas-solid interface activation while preserving its sp. 2 The technical approach aligns with the characteristics of carbon structure.
[0186] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.
Claims
1. A method of graphene modification based on activation of gas-solid interface, characterized in that, Includes the following steps: (1) Graphene is added to a liquid medium for dispersion to depolymerize the aggregated graphene and obtain a graphene dispersion system. (2) Add 2-methyleneglutaric acid to the graphene dispersion system to allow 2-methyleneglutaric acid to fully contact with the graphene and adsorb onto the graphene surface, wherein the amount of 2-methyleneglutaric acid added is 0.05% to 5% of the graphene mass; (3) After adsorption is completed, the system obtained in step (2) is subjected to solid-liquid separation to remove at least part of the unadsorbed free 2-methyleneglutaric acid in the liquid phase, and then the residual liquid phase medium in the solid phase is removed to obtain graphene with 2-methyleneglutaric acid preloaded on the surface. (4) The graphene with 2-methylene glutaric acid preloaded on the surface obtained in step (3) is placed in a weak oxidizing atmosphere composed of argon, carbon dioxide and water vapor for pulsed plasma treatment, wherein argon is the working gas, carbon dioxide and water vapor are oxygen-containing active components, and the active particles generated by the pulsed plasma activate the gas-solid interface of the graphene surface and the preloaded 2-methylene glutaric acid, so that the unsaturated double bond of 2-methylene glutaric acid reacts with the active sites on the graphene surface, and the organic structure containing dicarboxyl groups is grafted and fixed on the graphene surface. (5) The product obtained in step (4) is washed to remove the unstable 2-methyleneglutarate and soluble oligomers, and then dried to obtain modified graphene.
2. The method of claim 1, wherein the graphene is modified based on activation of the gas-solid interface. The liquid medium in step (1) is at least one of water, ethanol, isopropanol; the dispersion is at least one of mechanical stirring, high shear dispersion with shear rate of 10000-45000 s -1 , ultrasonic dispersion.
3. The method of claim 1, wherein the graphene is modified based on activation of the gas-solid interface. In step (2), the amount of 2-methyleneglutarate added is 0.1% to 2% of the mass of graphene.
4. The method of claim 1, wherein the graphene is modified based on activation of the gas-solid interface. The 2-methylene glutaric acid in step (2) is pre-dissolved in a liquid medium to form a 2-methylene glutaric acid solution, and then the 2-methylene glutaric acid solution is continuously, batchwise or dropwise added to the graphene dispersion system, and the 2-methylene glutaric acid is adsorbed on the surface of graphene under stirring or ultrasonic conditions to form sp 3 Low coverage, non-continuous distribution of 2-methylene glutaric acid pre-loaded state with carbon content less than 5%.
5. The method of claim 1, wherein the graphene is modified based on activation of the gas-solid interface. In step (3), the solid-liquid separation is performed by at least one of filtration, vacuum filtration, centrifugation, and membrane separation to remove free 2-methylene glutaric acid that is not adsorbed on the graphene surface in the liquid phase before removing the liquid phase medium; the removal of the residual liquid phase medium in the solid phase is performed by at least one of vacuum drying, reduced pressure drying, freeze drying, low temperature airflow drying at 50-90℃, or spray drying.
6. The method of graphene modification based on gas-solid interface activation according to claim 1, wherein, In step (4), the weak oxidizing atmosphere is balanced by argon, with a volume fraction of carbon dioxide of 0.5% to 5%, a volume fraction of water vapor of 0.01% to 1%, and the remainder being argon.
7. The method of graphene modification based on gas-solid interface activation according to claim 1, wherein, The pulsed plasma in step (4) is one of dielectric barrier discharge plasma, pulsed glow discharge plasma, pulsed radio frequency plasma or pulsed microwave plasma; the pulsed plasma adopts an intermittent discharge mode of periodic on and off, with a duty cycle of 5% to 80% and a cumulative effective processing time of 0.1 to 60s.
8. The modified graphene prepared by the method of claim 1 to 7, wherein, The modified graphene has a surface with a dicarboxyl-containing organic graft structure formed by the interfacial activation reaction of the unsaturated double bonds of 2-methyleneglutarate. The dicarboxyl-containing organic graft structure is stably bonded to the graphene surface and remains on the graphene surface after washing with a liquid medium that can dissolve 2-methyleneglutarate.
9. The modified graphene of claim 8, wherein, The modified graphene retains the sp 2 conjugated carbon structure of the graphene main body while introducing a double-carboxyl group-containing organic grafting structure.