A coconut shell-based porous carbon material, its preparation method and application
By optimizing the mass ratio of carbonized coconut shell to potassium hydroxide and the activation conditions, high-performance porous carbon materials were prepared, solving the problem of insufficient process parameters in the existing technology, and realizing simplified operation and industrial application suitable for CVD silicon-carbon anodes.
Patent Information
- Application Number
- CN202611393099.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-09
- Publication Date
- 2026-11-17
AI Technical Summary
The existing technology for preparing porous carbon materials lacks optimization of process parameters, especially the lack of systematic research on the mass ratio of carbonized coconut shell to potassium hydroxide, activation temperature and time. This results in complex operation, high equipment requirements, and a narrow process parameter window, which limits the industrial application of porous carbon materials.
By optimizing the mass ratio of carbonized coconut shell to potassium hydroxide to 1:1.5 to 1:7, and combining drying and activation treatment at 850 to 950°C for 3 to 10 hours under inert gas protection, followed by acid washing and water washing, a coconut shell-based porous carbon material was prepared.
It achieves high specific surface area, rich pore structure and tunable pore parameters of porous carbon materials, which are suitable for CVD silicon-carbon anodes, simplify the preparation process and facilitate industrial production.
Smart Images

Figure CN123105631A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of porous carbon material preparation technology, specifically to a coconut shell-based porous carbon material, its preparation method, and its application. Background Technology
[0002] Porous carbon materials, due to their high specific surface area, good electrical conductivity, excellent chemical stability, and abundant pore structure, have broad application prospects in fields such as CVD silicon-carbon anodes. Biomass, as a renewable, widely available, and low-cost carbon source, has attracted widespread attention from researchers in recent years. Coconut shells, as a common agricultural and forestry waste, possess a natural fibrous structure and high carbon content, making them an ideal raw material for preparing high-performance porous carbon materials.
[0003] Currently, the activation methods for preparing porous carbon materials mainly include physical activation and chemical activation. Physical activation typically uses water vapor, carbon dioxide, or air at high temperatures to create pores in the carbon material; however, this method usually requires high temperatures and long activation times, and the resulting product has a limited specific surface area. Chemical activation uses chemical reagents such as potassium hydroxide, sodium hydroxide, phosphoric acid, and zinc chloride as activators. Among these, potassium hydroxide activation is considered an effective method for preparing porous carbon materials with high specific surface area.
[0004] However, existing technologies still lack optimization of process parameters such as the mass ratio of carbonized coconut shell to potassium hydroxide and activation temperature. In particular, there is a lack of systematic research on the pore structure characteristics of porous carbon materials obtained under different carbon-alkali ratios, activation temperatures, and times. Furthermore, existing preparation methods generally suffer from problems such as complex operation, high equipment requirements, and narrow process parameter windows, which limit their industrial application. Summary of the Invention
[0005] The purpose of this invention is to at least solve one of the technical problems existing in the prior art, and to provide a coconut shell-based porous carbon material, its preparation method and application.
[0006] The technical solution of the present invention is as follows: In a first aspect, the present invention provides a method for preparing a coconut shell-based porous carbon material, comprising the following steps: Carbonized coconut shell, potassium hydroxide, and water are mixed evenly to form a mud-like mixture that does not separate into layers when left to stand; wherein the mass ratio of carbonized coconut shell to potassium hydroxide is 1:1.5 to 1:7. The mud-like mixture is dried, and the dried material is fed into a tube furnace and activated at 850-950°C for 3-10 hours under inert gas protection. After activation, the sample is taken out and successively acid-washed and water-washed until neutral. After drying, coconut shell-based porous carbon material is obtained.
[0007] In a preferred embodiment of the present invention, the preparation method includes the following specific steps: (1) Add pure water to the container, place it in a constant temperature magnetic stirring water bath, adjust the speed, and set the heating temperature to 80-100℃; (2) Weigh out potassium hydroxide and add it to the container described in step (1) according to the mass ratio of carbonized coconut shell to potassium hydroxide of 1:1.5 to 1:7. Stir until completely dissolved, then add carbonized coconut shell and continue stirring until a mud-like mixture that does not separate into layers is formed. (3) Place the mud-like mixture obtained in step (2) in an electric heating blast drying oven at 50-80℃ to dry; (4) Transfer the dried material from step (3) to a metal crucible, cover it, place the crucible in a sample boat and send it into the middle section of the tube furnace. Under the protection of inert gas, heat it to 850-950℃ for activation treatment for 3-10 hours. (5) Take out the activated sample from step (4), and wash it with acid and water until it is neutral. After drying, the coconut shell-based porous carbon material is obtained.
[0008] In a preferred embodiment of the present invention, The mass ratio of carbonized coconut shell to potassium hydroxide is 1:3 to 1:7; Heat to 820-870℃ for activation treatment for 5-10 hours.
[0009] In a preferred embodiment of the present invention, the mass ratio of carbonized coconut shell to potassium hydroxide is 1:5 to 1:7; The temperature was raised to 850℃ for activation treatment for 5 hours.
[0010] In a preferred embodiment of the present invention, the container in step (1) is a plastic beaker, and the heating temperature is 95°C; The drying temperature in step (3) is 60°C.
[0011] In a preferred embodiment of the present invention, the metal crucible in step (4) is a nickel crucible; The furnace tubes of the tubular furnace mentioned in step (4) are metal furnace tubes.
[0012] In a preferred embodiment of the present invention, the temperature of the activation treatment in step (4) is increased to 850°C at a heating rate of 5°C / min, and the activation treatment time is 5h. The acid washing in step (5) uses a 0.96 mol / L hydrochloric acid solution.
[0013] Secondly, the present invention provides a coconut shell-based porous carbon material prepared by the aforementioned preparation method.
[0014] In a preferred embodiment of the present invention, the specific surface area of the coconut shell-based porous carbon material is 1207–2051 m² / g, the pore volume is 0.50–0.96 cm³ / g, the micropore ratio is 85–96%, and the average pore size is 1.63–1.90 nm.
[0015] Preferably, the specific surface area of the coconut shell-based porous carbon material is 1705–2051 m² / g, the pore volume is 0.75–0.96 cm³ / g, the micropore ratio is 90–94%, and the average pore size is 1.69–1.90 nm.
[0016] Thirdly, the present invention provides the application of the aforementioned coconut shell-based porous carbon material in CVD silicon-carbon anodes.
[0017] A CVD silicon-carbon anode includes the aforementioned coconut shell-based porous carbon material.
[0018] Fourthly, the present invention provides a battery comprising the aforementioned CVD silicon-carbon anode.
[0019] This invention has at least one of the following beneficial effects: (1) By optimizing the mass ratio of carbonized coconut shell to potassium hydroxide, activation temperature, and activation time, this invention can systematically control the pore structure parameters (specific surface area, pore volume, micropore ratio, and average pore size) of the obtained porous carbon material to meet the needs of different application scenarios. Furthermore, systematic research has found that when the mass ratio of carbonized coconut shell to potassium hydroxide is 1:6, the activation temperature is 850℃, and the activation time is 5h, the prepared coconut shell-based porous carbon material has a specific surface area of 2051 m² / g, a pore volume of 0.96 cm³ / g, a micropore ratio of 90%, and an average pore size of 1.87 nm, showing excellent microporous structure characteristics and surface properties.
[0020] (2) The preparation method of the present invention is simple to operate and the process is controllable. It adopts conventional heating, stirring, drying and tube furnace activation equipment, which is easy to scale up for industrial production.
[0021] (3) The coconut shell-based porous carbon material prepared by the present invention has a high specific surface area and rich pore structure, and is suitable as a porous carbon for CVD silicon-carbon anode. Attached Figure Description
[0022] Figure 1 The nitrogen adsorption-desorption isotherms of coconut shell-based porous carbon materials prepared by activation treatment at 850°C for different times when the mass ratio of carbonized coconut shell to potassium hydroxide was 1:6 in Examples 1-2 of this invention are shown.
[0023] Figure 2The nitrogen adsorption-desorption isotherm of the coconut shell-based porous carbon material prepared by activation treatment at 850°C for 5 hours when the mass ratio of carbonized coconut shell to potassium hydroxide was different in Example 3 of the present invention.
[0024] Figure 3 The nitrogen adsorption-desorption isotherms of coconut shell-based porous carbon materials prepared by activation treatment at different temperatures for 5 hours in Example 4 of the present invention when the mass ratio of carbonized coconut shell to potassium hydroxide is 1:3 are different. Detailed Implementation
[0025] To make the technical problems solved, the technical solutions, and the beneficial effects of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention.
[0026] An embodiment of the present invention provides a method for preparing a coconut shell-based porous carbon material, comprising the following steps: (1) Add pure water to the container, place it in a constant temperature magnetic stirring water bath, adjust the speed, and set the heating temperature to 80-100℃; (2) Weigh out potassium hydroxide and add it to the container described in step (1) according to the mass ratio of carbonized coconut shell to potassium hydroxide of 1:1.5 to 1:7. Stir until completely dissolved, then add carbonized coconut shell and continue stirring until a mud-like mixture that does not separate into layers is formed. (3) Place the mud-like mixture obtained in step (2) in an electric heating blast drying oven at 50-80℃ to dry; (4) Transfer the dried material from step (3) to a metal crucible, cover it, place the crucible in a sample boat and send it into the middle section of the tube furnace. Under the protection of inert gas, heat it to 850-950℃ for activation treatment for 3-10 hours. (5) Take out the activated sample from step (4), and wash it with acid and water until it is neutral. After drying, the coconut shell-based porous carbon material is obtained.
[0027] In some embodiments, in step (1), the container is a plastic beaker.
[0028] In some embodiments, the heating temperature in step (1) is 95°C.
[0029] In some embodiments, in step (2), the mass ratio of the carbonized coconut shell to potassium hydroxide is 1:3 to 1:7; preferably, the mass ratio of the carbonized coconut shell to potassium hydroxide is 1:5 to 1:7; more preferably, the mass ratio of the carbonized coconut shell to potassium hydroxide is 1:6.
[0030] In some embodiments, the drying temperature in step (3) is 60°C.
[0031] In some embodiments, in step (4), the metal crucible is a nickel crucible.
[0032] In some embodiments, in step (4), the furnace tube of the tubular furnace is a metal furnace tube.
[0033] In some embodiments, in step (4), the inert gas is argon.
[0034] In some embodiments, in step (4), the temperature of the activation treatment is increased to 850°C at a heating rate of 5°C / min.
[0035] In some embodiments, the activation treatment in step (4) lasts for 5 hours.
[0036] In some embodiments, in step (5), the pickling is performed using a 0.96 mol / L hydrochloric acid solution.
[0037] Main mechanism of action of this invention: (1) By using potassium hydroxide as an activator, potassium hydroxide reacts with carbon in carbonized coconut shell during high-temperature activation to produce products such as potassium carbonate, water and hydrogen. At the same time, the carbon skeleton is etched to form a rich microporous structure. The strong alkalinity and corrosiveness of potassium hydroxide can effectively etch disordered carbon and impurity components in carbonized coconut shell, increase porosity and improve specific surface area.
[0038] (2) Plastic beakers were used instead of glass beakers for alkaline solution preparation and mixing activation, which avoided the reaction of potassium hydroxide with silicon dioxide in glass to form potassium silicate, thus ensuring the effective concentration of activator and the consistency of the reaction system. At the same time, metal crucibles were used instead of ceramic crucibles for high-temperature activation, which avoided the reaction of potassium hydroxide with silicon dioxide and alumina in ceramics at high temperature, thus avoiding crucible corrosion and sample contamination, and improving the stability of the activation process and the purity of the product.
[0039] (3) After the carbonized coconut shell and potassium hydroxide solution are thoroughly stirred to form a mud-like mixture, it is dried so that the potassium hydroxide is evenly coated on the surface and internal pores of the carbonized coconut shell, ensuring the uniformity and fullness of the solid-solid reaction during the subsequent high-temperature activation process.
[0040] (4) After high-temperature activation, acid washing and water washing are performed to effectively remove potassium carbonate, potassium oxide and other soluble inorganic salt impurities generated during the activation process, resulting in a pure porous carbon framework structure. The obtained porous carbon material has a high specific surface area, high pore volume and adjustable micropore ratio and average pore size, providing abundant active sites and diffusion channels for ion transport and charge storage, which is beneficial to improving the specific capacitance and rate performance of sodium-ion battery electrode materials, and also provides excellent physicochemical support for gas adsorption and catalyst support.
[0041] The present invention will be further described in detail below with reference to specific embodiments, but the present invention is not limited to the following specific embodiments.
[0042] The preparation method of carbonized coconut shell in the following embodiments includes: First, the coconut shell raw material is pretreated by washing it with a large amount of water to remove surface impurities, then dried, and then crushed and sieved to a suitable particle size (200 mesh) by a crusher; Second, the pretreated coconut shell powder is placed in a tube furnace for carbonization treatment under an argon atmosphere, heated to 500°C at a heating rate of 10°C / min and held at that temperature for 2 hours; After carbonization, it is ground into a fine powder.
[0043] Example 1 This invention provides a method for preparing coconut shell-based porous carbon materials, comprising the following steps: (1) Take a 250mL plastic beaker, add 50mL of pure water, put in a rotor, place it in a constant temperature magnetic stirring water bath and fix it with a clamp, adjust the speed to 400r / min, and set the heating temperature to 95℃.
[0044] (2) Weigh 3g of potassium hydroxide into the beaker described in step (1) according to the mass ratio of carbonized coconut shell to potassium hydroxide of 1:6. Stir until completely dissolved, then slowly add 0.5g of carbonized coconut shell and continue stirring for about 12 hours until a mud-like mixture that does not separate into layers is formed.
[0045] (3) Place the mud-like mixture obtained in step (2) in a 60°C electric heating drying oven and dry for 12 hours.
[0046] (4) Use a spatula to scoop the dried material from step (3) into a mortar and grind it quickly. Then transfer it to a nickel crucible, cover it, place the crucible in a sample boat and send it into the middle section of the tube furnace. Under an argon protective atmosphere, heat the material to 850°C at a heating rate of 5°C / min for 5 hours.
[0047] (5) Take a 250mL beaker, prepare 100mL of dilute hydrochloric acid solution with a concentration of 0.96mol / L, place the beaker on a magnetic stirrer and add a rotor, start the magnetic stirrer and set the speed to 400r / min, take out the sample activated in step (4), add it to the beaker and acid wash for 4h, then filter it and wash it with pure water for 4h until neutral, finally filter it and put it in a 60℃ electric heating drying oven to dry it to obtain coconut shell based porous carbon material.
[0048] Nitrogen adsorption test: The coconut shell-based porous carbon material prepared in Example 1 was subjected to nitrogen adsorption test using a BSD-660 fully automated high-throughput high-performance specific surface area and pore size analyzer.
[0049] like Figure 1 As shown in Table 1, the results showed that the coconut shell-based porous carbon material prepared in Example 1 had a specific surface area of 2051 m² / g, a pore volume of 0.96 cm³ / g, a micropore ratio of 90%, and an average pore diameter of 1.87 nm, exhibiting excellent microporous structure characteristics and surface properties.
[0050] Example 2 This embodiment examines the effect of different activation treatment times, using the following method: The activation time in step (4) of Example 1 was adjusted from "5h" to "3h" and "10h" respectively. Other preparation steps, conditions and tests were the same as in Example 1. The test results are as follows. Figure 1 As shown in Table 1 below.
[0051] Table 1. Effects of different activation treatment times Table 1 shows that, under the conditions of a fixed carbon-alkali mass ratio of 1:6 and an activation temperature of 850℃, extending the activation time from 3 hours to 10 hours resulted in an increase in specific surface area from 1619 m² / g to 1993 m² / g, an increase of approximately 23%, and pore volume from 0.67 cm³ / g to 0.90 cm³ / g, an increase of approximately 34%. Meanwhile, the proportion of micropores only slightly decreased from 94% to 93%, and the average pore size slightly increased from 1.67 nm to 1.80 nm. This indicates that extending the activation time is beneficial for a more complete activation reaction and a more developed pore structure, while still maintaining a framework dominated by micropores. 10 hours is the optimal activation time. Furthermore, an activation time of 5 hours is the optimal activation time.
[0052] Example 3 This example examines the effect of different carbon-to-alkali mass ratios, using the following method: The mass ratio of carbonized coconut shell to potassium hydroxide in step (2) of Example 1 was adjusted to 1:1.5, 1:2, 1:4, 1:5 and 1:7 respectively. Other preparation steps, conditions and tests were the same as in Example 1. The test results are shown in Table 2 below.
[0053] Table 2. Effects of different carbon-alkali mass ratios As shown in Table 2, as the carbon-alkali mass ratio gradually increases from 1:1.5 to 1:7, the specific surface area shows an overall upward trend of first slowly increasing, then fluctuating slightly at 1:4, and then surging significantly. Specifically: when the carbon-alkali mass ratio increased from 1:1.5 to 1:2, the specific surface area slightly increased from 1241 m² / g to 1270 m² / g, the pore volume slightly increased from 0.50 cm³ / g to 0.51 cm³ / g, the micropore ratio remained at 95%~96%, and the average pore size was approximately 1.63~1.67 nm, indicating that the activation reaction was relatively mild within this ratio range, and the pore structure did not change significantly. When the carbon-alkali mass ratio increased to 1:4, the specific surface area slightly increased to 1301 m² / g, the pore volume was 0.60 cm³ / g, the micropore ratio decreased to 90%, and the average pore size increased to 1.84 nm, indicating that at this ratio, excess potassium hydroxide caused excessive etching of the pore walls, some micropores collapsed and merged, and the orderliness of the pore structure was damaged to some extent. When the carbon-alkali mass ratio was further increased to 1:5, the specific surface area jumped significantly to 1705 m² / g, and the pore volume increased significantly to 0.75. The micropore volume increased to 92%, thanks to the generation of potassium vapor from excess potassium hydroxide at high temperatures. This potassium vapor embedded in the carbon layers caused physical expansion, effectively opening new pores. When the carbon-to-alkali mass ratio further increased to 1:7, the specific surface area reached 1790 m² / g, the pore volume was 0.76 cm³ / g, the micropore volume increased to 94%, and the average pore size was 1.69 nm, indicating superior overall pore structure parameters. Furthermore, the overall pore structure parameters were optimal at a carbon-to-alkali mass ratio of 1:6.
[0054] Example 4 This embodiment examines the effect of different activation temperatures, using the following method: The mass ratio of carbonized coconut shell to potassium hydroxide in step (2) of Example 1 was adjusted to 1:3, and the activation treatment temperature in step (4) of Example 1 was adjusted to 800℃, 850℃ and 900℃ respectively. Other preparation steps, conditions and tests were the same as in Example 1. The test results are shown in Table 3 below.
[0055] Table 3. Effects of different activation temperatures As shown in Table 3, as the activation temperature increases from 800℃ to 850℃ and then to 900℃, the specific surface area shows a trend of first significantly increasing and then significantly decreasing. Specifically: at an activation temperature of 800℃, the specific surface area was 1207 m² / g, the pore volume was 0.52 cm³ / g, the micropore ratio was 88%, and the average pore size was 1.72 nm. This indicates that the activation reaction between potassium hydroxide and carbon at this temperature was insufficient, the carbon framework was not fully etched, and the pore structure development was limited. When the activation temperature was increased to 850℃, the specific surface area increased significantly to 1626 m² / g, the pore volume increased to 0.68 cm³ / g, the micropore ratio significantly increased to 95%, and the average pore size slightly narrowed to 1.68 nm. This indicates that the chemical etching reaction of potassium hydroxide at 850℃ was sufficient and uniform, producing a large number of ordered microporous structures, which is the ideal temperature for preparing microporous carbon materials with a high micropore ratio. When the temperature was further increased to 900℃, the specific surface area plummeted to 1280 m² / g, the pore volume decreased to 0.61 cm³ / g, the micropore ratio decreased to 85%, and the average pore size increased to 1.90 nm. The nm value indicates that the chemical etching reaction is excessively intensified at this temperature. Excess potassium hydroxide deeply erodes the existing microporous framework, causing the micropore walls to thin or even collapse. Adjacent micropores merge into mesopores, disrupting the ordered structure of the pores. Simultaneously, the carbon framework undergoes thermal shrinkage at this temperature, further exacerbating the decrease in specific surface area. Therefore, a carbonization temperature of 850℃ yields the optimal overall pore structure parameters.
[0056] In summary, the method for preparing coconut shell-based porous carbon materials provided by this invention has widely available and low-cost raw materials, and the preparation process is simple and easy to scale up for production. The resulting porous carbon materials have high specific surface area and controllable pore structure, and can be widely used in fields such as CVD silicon-carbon anodes, showing good industrial application prospects and economic benefits.
[0057] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.
Claims
1. A method for preparing a coconut shell-based porous carbon material, characterized in that, Includes the following steps: Carbonized coconut shell, potassium hydroxide, and water are mixed evenly to form a mud-like mixture that does not separate into layers when left to stand; wherein the mass ratio of carbonized coconut shell to potassium hydroxide is 1:1.5 to 1:
7. The mud-like mixture is dried, and the dried material is fed into a tube furnace and activated at 850-950°C for 3-10 hours under inert gas protection. After activation, the sample is taken out and successively acid-washed and water-washed until neutral. After drying, coconut shell-based porous carbon material is obtained.
2. The preparation method according to claim 1, characterized in that, The preparation method includes the following specific steps: (1) Add pure water to the container, place it in a constant temperature magnetic stirring water bath, adjust the speed, and set the heating temperature to 80-100℃; (2) Weigh out potassium hydroxide and add it to the container described in step (1) according to the mass ratio of carbonized coconut shell to potassium hydroxide of 1:1.5 to 1:
7. Stir until completely dissolved, then add carbonized coconut shell and continue stirring until a mud-like mixture that does not separate into layers is formed. (3) Place the mud-like mixture obtained in step (2) in an electric heating blast drying oven at 50-80℃ to dry; (4) Transfer the dried material from step (3) to a metal crucible, cover it, place the crucible in a sample boat and send it into the middle section of the tube furnace. Under the protection of inert gas, heat it to 850-950℃ for activation treatment for 3-10 hours. (5) Take out the activated sample from step (4), and wash it with acid and water until it is neutral. After drying, the coconut shell-based porous carbon material is obtained.
3. The preparation method according to claim 1 or 2, characterized in that, The mass ratio of carbonized coconut shell to potassium hydroxide is 1:3 to 1:7; Heat to 820-870℃ for activation treatment for 5-10 hours.
4. The preparation method according to claim 1 or 2, characterized in that, The mass ratio of carbonized coconut shell to potassium hydroxide is 1:5 to 1:7; The temperature was raised to 850℃ for activation treatment for 5 hours.
5. The preparation method according to claim 2, characterized in that, The container mentioned in step (1) is a plastic beaker, and the heating temperature is 95°C; The drying temperature in step (3) is 60°C.
6. The preparation method according to claim 2, characterized in that, The metal crucible mentioned in step (4) is a nickel crucible; The furnace tubes of the tubular furnace mentioned in step (4) are metal furnace tubes.
7. The preparation method according to claim 2, characterized in that, The temperature of the activation treatment in step (4) is increased to 850°C at a heating rate of 5°C / min, and the activation treatment time is 5h. The acid washing in step (5) uses a 0.96 mol / L hydrochloric acid solution.
8. The coconut shell-based porous carbon material prepared by the preparation method according to any one of claims 1 to 7.
9. The coconut shell-based porous carbon material according to claim 8, characterized in that, The specific surface area of the coconut shell-based porous carbon material is 1207–2051 m² / g, the pore volume is 0.50–0.96 cm³ / g, the micropore ratio is 85–96%, and the average pore size is 1.63–1.90 nm.
10. The application of the coconut shell-based porous carbon material according to any one of claims 8 to 9 in CVD silicon-carbon anodes.