A method for recovering silicon and silver from waste solar cells
By using heat treatment and salt leaching separation with ammonium or potassium hydrogen fluoride molten salt, the problems of low efficiency and high cost in silicon and silver recovery in existing technologies have been solved, achieving efficient and low-cost separation and recovery of silicon and silver.
Patent Information
- Application Number
- CN202611536657.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-30
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies for recovering silicon and silver from waste solar cells suffer from problems such as loss of valuable components due to mechanical processing, long chemical processing procedures, high costs, and poor selectivity, making it difficult to efficiently recover silicon and silver.
After removing organic matter through heat treatment, the silver wires and silicon wafers are selectively separated by salt leaching using ammonium or potassium hydrogen fluoride molten salt at a specific temperature, thus avoiding the loss of silicon through dissolution.
This method achieves efficient separation of silver wires from silicon wafers, shortens operation time, improves recycling efficiency, and reduces costs.
Smart Images

Figure CN123105648A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of waste solar cell resource recycling technology, specifically relating to a method for recovering silicon and silver from waste solar cells. Background Technology
[0002] With the rapid development of the global photovoltaic industry, the installed capacity of crystalline silicon solar cells is constantly increasing, and the amount of waste crystalline silicon solar cells is also increasing year by year. These waste crystalline silicon cells mainly come from: first, defective products generated during the production process due to substandard quality, i.e., waste crystalline silicon solar cells; second, a large number of old crystalline silicon solar cells generated from early-installed crystalline silicon modules due to low photoelectric conversion efficiency, severe degradation, partial damage, or reaching the end of their service life. If a large number of waste solar panels are not effectively disposed of, it will not only bring environmental pressure but also waste valuable components. Waste solar panels contain valuable components such as silicon and precious metals like silver. Silicon is a widely used material in photovoltaics and semiconductors, while silver is commonly used as a grid line material for solar cells. Therefore, recycling valuable components such as silicon and silver from waste solar panels has significant environmental and economic value.
[0003] Existing methods for recovering silver and silicon from spent solar cells typically include mechanical processing, thermal treatment, chemical etching, and combinations thereof. For example, Chinese Patent Publication No. CN118719761A discloses a method for obtaining silver-silicon enriched products through mechanical crushing, thermal treatment, and sorting; Chinese Patent Publication No. CN115647007A discloses a method for etching by sequentially immersing diced solar cells in different chemical solutions to obtain an aluminum-containing solution, a silver-containing solution, and a silicon wafer; Chinese Patent Publication No. CN117943379A discloses a method for treating solar cells with reusable organic solvents to achieve the recovery of related materials; and Chinese Patent Publication No. CN117339981A discloses a method for separating and recovering silver and silicon from solar cells using a mixed molten salt of sodium hydroxide and potassium hydroxide.
[0004] However, while mechanical crushing and sorting processes are simple, they easily lead to the loss of valuable components; conventional chemical treatment methods usually have problems such as long process times, high reagent consumption, or high costs; and molten salts with alkalis have poor selectivity, easily causing a large loss of silicon. Therefore, it is necessary to develop a high-efficiency method for recovering silicon and silver from waste solar cells with minimal silver-silicon loss and low cost. Summary of the Invention
[0005] The purpose of this invention is to provide a method for recovering silicon and silver from waste solar cells. The method involves removing the aluminum electrode through etching and using the high selectivity of ammonium bifluoride and potassium bifluoride or a mixture of the two molten salts to precisely remove the functional layer on the surface of the cell and the interface between the silver wire and the silicon wafer. This achieves the separation and recovery of the silicon wafer and the silver wire while avoiding the dissolution and loss of silver and silicon.
[0006] To achieve the above objectives, the present invention adopts the following technical solution: A method for recovering silicon and silver from spent solar cells includes the following steps: Step S1: Heat-treat the waste solar cells to obtain solar cell wafers; Step S2: Immerse the solar cell in an etching solution for etching and then dry it to obtain a dry aluminum-free solar cell; wherein the etching solution is at least one of sulfuric acid solution, hydrochloric acid solution, potassium hydroxide solution, and sodium hydroxide solution; Step S3: Roast at least one of ammonium bifluoride and potassium bifluoride in air to obtain molten salt; Step S4: Immerse the dried aluminum-free battery cell in the molten salt for salt leaching separation, remove it and place it in water for cooling and washing to separate the silicon wafer and silver wire.
[0007] Further, in step S1, the heat treatment process refers to: heating to 400℃-800℃ at a heating rate of 2℃ / min-20℃ / min and holding for a period of time (e.g., 30min-90min), thereby decomposing or deactivating organic materials such as the encapsulant film and backsheet through heat treatment, thereby separating the solar cell.
[0008] Further, in step S2, the heat-treated solar cell is immersed in an etching solution and etched until the aluminum electrode dissolves; wherein the etching temperature is 20℃-90℃, the etching solution concentration is 0.5mol / L-3mol / L, and the etching time is 1min-120min; the drying temperature after etching is 50℃-200℃, and the drying time is 1h-24h.
[0009] Furthermore, in step S3, the calcination temperature is 100℃-500℃.
[0010] Furthermore, in step S4, the salt leaching separation time is 2s-1200s, and the molten salt temperature is 100℃-500℃.
[0011] Further, in step S4, after salt leaching separation, the battery cell is placed in water for cooling and washing until the silicon wafer and silver wire separate and the attached salt dissolves, to obtain the product of high-purity silicon wafer and silver wire.
[0012] Furthermore, the method described in this invention can be used to process different types of crystalline silicon solar cells, including Al-BSF, PERC, and TOPCon type cells.
[0013] The beneficial effects of this invention are: This invention uses waste solar cells as raw materials. First, organic materials such as EVA film and backsheet are decomposed or rendered ineffective through heat treatment to obtain solar cell wafers. Then, aluminum electrodes are removed through etching. Subsequently, high-purity silicon wafers and silver wires are obtained through salt leaching using ammonium bifluoride and / or potassium bifluoride molten salt. This molten salt system selectively acts on the functional layers on the surface of the solar cell and the interface between the silver wires and the silicon wafer, achieving separation of the silver wires from the silicon wafer in a short time, while simultaneously removing functional layers such as silicon nitride, alumina, and silicon oxide. This method has a short process and is relatively simple to operate, which is beneficial for improving the separation and recovery efficiency of silicon and silver. Attached Figure Description
[0014] Figure 1 The flowchart illustrates a method for recovering silicon and silver from waste crystalline silicon solar cells, as provided in this embodiment of the invention.
[0015] Figure 2 This is a reaction mechanism diagram according to an embodiment of the present invention; wherein, Figure 2 a is a schematic diagram of the mechanism for recovering Al-BSF type solar cells using the NH4HF2 system in Example 1. Figure 2 b is a schematic diagram illustrating the mechanism of PERC-I type solar cell recovery using the NH4HF2 system in Example 2. Figure 2 c is a schematic diagram illustrating the mechanism of PERC-II type solar cell recovery in the KHF2 system in Example 3. Figure 2 d is a schematic diagram of the mechanism for recovering TOPCon type solar cells in the KHF2 system in Example 4.
[0016] Figure 3 This is a diagram of the recovered products provided in an embodiment of the present invention; wherein, Figure 3 a is a diagram of the silicon wafer product from Example 1. Figure 3 b is a diagram of the silver wire product from Example 1. Figure 3 c is a diagram of the silicon wafer product from Example 2. Figure 3 d is a diagram of the silver wire product from Example 2. Figure 3 e is a diagram of the silicon wafer product in Example 3. Figure 3 f is a diagram of the silver wire product from Example 3. Figure 3 g is a diagram of the silicon wafer product from Example 4. Figure 3 h is a diagram of the silver wire product in Example 4. Detailed Implementation
[0017] The present invention will be described below with reference to specific embodiments and examples. Those skilled in the art should understand that the following specific embodiments and examples are for illustrative purposes only and should not be construed as limiting the scope of protection of the present invention.
[0018] In this invention, unless otherwise stated, all raw materials used are commercially available products conventional in the art.
[0019] This invention provides a method for recycling silicon and silver from waste solar panels, such as... Figure 1 As shown, the method includes the following steps: Step S1: Heat-treat the waste solar cells to obtain solar cell wafers. During the heat treatment, the heating rate is 2℃ / min-20℃ / min, and the heat treatment temperature is 400℃-800℃.
[0020] Step S2: Immerse the solar cell in an etching solution for etching until the aluminum electrode dissolves, and then dry it to obtain a dry, aluminum-free solar cell. The etching solution can be at least one of sulfuric acid solution, hydrochloric acid solution, potassium hydroxide solution, and sodium hydroxide solution.
[0021] Step S3: Immerse the dried aluminum-free solar cell in a molten salt formed by ammonium hydrogen fluoride, potassium hydrogen fluoride, or a mixture of both for salt leaching separation. The temperature of the molten salt is 100℃-500℃, and the salt leaching separation time is 2s-1200s. Salt leaching separation can disrupt the interface between the silver wire and the silicon wafer, achieving separation of the silver wire and silicon wafer with minimal reaction, while simultaneously removing functional layers such as silicon nitride.
[0022] Step S4: Remove the battery cells after salt immersion separation and place them in water to cool and wash them until the silicon wafer separates from the silver wire and the attached salt dissolves, thus obtaining the silicon wafer and silver wire.
[0023] The molten salt system used in this invention includes NH4HF2 and / or KHF2. This system can remove silicon nitride and some silicon, and also AlO2. x SiO x Functional layers, etc. Based on the above-mentioned effects, this invention can quickly remove the functional layers and recover silver wires and silicon wafers, which helps to shorten operation time and improve recycling efficiency. Furthermore, the method of this invention is applicable to Al-BSF, PERC, TOPCon and other types of crystalline silicon solar cells, and the reaction mechanism is as follows: Figure 2 As shown.
[0024] The method of this application will be further described below with reference to the embodiments and experimental data.
[0025] Example 1 A method for recycling silicon and silver from waste solar panels, comprising the following steps: Waste Al-BSF solar panels were placed in a high-temperature furnace and heated to 480°C at a rate of 2°C / min, held at that temperature for 60 min, and the complete Al-BSF solar cells were separated. The Al-BSF solar cells were then immersed in a 1 mol / L hydrochloric acid solution at 25°C for 30 min to obtain aluminum-free solar cells. These aluminum-free solar cells were then immersed in molten ammonium bifluoride and salt-leached at 200°C for 20 s. Finally, the solar cells were removed and placed in cold water to separate the silicon wafers and silver wires. Figure 3 a- Figure 3 b).
[0026] Example 2 A method for recycling silicon and silver from waste solar panels, comprising the following steps: Waste PERC-I solar panels were placed in a high-temperature furnace and heated to 650°C at a rate of 10°C / min, held at that temperature for 30 min, and the complete PERC-I solar cell was obtained. The PERC-I solar cell was then immersed in a 0.5 mol / L sulfuric acid solution at 40°C for 30 min to obtain aluminum-free solar cells. The aluminum-free solar cells were then immersed in molten ammonium bifluoride and salt-leached at 150°C for 600 s. Subsequently, the solar cells were removed and placed in cold water to separate the silicon wafer and silver wire. Figure 3 c- Figure 3 d).
[0027] Example 3 A method for recycling silicon and silver from waste solar panels, comprising the following steps: Waste PERC-II solar panels were placed in a high-temperature furnace and heated to 550°C at a rate of 20°C / min, held at that temperature for 90 min, and the complete PERC-II solar cells were separated. The PERC-II solar cells were then immersed in a 2.5 mol / L sodium hydroxide solution at 80°C for 30 min to obtain aluminum-free solar cells. These aluminum-free solar cells were then immersed in molten potassium hydrogen fluoride and salt-leached at 350°C for 2 s. Finally, the solar cells were removed and placed in cold water to separate the silicon wafers and silver wires. Figure 3 e- Figure 3 f).
[0028] Example 4 A method for recycling silicon and silver from waste solar panels, comprising the following steps: Waste TOPCon solar panels were placed in a high-temperature furnace and heated to 500°C at a rate of 15°C / min, held at that temperature for 45 min, and the complete TOPCon solar cells were separated. The TOPCon solar cells were then immersed in a 2 mol / L potassium hydroxide solution at 50°C for 30 min to obtain aluminum-free solar cells. These aluminum-free solar cells were then immersed in molten potassium fluoride and salt-leached at 300°C for 10 s. Finally, the solar cells were removed and placed in cold water to separate the silicon wafers and silver wires. Figure 3 g- Figure 3 h).
[0029] Comparative Example 1 In this comparative example, the molten salt temperature is 50°C, and the other steps are the same as in Example 1.
[0030] Comparative Example 2 In this comparative example, the molten salt temperature is 600°C, and the other steps are the same as in Example 1.
[0031] Comparative Example 3 In this comparative example, the molten salt used was a mixed molten salt of NaOH and KOH (mass ratio of NaOH:KOH=0.42:0.58), and the other steps were the same as in Example 1.
[0032] Comparative Example 4 In this comparative example, the molten salt used was a mixed molten salt of NaOH and KOH (mass ratio of NaOH:KOH=0.42:0.58), the molten salt temperature was 300℃, and the other steps were the same as in Example 1.
[0033] Performance testing: The statistics of each embodiment and each comparative example are shown in Table 1; Table 1 Test results of Examples 1-4 and Comparative Examples 1-4
[0034] As shown in Table 1, in Comparative Example 1, the molten salt temperature was 50℃, which is lower than the molten salt temperature range specified in this invention, resulting in problems such as incomplete melting of the molten salt and insufficient reactivity. In Comparative Example 2, the molten salt temperature was 600℃, which is higher than the molten salt temperature range specified in this invention, resulting in problems such as excessive reactivity, intensified silicon wafer erosion, and intensified volatilization of ammonium bifluoride. In Comparative Examples 3 and 4, the mixed molten salt of NaOH and KOH showed poor selectivity for the functional layer on the surface of the battery cell, as well as the silver-silicon interface and the silicon substrate, resulting in problems such as incomplete silver wire stripping or significant silicon wafer loss. In Examples 1 to 4, the method of this invention can obtain silicon and silver with high purity and has the advantages of wide availability of raw materials, short process flow, relatively simple operation, and short processing time.
[0035] Finally, it should be noted that the terms “comprising,” “including,” or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements may include not only the listed elements but also other elements not expressly listed, or elements inherent to the process, method, article, or apparatus.
[0036] Although preferred embodiments of the invention have been described, those skilled in the art, upon learning the basic concept of the invention, can make changes and modifications to these embodiments.
[0037] Obviously, those skilled in the art can make various modifications and variations to this invention without departing from its spirit and scope. If such modifications and variations fall within the scope of equivalents of this invention, then this invention also intends to include such modifications and variations.
Claims
1. A method for recovering silicon and silver from waste solar cells, characterized in that, Includes the following steps: Step S1: Heat-treat the waste solar cells to obtain solar cell wafers; Step S2: Immerse the solar cell in an etching solution for etching and then dry it to obtain a dry aluminum-free solar cell; wherein the etching solution is at least one of sulfuric acid solution, hydrochloric acid solution, potassium hydroxide solution, and sodium hydroxide solution; Step S3: Roast at least one of ammonium bifluoride and potassium bifluoride in air to obtain molten salt; Step S4: Immerse the dried aluminum-free battery cell in the molten salt for salt leaching separation, remove it and place it in water for cooling and washing to separate the silicon wafer and silver wire.
2. The method for recovering silicon and silver from waste solar cells according to claim 1, characterized in that, In step S1, the heat treatment process refers to: heating to 400℃-800℃ at a heating rate of 2℃ / min-20℃ / min and holding for a period of time, so as to decompose or deactivate organic materials such as the encapsulant film and backsheet through heat treatment, thereby separating the solar cell.
3. The method for recovering silicon and silver from waste solar cells according to claim 1, characterized in that, In step S2, the heat-treated solar cell is immersed in an etching solution and etched until the aluminum electrode dissolves. The etching temperature is 20℃-90℃, the etching solution concentration is 0.5mol / L-3mol / L, and the etching time is 1min-120min. The drying temperature after etching is 50℃-200℃, and the drying time is 1h-24h.
4. The method for recovering silicon and silver from waste solar cells according to claim 1, characterized in that, In step S3, the calcination temperature is 100℃-500℃.
5. The method for recovering silicon and silver from waste solar cells according to claim 1, characterized in that, In step S4, the salt leaching separation time is 2s-1200s, and the molten salt temperature is 100℃-500℃.
6. The method for recovering silicon and silver from waste solar cells according to claim 1, characterized in that, In step S4, after salt leaching separation, the battery cells are placed in water for cooling and washing until the silicon wafer and silver wire separate and the attached salt dissolves to obtain the product of high-purity silicon wafer and silver wire.
7. The method for recovering silicon and silver from waste solar cells according to claim 1, characterized in that, The method is used to process different types of crystalline silicon solar cells, including Al-BSF, PERC and TOPCon type cells.
Citation Information
Patent Citations
Comprehensive recovery method of waste photovoltaic module
CN115647007A
Method for recycling silicon and silver in waste solar panel
CN117339981A
Process and method for separating different components from waste photovoltaic module
CN117943379A
Method for comprehensively recovering all components of waste photovoltaic module
CN118719761A