A method for preparing quartz sand
By using hydrolysis, washing, soaking, supercritical carbon dioxide extraction, and sintering treatments in the preparation process of quartz sand, the problems of carbon content and black spots in quartz sand were solved, high-purity quartz sand was prepared, and the bubble density of quartz crucibles was reduced.
Patent Information
- Application Number
- CN202611120395.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-27
- Publication Date
- 2026-11-17
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of quartz material technology, and particularly relates to a method for preparing quartz sand. Background Technology
[0002] High-purity quartz sand is a core material in the semiconductor, photovoltaic, and optical materials manufacturing industries, and its performance directly affects the quality and reliability of downstream products. In the semiconductor industry, high-purity quartz sand is mainly used to manufacture quartz crucibles, quartz tubes and rods, and semiconductor optical components. As integrated circuit technology develops towards 12-inch and larger wafers and N-type silicon wafers, the performance requirements for quartz crucibles in the single-crystal silicon pulling process are becoming increasingly stringent. Quartz crucibles must possess ultra-high purity (SiO2 purity ≥ 99.998%), the bubble density in the transparent layer of the quartz crucible must be extremely low, and carbonaceous black spots are not allowed; otherwise, defects such as edge breakage and cracks will occur during the single-crystal silicon pulling process, severely reducing production yield.
[0003] However, natural quartz ore generally suffers from the problem of difficulty in deeply removing fluid inclusions and lattice impurities, making it difficult to meet the purity requirements of high-end manufacturing. Therefore, there is an urgent need to develop a method for preparing quartz sand to reduce its carbon content, the number of black spots, and improve its purity, thereby reducing the bubble density in the quartz crucible. Summary of the Invention
[0004] The main objective of this invention is to provide a method for preparing quartz sand, which can reduce the carbon content and number of black spots in the quartz sand and improve its purity, thereby reducing the bubble density of the quartz crucible.
[0005] This invention provides a method for preparing quartz sand, comprising the following steps:
[0006] 1) The raw material system, including silicate ester, alcohol solvent, ultrapure water and catalyst, was subjected to hydrolysis and aging treatment in sequence to obtain the first gel;
[0007] 2) The first gel was washed with ultrapure water to obtain the second gel;
[0008] 3) The second gel is soaked in an alcohol solvent to obtain a third gel;
[0009] 4) The third gel is subjected to supercritical carbon dioxide extraction to obtain the fourth gel;
[0010] 5) The fourth gel is sintered to obtain the quartz sand.
[0011] In the preparation method described above, the silicate ester includes at least one of methyl silicate, ethyl silicate, and propyl silicate;
[0012] And / or, the alcohol solvent includes at least one of methanol, ethanol, and propanol;
[0013] And / or, the molar ratio of the silicate ester, the alcohol solvent, and the ultrapure water is 1:(3~4):(2~6).
[0014] In the preparation method described above, the hydrolysis temperature is 20~60℃;
[0015] And / or, the hydrolysis treatment time is 2-4 hours;
[0016] And / or, the aging treatment temperature is 40~60℃;
[0017] And / or, the aging process takes 12 to 24 hours.
[0018] In the preparation method described above, the pH of the raw material system is 1.5~2.5 or 9.0~10.0.
[0019] In the preparation method described above, the catalyst includes an acidic catalyst and / or a basic catalyst;
[0020] Preferably, the acidic catalyst includes at least one of hydrochloric acid, nitric acid, and acetic acid;
[0021] Preferably, the alkaline catalyst includes at least one of ammonia and tetramethylammonium hydroxide.
[0022] In the preparation method described above, the soaking treatment is performed 3 to 5 times;
[0023] And / or, the soaking time for each soaking treatment is 1 to 2 hours.
[0024] In the preparation method described above, the temperature of the supercritical carbon dioxide extraction treatment is 40~60℃, preferably 45~55℃;
[0025] And / or, the pressure of the supercritical carbon dioxide extraction treatment is 10~20MPa, preferably 12~18MPa;
[0026] And / or, the supercritical carbon dioxide extraction treatment time is 3~8h.
[0027] The preparation method described above, wherein the sintering treatment includes a first sintering treatment and a second sintering treatment performed sequentially;
[0028] Preferably, the temperature of the first sintering treatment is 600~850℃, more preferably 700~800℃;
[0029] And / or, the time for the first sintering treatment is 2 to 6 hours, preferably 3 to 5 hours;
[0030] And / or, the temperature of the second sintering treatment is 1150~1250℃;
[0031] And / or, the second sintering treatment time is 4~8 hours.
[0032] In the preparation method described above, the depressurization rate after supercritical carbon dioxide extraction is 0.5~2.0 MPa / h, preferably 0.5~1.5 MPa / h.
[0033] The preparation method described above further includes, after the supercritical carbon dioxide extraction treatment, the fourth gel is subjected to a crushing treatment.
[0034] Preferably, the Dv50 of the gel after the crushing treatment is 100~150μm and the Dv90 is ≤200μm.
[0035] The method for preparing quartz sand provided by this invention involves sequentially hydrolyzing and aging a raw material system comprising silicate ester, alcohol solvent, ultrapure water, and catalyst to form a first gel, followed by sequential washing with ultrapure water, soaking in alcohol solvent, supercritical carbon dioxide extraction, and sintering. This method effectively removes residual components inside the gel and reduces the risk of pore structure shrinkage or collapse during the quartz sand preparation process, thereby reducing residual carbon and black spot defects, improving the purity of the quartz sand, and consequently reducing the bubble density of the quartz crucible. Detailed Implementation
[0036] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions in the embodiments of this invention will be clearly and completely described below in conjunction with the embodiments of this invention. Obviously, the described embodiments are only some embodiments of this invention, not all embodiments. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.
[0037] High-purity silica materials are typically prepared using methods such as gas-phase hydrolysis, water glass precipitation, or sol-gel methods. Among these, the sol-gel method, which involves the hydrolysis and condensation of silicates in an alcohol and water system to form a gel, followed by washing, drying, and heat treatment to convert it into silica sand, offers advantages such as high raw material purity and controllable composition, making it more suitable for the preparation of high-end silica sand.
[0038] However, in this type of technical route, the pore structure is prone to shrinkage or even collapse during the gel drying stage, and the originally connected internal channels are partially blocked, making it difficult for residual alcohols and other organic components inside the particles to migrate and be discharged smoothly. During the subsequent sintering process, these organic residues are difficult to remove completely, easily forming defects such as residual carbon and black spots, affecting the purity of the quartz sand and causing an increase in the bubble density of the quartz crucible.
[0039] The inventors of this application have discovered that by sequentially hydrolyzing and aging a raw material system containing silicate esters, alcohol solvents, ultrapure water, and catalysts, followed by sequential washing, alcohol solvent soaking, supercritical carbon dioxide extraction, and sintering, the removal of organic components inside the gel can be effectively improved, thereby increasing the purity of the obtained quartz sand.
[0040] Based on this, the present invention provides a method for preparing quartz sand, comprising the following steps:
[0041] 1) The raw material system, including silicate ester, alcohol solvent, ultrapure water and catalyst, was subjected to hydrolysis and aging treatment in sequence to obtain the first gel;
[0042] 2) The first gel was washed with ultrapure water to obtain the second gel;
[0043] 3) The second gel was soaked in an alcohol solvent to obtain the third gel;
[0044] 4) The third gel was subjected to supercritical carbon dioxide extraction to obtain the fourth gel;
[0045] 5) The fourth gel is sintered to obtain quartz sand.
[0046] In this invention, the silicate ester in the raw material system of step 1) can serve as a silicon source, the alcohol solvent is used to construct the reaction medium, ultrapure water (resistivity ≥18.2 MΩ·cm) is used to provide the water required for controlled hydrolysis, and the catalyst is used to regulate the hydrolysis and polycondensation processes. In the hydrolysis stage, the silicate ester is typically mixed with the alcohol solvent and ultrapure water first, and then the catalyst is added under stirring conditions. This allows the silicate ester molecules to hydrolyze in a controlled environment to generate silanol groups, which are then gradually constructed through polycondensation to form a silicon-oxygen bond network and an initial gel framework. By controlling the feeding sequence, system uniformity, and catalytic environment during the hydrolysis stage, the hydrolysis and polycondensation rates can be coordinated, avoiding excessively rapid local gelation that could lead to uneven pore structures or particle agglomeration, thus laying the foundation for subsequent impurity removal and pore opening. Among these, raw material purity control is the decisive factor in the final product's metal impurity content. All liquid raw materials must meet electronic-grade purity requirements, and the total content of metal impurities (Fe, Al, Ca, Na, etc.) in the silicate ester must be less than 1 ppm.
[0047] After hydrolysis, the gel undergoes an aging process. It is kept at a set temperature and either allowed to stand or stirred at low speed for a period of time, allowing unreacted silanol groups within the gel to continue condensing, promoting network rearrangement and skeletal reinforcement. During aging, the gel pore walls gradually thicken, and the pore connectivity stabilizes, thus reducing the risk of collapse due to a fragile skeletal structure during subsequent washing, soaking, and extraction. This treatment ensures the gel maintains a certain degree of mechanical integrity before entering subsequent purification steps and provides stable pathways for internal solvent migration.
[0048] Step 2) After the first gel forms, it is washed with ultrapure water. The resistivity and low impurity characteristics of ultrapure water allow it to displace residual catalyst, by-product alcohol, and low-molecular-weight impurities in the gel pores without introducing new metal ions, anions, or particulate contamination. During washing, soluble impurities in the outer layer and connecting channels gradually diffuse into the washing solution and are carried out, thus obtaining the second gel. The number of washes, liquid-to-solid ratio, and washing time per wash can be determined based on the concentration of residual impurities to ensure that the pH and ion residues are reduced to a level suitable for subsequent solvent replacement. Because ultrapure water has good compatibility with the aqueous phase components remaining in the pores of the gel, this step can preferentially remove inorganic ions and polar impurities and reduce volatile contaminants in subsequent heat treatment.
[0049] In one embodiment, the first gel obtained in step 1) is subjected to multi-stage countercurrent washing with ultrapure water under room temperature (20~25°C), normal pressure or pressurized filtration (0.2~0.3MPa) conditions, with no less than 5 washing stages and a total washing time of 6~10h.
[0050] The conductivity and Cl- of the washing solution need to be monitored throughout the washing process. - The concentration was adjusted until the conductivity of the final washing solution dropped below 2 μS / cm. After confirming that alcohol byproducts, catalysts, and metal impurity ions were fully removed, the solution was filtered and separated to obtain a second gel filled with water in its pores.
[0051] Step 3) The second gel is then soaked in an alcohol solvent to obtain the third gel. This soaking treatment further facilitates solvent replacement within the gel pores, gradually replacing the residual aqueous phase with the alcohol solvent and creating a suitable solvent environment for supercritical carbon dioxide extraction. Since supercritical carbon dioxide has limited solubility and extraction capabilities for water but higher compatibility with some organic solvents and alcohols, first soaking the gel in alcohol to convert the internal medium into a state easily carried by carbon dioxide significantly improves subsequent extraction efficiency. During this process, the alcohol solvent also mitigates changes in gel capillary pressure, reducing the possibility of localized shrinkage of the pore structure during solvent switching.
[0052] In one embodiment, the second gel obtained in step 2) is immersed in a sufficient amount of alcohol solvent (electronic grade, purity ≥99.9%) and left to soak at room temperature (20~25°C). The alcohol solvent gradually penetrates into the pores of the second gel and displaces the water. The water content of the final displacement solution is detected online using a Karl Fischer moisture analyzer until it is below 500 ppm, confirming that the solvent in the pores has been replaced by alcohol solvent from water, thus obtaining the third gel. Since the solubility of supercritical CO2 in alcohol solvents is approximately 10~20 mol% (50°C, 15 MPa), and alcohol solvents, such as ethanol, are completely miscible with water, repeated soaking and displacement can reduce the water content in the pores to an acceptable level, providing a well-compatible liquid medium for subsequent supercritical CO2 extraction and drying.
[0053] Step 4) After the third gel undergoes supercritical carbon dioxide (carbon dioxide in a supercritical fluid state at temperatures above 31.1℃ and pressures above 7.38MPa) extraction, the carbon dioxide is brought into full contact with the alcohol solvent inside the gel under supercritical conditions. Supercritical carbon dioxide possesses both high diffusivity of gases and high solubility of liquids, allowing it to penetrate the gel pores and dissolve and carry away residual alcohols and some low-boiling-point organic matter from the pores. These are then carried out of the system under reduced pressure or circulating flow conditions to obtain the fourth gel. The key to this step is utilizing the near-zero surface tension and high diffusion coefficient of supercritical fluids to avoid pore blockage and framework collapse caused by capillary forces during conventional evaporation and drying. This allows most of the organic residues inside the gel to be removed under low mechanical disturbance conditions, significantly reducing the sources of outgassing and residual carbon during subsequent sintering.
[0054] In one embodiment, the third gel obtained in step 3) is loaded into a supercritical extraction device (pressure-resistant container, design pressure ≥30MPa), sealed, and then food-grade or industrial-grade CO2 (purity ≥99.9%) is introduced. The pressure is slowly increased while the temperature is increased, so that the CO2 enters the supercritical state (critical parameters: Tc=31.1℃, Pc=7.38MPa).
[0055] Under supercritical conditions, supercritical CO2 is continuously introduced at a constant flow rate to extract alcohol solvents from the pores of the third exchange gel. During the exchange process, the supercritical CO2 fluid containing alcohol solvents is discharged from the extraction vessel outlet, depressurized by a back pressure valve, and then enters a gas-liquid separator: the alcohol solvents are collected at the bottom of the separator, and the CO2 gas phase is pressurized and liquefied by a compressor and then recycled back to the extraction vessel, realizing closed-loop CO2 recycling. The recovered alcohol solvents, after passing a test, are returned to step 1) for use. The alcohol solvent content in the discharged gas can be detected online at the extraction vessel outlet. When the alcohol solvent concentration is below 1 g / m³... 3 The replacement is determined to be complete at that time.
[0056] After the replacement is completed, the pressure is slowly reduced to normal pressure at a certain rate to complete the drying process, resulting in SiO2 dry gel (aerogel framework) with a fully open-pore mesoporous structure.
[0057] The technical principle of this scheme is as follows: the gas-liquid interface of supercritical CO2 disappears, and the surface tension is almost zero (γ=0). According to the Laplace equation (ΔP=2γcosθ / r), the capillary pressure is zero during the depressurization process, the gel channels are not destroyed by capillary force, and the SiO2 framework can maintain a three-dimensional interconnected fully open-pore mesoporous structure.
[0058] Step 5) The fourth gel undergoes supercritical carbon dioxide extraction followed by sintering. During sintering, the residual organic matter in the gel framework is further decomposed and released by heating, while simultaneously promoting the densification of the silica network and the crystal phase transformation, ultimately yielding quartz sand. Through the synergistic effect of the aforementioned washing, solvent replacement, and supercritical carbon dioxide extraction, the content of volatile organic compounds in the fourth gel entering the sintering stage is significantly reduced. Therefore, gas release during sintering is more stable, and the resulting quartz sand meets the application requirements of high-end quartz raw materials in terms of purity, internal structural integrity, and high-temperature stability.
[0059] Based on the above analysis, the method for preparing quartz sand provided in this application involves sequentially hydrolyzing and aging a raw material system comprising silicate ester, alcohol solvent, ultrapure water, and catalyst to form a structurally stable first gel. This gel is then sequentially washed with ultrapure water, soaked in alcohol solvent, extracted with supercritical carbon dioxide, and sintered to finally obtain quartz sand. This method removes inorganic impurities after gel formation, replaces the solvent system, and removes deep organic residues using supercritical carbon dioxide. This ensures that the gel channels maintain good openness and structural integrity before subsequent heat treatment, thereby reducing the outgassing during sintering. The resulting quartz sand has a lower carbon content and fewer black spots, resulting in higher purity and a reduced bubble density in the quartz crucible.
[0060] In some embodiments of the present invention, the silicate ester includes at least one of methyl silicate, ethyl silicate, and propyl silicate, preferably ethyl silicate, with a purity ≥99.999%.
[0061] In some embodiments, the alcohol solvent includes at least one of methanol, ethanol, and propanol, preferably electronic-grade anhydrous ethanol.
[0062] In some embodiments, the molar ratio of silicate ester, alcohol solvent, and ultrapure water is 1:(3~4):(2~6), for example, it can be a range of 1:3:2, 1:4:6, 1:3:6, 1:3:5, 1:4:2, 1:4:5, or any two of them.
[0063] In this embodiment, silicate ester, alcohol solvent, and ultrapure water are prepared as a raw material system in a molar ratio of 1:(3~4):(2~6). When the amount of silicate ester is set to 1 part, the alcohol solvent is controlled at 3~4 parts, and the ultrapure water at 2~6 parts. This ensures that the system has sufficient dissolving and dispersing capabilities while guaranteeing that the hydrolysis reaction proceeds fully without causing localized, excessively rapid gelation. This ratio allows hydrolysis and polycondensation to proceed simultaneously in a relatively uniform environment, resulting in a relatively continuous and more stable first gel pore structure. This facilitates the migration and removal of residual components during subsequent washing, solvent replacement, and supercritical carbon dioxide extraction, thereby reducing the risk of residual carbon, black spots, and bubble defects after sintering.
[0064] In specific formulations, silicate esters can be selected individually from methyl silicate, ethyl silicate, or propyl silicate, or a combination of two or three can be used to suit different reaction rates and gel strength requirements. Alcohol solvents can be selected individually from methanol, ethanol, or propanol, or a combination of several can be used to improve the solubility of the raw material system and the compatibility with subsequent displacement processes. Through the above selection of raw materials and control of molar ratios, a homogeneous precursor solution suitable for subsequent processing can be formed, thereby improving the integrity of the gel structure and the purity and stability of the final quartz sand.
[0065] In some embodiments of the present invention, the hydrolysis temperature is 20~60°C, for example, it can be a range of 20°C, 30°C, 40°C, 50°C, 60°C or any combination thereof.
[0066] In some embodiments, the hydrolysis treatment time is 2 to 4 hours, for example, it can be a range of 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours or any two of these.
[0067] In some embodiments, the aging temperature is 40~60°C, for example, it can be a range of 40°C, 45°C, 50°C, 55°C, 60°C or any combination thereof.
[0068] In some embodiments, the aging time is 12 to 24 hours, for example, it can be a range of 12 hours, 18 hours, 20 hours, 22 hours, 24 hours or any two of them.
[0069] In this embodiment, the hydrolysis treatment is carried out at 20~60°C, with a hydrolysis time of 2~4 hours, so that the silicate ester can be hydrolyzed under relatively mild conditions without excessively initiating local rapid condensation. This temperature range can meet the activation conditions required for the reaction, while avoiding excessively rapid local densification of the gel and premature shrinkage of the pores due to excessively high temperatures, thereby hindering the migration of subsequent internal components. Controlling the hydrolysis time to 2~4 hours ensures that the degree of hydrolysis reaches the level required for the formation of a stable gel, reduces unreacted silicate ester residue, and ensures the uniformity of the first gel formation.
[0070] The aging process is carried out at 40–60°C and maintained for 12–24 hours, allowing the gel network to continue to complete condensation and structural rearrangement in a relatively stable thermal environment. This temperature range promotes further cross-linking of the gel backbone while inhibiting insufficient aging due to insufficient temperature and excessively rapid structural shrinkage due to excessive temperature. By setting the aging time to 12–24 hours, the solvent, oligomers, and unreacted components within the gel are redistributed in the network, resulting in a more stable and better-connected first gel structure. This creates favorable conditions for subsequent washing, alcohol solvent replacement, and supercritical carbon dioxide extraction, and reduces the possibility of bubbles and black spot defects caused by residual components releasing gas during the sintering stage.
[0071] In some embodiments of the present invention, the pH of the raw material system is 1.5 to 2.5 (for example, it can be a range of 1.5, 1.8, 2.0, 2.2, 2.5 or any two of them) or 9.0 to 10.0 (for example, it can be a range of 9.0, 9.2, 9.5, 9.8, 10.0 or any two of them).
[0072] In this embodiment, the raw material system is adjusted by a pH adjuster after batching to maintain it within the aforementioned acidic or alkaline range. This pH range allows the Si-OR bonds in the silicate ester molecules to be effectively broken under catalysis and converted into Si-OH groups, subsequently forming a continuous first gel backbone through polycondensation. Meanwhile, the gel network formed under acidic conditions is generally more uniform, while under alkaline conditions, the structural inhomogeneity caused by excessively rapid local polymerization can be reduced by adjusting the matching relationship between the hydrolysis rate and the polycondensation rate. This provides a precursor with a more stable pore distribution for subsequent washing, soaking, supercritical carbon dioxide extraction, and sintering processes.
[0073] When the pH of the raw material system is below 1.5 or above 10.0, the hydrolysis or condensation reaction is prone to imbalance, which leads to local densification of the gel structure or discontinuity of the skeleton, which is not conducive to the migration and removal of internal organic components. However, when the pH is limited to 1.5~2.5 or 9.0~10.0, the controllable formation of the gel structure can be maintained while ensuring the reactivity. This allows the first gel to have better network integrity and adaptability to subsequent processing, thereby reducing black spots and bubble defects caused by residual organic matter in the sintering stage and improving the purity and structural stability of the obtained quartz sand.
[0074] In some embodiments of the present invention, the catalyst includes an acidic catalyst and / or a basic catalyst. The acidic catalyst includes at least one selected from hydrochloric acid, nitric acid, and acetic acid, preferably hydrochloric acid. The basic catalyst includes at least one selected from ammonia and tetramethylammonium hydroxide, preferably ammonia.
[0075] During the preparation process, adding the catalyst to the raw material system, which includes silicate esters, alcohol solvents, and ultrapure water, maintains the pH of the system within a range suitable for hydrolysis and aging. This facilitates the hydrolysis of alkoxy groups in the silicate ester molecules, generating silanol intermediates, which further form a uniform gel network through polycondensation. Using an acidic catalyst allows for a more stable hydrolysis rate via an acidic catalytic pathway, enabling the gel framework to form gradually without localized rapid gelation. Using an alkaline catalyst promotes polycondensation between silanols via an alkaline catalytic pathway, resulting in a more fully cross-linked gel network. By limiting the acidic and alkaline catalysts to at least one of hydrochloric acid, nitric acid, acetic acid, ammonia, and tetramethylammonium hydroxide, the catalytic activity, impurity introduction level, and ease of subsequent washing and removal can be controlled. This results in a more uniform pore structure in the obtained first gel, which is beneficial for the removal of organic components during subsequent washing, solvent replacement, supercritical carbon dioxide extraction, and sintering processes, reducing residual carbon and bubble defects.
[0076] In some embodiments of the present invention, the number of soaking treatments is 3 to 5 times, for example, it can be a range of 3 times, 4 times, 5 times or any combination thereof.
[0077] In some embodiments, the soaking time for each treatment is 1 to 2 hours, for example, it can be a range of 1 hour, 1.2 hours, 1.5 hours, 1.8 hours, 2 hours or any two of these.
[0078] In this embodiment, the second gel is immersed in an alcohol solvent 3-5 times, with each immersion lasting 1-2 hours. This allows the alcohol solvent to repeatedly diffuse into the gel and gradually renew the residual medium within the pores. Controlling the number of immersions to 3-5 times ensures sufficient repeatability and thoroughness of the replacement process, preventing the outer solvent from quickly reaching local equilibrium during a single treatment, which would hinder the continued migration of internal residues. Controlling the immersion time to 1-2 hours ensures sufficient mass transfer while avoiding excessive shrinkage and structural disturbance of the gel skeleton caused by prolonged immersion. Through this synergistic control of the number of immersions and time, the alcohol solvent can continuously remove residual organic components from the gel pores, significantly reducing the volatile residues within the third gel. This mitigates outgassing during subsequent high-temperature processing, thereby reducing bubbles and black spot defects and improving the purity, structural stability, and reliability of the resulting quartz sand for subsequent use.
[0079] In this invention, the alcohol solvent is replaced with fresh solvent after each soaking for 1-2 hours, for a total of 3-5 times. For example, after the first soaking, the water content in the replacement solution is 15-20%; after the second soaking, the water content is 3-5%; after the third soaking, the water content is 0.5-1%; after the fourth soaking, the water content is 0.1-0.2%; and after the fifth soaking, the water content is <500 ppm.
[0080] In some embodiments of the present invention, the temperature of the supercritical carbon dioxide extraction process is 40~60°C, for example, it can be a range of 40°C, 45°C, 50°C, 55°C, 60°C or any combination thereof; preferably 45~55°C.
[0081] In some embodiments, the pressure of supercritical carbon dioxide extraction is 10-20 MPa, for example, it can be a range of 10 MPa, 12 MPa, 15 MPa, 18 MPa, 20 MPa or any two of them; preferably 12-18 MPa.
[0082] In some embodiments, the supercritical carbon dioxide extraction treatment time is 3 to 8 hours, for example, it can be a range of 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours or any two of them.
[0083] In practice, the third gel is placed in a high-pressure extraction vessel, carbon dioxide is introduced and pressurized to 10-20 MPa, while the system temperature is controlled at 40-60°C, allowing the carbon dioxide to form a supercritical fluid with both gas diffusion and liquid solubility capabilities. This temperature and pressure combination ensures stable mass transfer of supercritical carbon dioxide while preventing thermal shrinkage of the gel structure due to excessively high temperatures, thus allowing the extraction medium to more fully enter the pores and carry out residual organic matter. When the temperature is controlled at 45-55°C and the pressure at 12-18 MPa, the density and diffusion capacity of carbon dioxide are in optimal balance, thereby enhancing the dissolution and migration of alcohol residues and reducing outgassing sources during subsequent sintering.
[0084] The extraction time is controlled at 3-8 hours to ensure sufficient contact and exchange time between the supercritical medium and the internal pores of the gel, so that the residual organic components in the deep pores can be gradually precipitated and continuously carried away; if the time is too short, the extraction will be insufficient, and if the time is too long, it will increase energy consumption and have limited effect on the removal effect.
[0085] By synergistically limiting temperature, pressure, and time within the aforementioned ranges, the organic residue content can be significantly reduced while maintaining the integrity of the gel skeleton. This makes the resulting fourth gel less prone to defects such as bubbles, black spots, and residual carbon during subsequent sintering, thereby improving the purity, density, and high-temperature stability of the final quartz sand.
[0086] In some embodiments of the present invention, the sintering process includes a first sintering process and a second sintering process performed sequentially.
[0087] Preferably, the temperature of the first sintering treatment is 600~850℃, for example, it can be a range of 600℃, 700℃, 750℃, 800℃, 850℃ or any two of them; preferably 700~800℃.
[0088] In some embodiments, the time for the first sintering treatment is 2 to 6 hours, for example, it can be a range of 2 hours, 3 hours, 4 hours, 5 hours, 6 hours or any two of them; preferably 3 to 5 hours.
[0089] In some embodiments, the temperature of the second sintering process is 1150~1250°C, for example, it can be a range of 1150°C, 1180°C, 1200°C, 1220°C, 1250°C or any two of these.
[0090] In some embodiments, the second sintering treatment time is 4 to 8 hours, for example, it can be a range of 4 hours, 5 hours, 6 hours, 7 hours, 8 hours or any two of them.
[0091] The first sintering process involves pre-firing the fourth gel, which gradually removes residual organic components, volatile components, and some hydroxyl structures from the gel, and promotes initial necking and skeletal rearrangement between particles. The second sintering process involves further high-temperature sintering of the pre-fired material at a higher temperature, which further transforms and densifies the quartz network, thereby forming structurally stable quartz sand.
[0092] In practice, the porous SiO2 sand-like precursor, i.e., the fourth gel, is placed in a tube furnace or box furnace and subjected to a first sintering treatment in a clean, dry air atmosphere. The temperature is raised to 600-850°C at a rate of 2-5°C / min and held at this temperature for 2-6 hours, followed by furnace cooling to room temperature. This allows residual organic matter inside the gel to gradually decompose and escape under relatively gentle thermal action, i.e., the residual alkoxy groups (-OR) and organic carbon components are oxidized to generate CO2 and H2O, which then volatilize and escape. Simultaneously, it avoids premature surface densification due to excessively rapid heating, which could lead to internal gas trapping. This temperature range is below the viscous flow temperature of SiO2 (>1100°C), ensuring that the gel pores remain open during decarburization, preventing premature sintering and closure that could result in residual carbon encapsulation. After this step, the particles remain in a porous, low-density state (bulk density approximately 0.05-0.20 g / cm³). 3 The carbon content was detected using the high-temperature combustion-infrared method (LECO), with a target value of <1ppm.
[0093] The temperature is then raised to 1150-1250℃ for a second sintering treatment and maintained for 4-8 hours. Within this high-temperature range, the silica network further rearranges and sinters, the residual micropores continue to close, and the interparticle bonding becomes tighter, resulting in quartz sand with higher purity and more uniform structure. By using a segmented approach of first removing residues at low temperature and then densifying at high temperature, the probability of black spots, residual carbon, and bubble defects can be effectively reduced, and the high-temperature stability of the obtained quartz sand can be improved.
[0094] In one embodiment, porous SiO2 precursor powder with the first sintering treatment completed and the carbon content meeting the standard is placed in a high-temperature sintering furnace and heated to 1150-1250°C at a heating rate of 2-5°C / min, and held at that temperature for 4-8 hours. This causes the SiO2 particles to undergo viscous flow, and the residual mesopores inside the particles gradually close and shrink until they disappear. The true density of the particles gradually approaches the theoretical density of amorphous SiO2 (approximately 2.20 g / cm³). 3 The final product is a dense, low-hydroxyl synthetic high-purity quartz sand. The cooling rate is controlled at 2~5°C / min to prevent thermal stress cracking. After exiting the furnace, it is sealed in double-layer high-purity polyethylene bags in a Class 100 cleanroom.
[0095] In some embodiments of the present invention, the depressurization rate after supercritical carbon dioxide extraction is 0.5~2.0 MPa / h, for example, it can be a range of 0.5 MPa / h, 0.8 MPa / h, 1.0 MPa / h, 1.5 MPa / h, 2.0 MPa / h or any two of them; preferably 0.5~1.5 MPa / h.
[0096] By controlling the depressurization rate within the range of 0.5–2.0 MPa / h, with 0.5–1.5 MPa / h being the preferred range, supercritical carbon dioxide can be released smoothly, avoiding excessive pressure difference between the inside and outside of the pores caused by sudden pressure drops, which could lead to shrinkage, cracking, or local collapse of the gel skeleton, thus maintaining the stability of the fourth gel. The mechanism is that slow depressurization allows sufficient time for residual carbon dioxide and dissolved components to diffuse and migrate, gradually balancing the pressure inside and outside the pores. This reduces structural disturbance and minimizes defect sources before subsequent sintering, ultimately ensuring the uniformity of the resulting quartz sand's structure and the stability of its purity.
[0097] When the depressurization rate is too fast, some CO2 in the reactor enters the gas-liquid two-phase region, and the interfacial tension reappears, which may cause some channels to collapse; the preferred depressurization rate is 0.5~1.5MPa / h to ensure that CO2 is discharged in a supercritical or near-supercritical state.
[0098] In some embodiments of the present invention, the supercritical carbon dioxide extraction process further includes: crushing the fourth gel; preferably, the Dv50 of the crushed gel is 100~150μm, for example, it can be a range of 100μm, 110μm, 120μm, 130μm, 140μm, 150μm or any two of these; Dv90≤200μm, for example, it can be a range of 100μm, 110μm, 120μm, 130μm, 140μm, 150μm, 160μm, 170μm, 180μm, 190μm, 200μm or any two of these.
[0099] Wherein, Dv50 represents the particle size corresponding to 50% of the particle volume in the cumulative distribution, and Dv90 represents the particle size corresponding to 90% of the particle volume in the cumulative distribution. Both are used to characterize the median particle size and the upper limit of coarse particles of the gel particles after breakage.
[0100] After supercritical carbon dioxide extraction, the resulting fourth gel (aerogel framework) is a low-density porous mass with a brittle texture. It requires mechanical crushing and particle size classification to obtain sand-like particles that meet the requirements of the crucible forming process. The fourth gel is fed into crushing equipment for mechanical crushing. For example, the fourth gel mass is fed into a jaw crusher or roller crusher lined with high-purity corundum or zirconia ceramic for primary crushing, followed by screening by an air classifier or vibrating screen, collecting the product according to the target particle size range. According to the crucible production process requirements, the target particle size range is 70~300 mesh (i.e., 50~200μm). Particles of unqualified sizes (too coarse or too fine) are returned for further crushing or processing. The gel transforms from a continuous mass or large agglomerate into a more uniform granular material. Controlling the crushed gel to a Dv50 of 100-150 μm, Dv90 ≤ 200 μm, and Dv10 not less than 30 μm ensures that the particle size matches the heat and mass transfer processes during subsequent sintering. This avoids excessively long diffusion paths for residual components due to overly large particles, and also prevents excessive agglomeration, uneven packing, or abnormal sintering shrinkage due to overly fine particles. Since the fourth gel is already in a low organic residue state after supercritical carbon dioxide extraction, moderate crushing can further expose internal pores and surface channels, allowing for smoother gas escape during subsequent sintering. This reduces defects such as closed pores, black spots, and bubbles caused by localized gas release, resulting in a simultaneous improvement in the purity, uniformity, and structural stability of the obtained quartz sand.
[0101] It should be noted that the product obtained in this step is a high specific surface area porous SiO2 powder, which appears as a white, loose, sandy substance. The internal pores of the particles still maintain a fully open mesoporous structure, and the particle bulk density at this stage is approximately 0.05~0.20 g / cm³. 3 (Aerogel characteristic density), different from the final densed quartz sand product. Particle morphology control (particle size, sphericity) is completed in this step; subsequent sintering processes only treat the chemical composition and structural density, without altering the particle size distribution. Crushing and screening are carried out entirely in a Class 100 cleanroom, and the contact surfaces between the equipment and the gel must be passivated with high-purity acid to prevent metal contamination.
[0102] The technical solution of the present invention will be further described below with reference to specific embodiments.
[0103] Example 1
[0104] The method for preparing quartz sand in this embodiment includes the following steps:
[0105] 1) Mix ethyl silicate, ethanol and water in a molar ratio of 1:3.5:4 to obtain a mixture; add high-purity hydrochloric acid to the mixture to adjust the pH of the system to 2.0, carry out hydrolysis reaction at 40°C for 3 hours, age at 50°C for 2 hours, and then let stand for 18 hours to obtain the first gel.
[0106] 2) The first gel was washed with ultrapure water in a six-stage countercurrent process at 25°C and normal pressure. The conductivity of the final washing solution was 1.2 μS / cm, and the second gel was obtained.
[0107] 3) Immerse the second gel in sufficient anhydrous ethanol and let it stand at 25°C for a total of 4 times, each time for 1.5 hours. The water content of the final soaking solution is 320 ppm, and the third gel is obtained.
[0108] 4) The third gel was loaded into a supercritical fluid extraction apparatus, sealed, and then food-grade CO2 (purity ≥99.9%) was introduced. The pressure was slowly increased to 15 MPa, while the temperature was simultaneously raised to 50°C, allowing the CO2 to enter a supercritical state. Under supercritical conditions, supercritical CO2 was continuously introduced to extract and displace the ethanol in the pores of the third gel for 5 hours, yielding the fourth gel. After displacement, the pressure was slowly reduced to atmospheric pressure at a rate of 1.0 MPa / h to complete the drying process.
[0109] 5) The fourth gel is fed into a zirconia ceramic-lined jaw crusher for primary crushing, and then screened by an air classifier to crush and screen the fourth gel to Dv50 of 130μm and Dv90 of 180μm.
[0110] 6) Under a clean air atmosphere, the fourth gel was subjected to a first sintering treatment at 700°C for 4 hours at a heating rate of 3°C / min; then, the temperature was increased at 1200°C for a second sintering treatment at a heating rate of 3°C / min for 6 hours to obtain quartz sand.
[0111] Example 2
[0112] The preparation method of quartz sand in this embodiment is basically the same as that in Example 1, except that the temperature of the supercritical carbon dioxide extraction treatment in step 4) is 60°C.
[0113] Example 3
[0114] The preparation method of quartz sand in this embodiment is basically the same as that in Example 1, except that the temperature of supercritical carbon dioxide extraction treatment in step 4) is 40°C.
[0115] Example 4
[0116] The preparation method of quartz sand in this embodiment is basically the same as that in Example 1, except that the pressure of supercritical carbon dioxide extraction treatment in step 4) is 20 MPa.
[0117] Example 5
[0118] The preparation method of quartz sand in this embodiment is basically the same as that in Example 1, except that the pressure of supercritical carbon dioxide extraction treatment in step 4) is 10 MPa.
[0119] Example 6
[0120] The preparation method of quartz sand in this embodiment is basically the same as that in Example 1, except that the supercritical carbon dioxide extraction treatment time in step 4) is 8 hours.
[0121] Example 7
[0122] The preparation method of quartz sand in this embodiment is basically the same as that in Example 1, except that the supercritical carbon dioxide extraction treatment time in step 4) is 3 hours.
[0123] Example 8
[0124] The preparation method of quartz sand in this embodiment is basically the same as that in Example 1, except that in step 4), the pressure reduction rate is 0.5 MPa / h.
[0125] Example 9
[0126] The preparation method of quartz sand in this embodiment is basically the same as that in Example 1, except that in step 4), the pressure reduction rate is 2.0 MPa / h.
[0127] Example 10
[0128] The preparation method of the quartz sand in this embodiment is basically the same as that in Example 1. The difference is that in step 1), ethyl silicate, ethanol and water are mixed in a molar ratio of 1:4:6 to obtain a mixture; high-purity ammonia is added to the mixture to adjust the pH of the system to 9.5, and hydrolysis reaction is carried out at 50°C for 4 hours, aged at 55°C for 2 hours and then allowed to stand for 24 hours to obtain the first gel.
[0129] Example 11
[0130] The preparation method of quartz sand in this embodiment is basically the same as that in Example 1, except that in step 4), the pressure reduction rate is 5 MPa / h.
[0131] Example 12
[0132] The preparation method of quartz sand in this embodiment is basically the same as that in Example 1, except that in step 6), the temperature of the first sintering treatment is 500°C.
[0133] Example 13
[0134] The preparation method of quartz sand in this embodiment is basically the same as that in Example 1, except that in step 6), the temperature of the first sintering treatment is 950°C.
[0135] Example 14
[0136] The preparation method of quartz sand in this embodiment is basically the same as that in Example 1, except that the supercritical carbon dioxide extraction treatment time in step 4) is 1 hour.
[0137] Example 15
[0138] The preparation method of quartz sand in this embodiment is basically the same as that in Example 1, except that in step 3), the soaking treatment is performed once.
[0139] Comparative Example 1
[0140] The preparation method of this comparative example is basically the same as that of the quartz sand in Example 1, except that steps 3) and 4) are replaced by drying the second gel at -0.09 MPa and 100°C for 18 h.
[0141] Comparative Example 2
[0142] The preparation method of the comparative example and the quartz sand in Example 1 are basically the same, except that in step 4), the temperature is 25°C (lower than the critical temperature of CO2 31.1°C), under which CO2 is in liquid state.
[0143] Comparative Example 3
[0144] The preparation method of the quartz sand in this comparative example is basically the same as that in Example 1. The difference is that in step 4), the pressure is 6 MPa (lower than the critical pressure of CO2 7.38 MPa). Under this condition, CO2 is in a gaseous state and has a very low density (about 0.15 g / L).
[0145] Comparative Example 4
[0146] The preparation method of the comparative example and the quartz sand in Example 1 are basically the same, except that steps 3) and 4) are replaced by: placing the second gel in a ventilated environment and drying it under normal pressure (25°C, relative humidity <50%) for 24 hours.
[0147] Comparative Example 5
[0148] The preparation method of the comparative example and the quartz sand in Example 1 are basically the same, except that in step 4), supercritical N2 (critical temperature of -147°C and critical pressure of 3.39 MPa) is used for extraction and displacement.
[0149] Experimental example:
[0150] Quartz crucible sample preparation:
[0151] The quartz sand obtained in each embodiment and comparative example was used as the raw material for the transparent layer of the quartz crucible. It was molded and melted according to the same crucible preparation process: first, the quartz sand was loaded into a clean quartz mold and compacted; then, it was heated and melted in a vacuum rotary melting device; after cooling, the quartz crucible samples were obtained. The raw material dosage, molding pressure, melting temperature, holding time, and cooling conditions were kept consistent for each group of samples to eliminate the influence of the crucible preparation process on the test results.
[0152] 1. Carbon content was detected using the high-temperature combustion-infrared method (LECO CS844), with a detection limit of 0.1 ppm and repeatability of ±0.1 ppm.
[0153] 2. The bubble density is the number of bubbles per unit area of the transparent layer of the crucible, measured by microscopy at a magnification of 50×.
[0154] Table 1
[0155]
[0156] As shown in Table 1, compared with the comparative example, the method for preparing quartz sand provided by the present invention, by sequentially hydrolyzing and aging a raw material system including silicate ester, alcohol solvent, ultrapure water and catalyst to form a first gel, and then sequentially washing with ultrapure water, soaking in alcohol solvent, supercritical carbon dioxide extraction and sintering, can effectively remove residual components inside the gel and reduce the risk of pore structure shrinkage or collapse during the preparation of quartz sand, thereby reducing residual carbon and black spot defects, improving the purity of quartz sand, and thus reducing the bubble density of the quartz crucible.
[0157] Comparative Examples 1 and 11: In Example 11, the rapid depressurization caused some CO2 to enter the gas-liquid two-phase region, the capillary force at the interface reappeared, and about 20-30% of the channels collapsed.
[0158] Comparative Examples 1 and 12: The first sintering temperature in Example 12 was too low, resulting in a slower oxidation kinetic rate of organic carbon. In particular, the activation energy for breaking silane coupling functional groups (Si-OC2H5 bonds) embedded deep in the gel skeleton was high, leading to incomplete oxidation reaction.
[0159] Compared with Example 1 and Example 13, the first sintering temperature of Example 13 was too high, and the amorphous SiO2 began to undergo initial viscous flow. Some small-diameter mesopores (<5nm) showed local necking and narrowing, a small number of channels were closed in advance, and residual organic matter was encapsulated.
[0160] Compared with Comparative Examples 1 and 14, the supercritical carbon dioxide extraction treatment time in Example 14 was too short. Supercritical CO2 could only replace about 30-50% of the pore volume on the surface of the particles, resulting in a high residual amount of ethanol in the deep pores.
[0161] Comparative Examples 1 and 15: In Example 15, the number of soaking treatments was too few, and a large amount of water remained in the pores of the third gel. After entering the supercritical extraction vessel, the solubility of water in supercritical CO2 was extremely low, and the water in the pores could not be effectively replaced. When the pressure was reduced, the capillary force of water (γ≈72 mN / m) caused a large number of pores to collapse.
[0162] Comparative Examples 1 and 2: In Comparative Example 2, CO2 is in liquid form and has a certain solubility in ethanol (about 5-8 mol%), which can partially replace the ethanol in the gel pores. However, when the liquid CO2 is depressurized, capillary forces are generated at the gas-liquid interface, causing some pores to collapse. This leads to an increase in the carbon content and number of black spots in the quartz sand, and a decrease in purity, which in turn leads to an increase in the bubble density of the quartz crucible.
[0163] Comparative Examples 1 and 3. In Comparative Example 3, CO2 is in a gaseous state with extremely low density (approximately 0.15 g / L), has very weak ethanol solubility, and low ethanol replacement rate.
[0164] In Comparative Examples 1 and 4, during the drying process of the second gel in Comparative Example 4, the natural evaporation of moisture generated gas-liquid interface and capillary force, resulting in the collapse of a large number of gel channels.
[0165] Comparative Examples 1 and 5: In Comparative Example 5, N2 is a nonpolar small molecule, with a significant difference in polarity compared to ethanol. The Hildebrand solubility parameters differ considerably, indicating that N2's ability to dissolve and carry ethanol is far lower than that of supercritical CO2. Supercritical N2 has zero surface tension, and its pores are not damaged by capillary forces during drying, resulting in pore-preserving effects comparable to supercritical CO2. However, its ethanol extraction efficiency is low, requiring longer extraction times or larger N2 volumes to achieve the same displacement effect. Furthermore, N2 is more expensive (>10 times the cost of CO2), and its storage and transportation are less convenient than liquid CO2, making it less practical for engineering applications.
[0166] Finally, it should be noted that other embodiments of the invention will readily occur to those skilled in the art upon consideration of the specification and practice of the invention disclosed herein. This invention is intended to cover any variations, uses, or adaptations of the invention that follow the general principles of the invention and include common knowledge or customary techniques in the art not disclosed herein, and is not limited to what has been described above. Various modifications and changes can be made without departing from its scope. The scope of the invention is limited only by the appended claims.
Claims
1. A method for preparing quartz sand, characterized in that, Includes the following steps: 1) The raw material system, including silicate ester, alcohol solvent, ultrapure water and catalyst, was subjected to hydrolysis and aging treatment in sequence to obtain the first gel; 2) The first gel was washed with ultrapure water to obtain the second gel; 3) The second gel is soaked in an alcohol solvent to obtain a third gel; 4) The third gel is subjected to supercritical carbon dioxide extraction to obtain the fourth gel; 5) The fourth gel is sintered to obtain the quartz sand.
2. The preparation method according to claim 1, characterized in that, The silicate ester includes at least one of methyl silicate, ethyl silicate, and propyl silicate; And / or, the alcohol solvent includes at least one of methanol, ethanol, and propanol; And / or, the molar ratio of the silicate ester, the alcohol solvent, and the ultrapure water is 1:(3~4):(2~6).
3. The preparation method according to claim 1 or 2, characterized in that, The hydrolysis treatment temperature is 20~60℃; And / or, the hydrolysis treatment time is 2-4 hours; And / or, the aging treatment temperature is 40~60℃; And / or, the aging process takes 12 to 24 hours.
4. The preparation method according to any one of claims 1-3, characterized in that, The pH of the raw material system is 1.5~2.5 or 9.0~10.
0.
5. The preparation method according to any one of claims 1-4, characterized in that, The catalyst includes acidic catalysts and / or basic catalysts; Preferably, the acidic catalyst includes at least one of hydrochloric acid, nitric acid, and acetic acid; Preferably, the alkaline catalyst includes at least one of ammonia and tetramethylammonium hydroxide.
6. The preparation method according to any one of claims 1-5, characterized in that, The soaking treatment is repeated 3 to 5 times; And / or, the soaking time for each soaking treatment is 1 to 2 hours.
7. The preparation method according to any one of claims 1-6, characterized in that, The temperature for supercritical carbon dioxide extraction is 40~60℃, preferably 45~55℃; And / or, the pressure of the supercritical carbon dioxide extraction treatment is 10~20MPa, preferably 12~18MPa; And / or, the supercritical carbon dioxide extraction treatment time is 3~8h.
8. The preparation method according to any one of claims 1-7, characterized in that, The sintering process includes a first sintering process and a second sintering process performed sequentially. Preferably, the temperature of the first sintering treatment is 600~850℃, more preferably 700~800℃; And / or, the time for the first sintering treatment is 2 to 6 hours, preferably 3 to 5 hours; And / or, the temperature of the second sintering treatment is 1150~1250℃; And / or, the second sintering treatment time is 4~8 hours.
9. The preparation method according to any one of claims 1-8, characterized in that, The depressurization rate after supercritical carbon dioxide extraction is 0.5~2.0 MPa / h, preferably 0.5~1.5 MPa / h.
10. The preparation method according to any one of claims 1-9, characterized in that, The supercritical carbon dioxide extraction process further includes: breaking down the fourth gel. Preferably, the Dv50 of the gel after the crushing treatment is 100~150μm and the Dv90 is ≤200μm.