Optical fibers and their fabrication methods
By using optical fibers with silica aerogel cores, the problem of quartz-aerogel interface loss is solved, achieving high sensitivity and fast response of fiber optic gas sensors, which are suitable for dry gas Raman sensors.
Patent Information
- Application Number
- CN202611315826.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-27
- Publication Date
- 2026-11-17
AI Technical Summary
Existing optical fibers use quartz as the main light guide and aerogel as an auxiliary structure. When light is scattered and lost at the quartz-aerogel interface, the improvement of detection sensitivity is limited when the optical fiber is used in gas sensors.
Using silica aerogel as the fiber core material, an integrally formed optical fiber is prepared by mixing silicon source, catalyst, stress modifier and solvent, combined with supercritical carbon dioxide drying technology. The high specific surface area and suitable refractive index of silica aerogel are used to realize the functions of light transmission and gas enrichment, avoiding interface loss.
It improves the sensitivity of fiber optic gas sensors, enables stable long-distance transmission of optical signals and rapid gas enrichment, reduces the difficulty of optical path coupling, and is suitable for dry gas Raman sensors.
Smart Images

Figure CN123105666A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of optical fiber technology, and in particular to an optical fiber and its fabrication method. Background Technology
[0002] Existing optical fibers, such as those used in dry gas Raman sensors, typically use high-refractive-index quartz glass as the light-guiding body and aerogel in bulk, thin film, or powder form as the spectral enhancement substrate. For example, aerogel films are modified onto the end face of ordinary quartz optical fibers to construct a surface-enhanced Raman spectroscopy gas sensing substrate, relying on the large specific surface area of the aerogel to increase gas adsorption and thus enhance the Raman detection signal. Another example is using pre-fabricated aerogel powder or sol-gel precursor liquid as a filling coating, covering or filling the cladding gaps or hollow core of commercial quartz optical fibers, serving only as a sensing auxiliary medium; the optical fiber's own light transmission still relies on the quartz core layer. However, optical fibers using quartz as the light-guiding body and combined with aerogel have interface defects. Light is prone to scattering loss at the quartz-aerogel interface, limiting the improvement in detection sensitivity when the fiber is used in gas sensors.
[0003] Therefore, there is an urgent need for an optical fiber and its fabrication method to solve the above-mentioned technical problems. Summary of the Invention
[0004] In view of this, the present invention proposes an optical fiber and its preparation method to solve the technical problem that existing optical fibers use quartz as the main light guide and aerogel as an auxiliary structure, which easily causes interface loss and makes it difficult to improve the detection sensitivity of sensors using optical fibers.
[0005] The technical solution of this invention is implemented as follows: In a first aspect, the present invention provides an optical fiber, comprising: a fiber core, wherein the fiber core is made of silica aerogel; The specific surface area of the fiber core is 800 m². 2 / g to 900m 2 / g, wherein the refractive index of the fiber core is 1.03 to 1.05.
[0006] In some embodiments, the optical fiber further includes a cladding that covers the surface of the fiber core, the cladding being air; The optical fiber has a numerical aperture of 0.26 to 0.32 and a fiber core optical loss per unit length of 0.15 dB / cm to 0.19 dB / cm.
[0007] In some embodiments, the total pore volume at a single point in the fiber core is 0.7 cm. 3 / g to 0.85cm 3 / g, the average pore size of the fiber core is 3.5nm to 4nm.
[0008] Secondly, the present invention also provides a method for preparing an optical fiber, comprising: A silicon source, catalyst, stress modifier, first solvent, and water are mixed and then treated to obtain a precursor. The precursor is gelled in a tubular mold to obtain a wet gel fiber core preform. The wet gel fiber core preform is subjected to aging treatment to obtain a wet gel fiber core; The wet gel fiber core is subjected to supercritical carbon dioxide drying to obtain the optical fiber; Wherein, the silicon source is selected from at least one of tetramethoxysilane and tetraethyl orthosilicate, the catalyst is selected from at least one of ammonia, an aqueous solution of ethylamine and an aqueous solution of monomethylamine, the stress modifier is selected from at least one of N,N-dimethylformamide and N,N-dimethylacetamide, and the first solvent is selected from at least one of methanol and anhydrous ethanol. The mass ratio of the silicon source, the catalyst, the stress modifier, the first solvent, and the water is (31 to 34 parts): (0.21 to 0.3 parts): (1.19 to 1.63 parts): (71.78 to 93.03 parts): (22.02 to 28.17 parts).
[0009] In some embodiments, the gelation treatment time is greater than or equal to 10 minutes, and the gelation treatment time is less than or equal to 10 hours; The gelation treatment temperature is greater than or equal to 20°C, and the gelation treatment temperature is less than or equal to 40°C.
[0010] In some embodiments, the inner diameter of the tubular mold is 100 micrometers to 2 millimeters, and the length of the tubular mold is 1 centimeter to 10 centimeters; The tubular mold is made of at least one of polytetrafluoroethylene, polypropylene, and polyethylene.
[0011] In some embodiments, the step of obtaining a wet gel fiber core by aging the wet gel fiber core preform includes: The wet gel fiber core preform is obtained by aging in a second solvent at an aging temperature and for an aging time. The second solvent is selected from at least one of anhydrous ethanol, isopropanol and methanol, the aging temperature is 20°C to 30°C, and the aging time is 24 hours to 96 hours.
[0012] In some embodiments, the second solvent is replaced three times or more during the aging process.
[0013] In some embodiments, the step of obtaining the optical fiber by supercritical carbon dioxide drying of the wet gel fiber core includes: The wet gel fiber core is dried under supercritical carbon dioxide for a specified time under drying pressure and temperature to obtain the optical fiber. The drying pressure is 8 MPa to 9 MPa, the drying temperature is 35°C to 40°C, and the drying time is greater than or equal to 2.5 hours and less than or equal to 6 hours.
[0014] In some embodiments, the rate of pressure increase to reach the drying pressure is from 0.5 MPa / min to 1 MPa / min; After the supercritical carbon dioxide drying process is completed, the pressure relief rate is greater than 0 MPa / h and less than or equal to 0.5 MPa / h.
[0015] The optical fiber and its preparation method of the present invention have the following advantages over the prior art: by using a silica aerogel core as the light guide body, and utilizing the high specific surface area and suitable refractive index of silica aerogel, the functions of light transmission and gas enrichment are completed in one piece, avoiding the interface loss of light between silica aerogel and the light guide body, and improving the sensitivity of gas sensors using optical fibers. Attached Figure Description
[0016] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0017] Figure 1a This is a schematic diagram of the structure of the optical fiber of the present invention; Figure 1b for Figure 1a A schematic diagram of the optical fiber's profile at section AA'. Figure 1c for Figure 1a A schematic diagram of the microporous network structure of optical fiber in section AA'. Figure 1d This is a schematic diagram of an optical path transmission of light within the optical fiber of this invention. Figure 2 This is a schematic diagram of the optical fiber fabrication process according to Embodiment 1 of the present invention; Figure 3a The image shows a first scanning electron microscope (SEM) result of the cross-section of the optical fiber prepared in Example 1 of the present invention. Figure 3bA scanning electron microscope image of the natural fracture surface of the optical fiber prepared in Example 1 of the present invention; Figure 3c A second scanning electron microscope image of the cross-section of the optical fiber prepared in Example 1 of the present invention; Figure 3d A third scanning electron microscope image of the cross-section of the optical fiber prepared in Example 1 of the present invention; Figure 4 The 77K nitrogen adsorption-desorption isotherm linear curve of the optical fiber prepared in Example 1 of the present invention; Figure 5 The differential pore size distribution curve of the BJH (Barrett-Joyner-Halenda) adsorption branch of the optical fiber prepared in Example 1 of the present invention is shown. Detailed Implementation
[0018] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0019] Currently, existing optical fibers use quartz as the main light guide and aerogel as an auxiliary structure. Light is easily lost at the quartz-aerogel interface, which poses a technical problem that makes it difficult to improve the detection sensitivity of sensors using optical fibers.
[0020] Please see Figures 1a to 1c In a first aspect, the present invention provides an optical fiber 100, comprising: a fiber core 110, wherein the material of the fiber core 110 is silica aerogel; The specific surface area of the fiber core 110 is 800 m². 2 / g to 900m 2 / g, the refractive index of the fiber core 110 is 1.03 to 1.05.
[0021] The optical fiber provided in this application uses a silica aerogel core as the light guide body. By utilizing the high specific surface area of silica aerogel, it integrates light transmission and gas enrichment functions, avoiding light loss at the interface between silica aerogel and the light guide body, and improving the sensitivity of the gas sensor using the optical fiber 100.
[0022] In some embodiments, the porosity of the fiber core 110 is 80% to 95%. The porosity of the fiber core 110 can be 80%, 82%, 85%, 88%, 90%, 92%, 95%, etc., which is beneficial to provide sufficient channels inside the fiber core 110 to achieve free gas permeation and gas enrichment. At the same time, it maintains the mechanical strength of the optical fiber 100 and avoids breakage and failure of the optical fiber 100 during bending, transportation, or packaging due to excessive porosity.
[0023] In some embodiments, the visible light transmittance of the fiber core 110 is 85% to 95%, and the visible light transmittance of the fiber core 110 can be 85%, 88%, 90%, 92%, 95%, etc., to achieve the high light transmittance characteristics of the fiber core 110.
[0024] In some embodiments, the refractive index of the fiber core 110 can be 1.03, 1.04, 1.05, etc., which is beneficial for the sufficient refractive index difference between the fiber core 110 and air to achieve stable total internal reflection, realize long-distance light guiding, and simultaneously control the reflection loss at the interface between the fiber core 110 and air, extend the transmission distance of light within the fiber core 110, and reduce the difficulty of optical path coupling. Figure 1d As shown, Figure 1d In the diagram, the solid line with arrows and the dashed line without arrows together represent the optical path of the light beam. When the light beam enters the core 110 from one end of the optical fiber 100, the light undergoes total internal reflection at the interface between the sidewall of the core 110 and the air. In the absence of quartz as the core layer, the optical signal is stably transmitted over a long distance along the axial direction of the optical fiber 100.
[0025] In some embodiments, the optical fiber 100 has no additional coating layer, and the fiber core 110 is in direct contact with air. That is, the optical fiber 100 also includes a cladding layer that covers the surface of the fiber core 110, and the cladding layer is air.
[0026] In some embodiments, the numerical aperture of the optical fiber 100 is 0.26 to 0.32, for example, it can be 0.26, 0.28, 0.29, 0.3, 0.31, 0.32, etc., which is beneficial to the transmission of light by the optical fiber 100 and reduces the difficulty of optical path coupling of the optical fiber 100.
[0027] In some embodiments, the optical loss per unit length of the fiber core 110 is 0.15 dB / cm to 0.19 dB / cm, for example, it can be 0.15 dB / cm, 0.16 dB / cm, 0.17 dB / cm, 0.18 dB / cm, 0.19 dB / cm, etc. Low optical loss is beneficial for maintaining sufficient signal strength after the optical signal is transmitted over a long distance in the fiber core 110, which is beneficial for improving the sensitivity of the gas sensor using the optical fiber 100.
[0028] In some embodiments, the specific surface area of the fiber core 110 is 800 m². 2 / g to 900m 2 / g, for example, can be 800m 2 / g、820m 2 / g、850m 2 / g、880m 2 / g、900m 2 / g, etc. The total pore volume at a single point of the fiber core 110 is 0.7cm. 3 / g to 0.85cm 3 / g, for example, can be 0.7cm 3 / g, 0.72cm 3 / g, 0.75cm 3 / g, 0.78cm 3 / g, 0.8cm 3 / g, 0.82cm 3 / g, 0.85cm 3 / g, etc. The average pore size of the fiber core 110 is 3.5nm to 4nm, for example, it can be 3.5nm, 3.6nm, 3.8nm, 4nm, etc. By controlling the specific surface area, total pore volume at a single point, and average pore size of the fiber core 110 to be within the above ranges, it is beneficial that when the optical fiber 100 is used in a gas sensor, the gas to be measured can quickly enter the interior of the optical fiber 100, providing abundant adsorption sites, achieving sufficient enrichment of the gas molecules to be measured, reducing the response time of the gas sensor, and improving the detection sensitivity of the gas sensor. Specifically, such as Figure 1cAs shown, the optical fiber 100 contains three-dimensional, interconnected nanopores, without any closed or isolated dead pores. Silica nanoparticles interlock to form a continuous solid support framework. When the optical fiber 100 is used in a gas sensor, the gas to be measured can freely diffuse from both ends or sidewalls of the optical fiber 100, thus rapidly penetrating the entire interior area of the optical fiber 100. The gas molecules are uniformly adsorbed onto the surface of the solid support framework formed by the silica nanoparticles of the silica gel material. This solid support framework also constitutes a light transmission carrier. At this time, the light transmission channel and gas adsorption channel of the optical fiber 100 completely overlap. The fiber core 110 undertakes the dual functions of light transmission and gas enrichment. During the propagation of the light signal, there is full contact with the enriched gas molecules, effectively enhancing the enhancement effect of the measured signal (e.g., Raman spectral signal) and improving the detection sensitivity of the gas sensor using the optical fiber 100.
[0029] When traditional aerogels are applied to optical fibers, they are attached to the fiber core surface or localized areas as coatings or fillers. Gases can only contact the surface pores of the aerogel, while the internal pores are blocked by the quartz substrate or cladding and cannot be utilized, resulting in limited effective adsorption sites and low gas enrichment capacity. Furthermore, gas molecules must slowly diffuse to the depths of the aerogel based on a concentration gradient, leading to a long adsorption equilibrium time (typically several minutes), which is insufficient for rapid response detection requirements. The optical fiber 100 provided by this invention has entirely open internal pores, allowing the analyte gas to diffuse simultaneously and bidirectionally from the end face and sidewalls, rapidly penetrating the entire optical fiber 100. This ensures that all internal pores of the optical fiber 100 participate in gas adsorption, increasing the number of effective adsorption sites several times compared to traditional coating-type solutions, and significantly increasing the gas enrichment capacity. Simultaneously, multi-path diffusion greatly shortens the path length for gas molecules to reach the adsorption sites, significantly reducing the adsorption-desorption equilibrium time, which is beneficial for achieving rapid response. Furthermore, the optical fiber 100 is an integrally molded skeleton constructed from continuous silica nanoparticles, without any attached coating. It is resistant to airflow erosion and mechanical vibration, and has good long-term stability. When applied to fiber optic sensors, it adopts dry solid-state physical adsorption, eliminating the need for electrolytes and avoiding problems such as leakage, low-temperature icing, and chemical corrosion. It is suitable for dry, liquid-free industrial gas sensing and detection scenarios.
[0030] In some embodiments, the optical fiber 100 is an integral structure, that is, the optical fiber 100 is integrally formed from the silica gel material.
[0031] In some embodiments, the fiber core 110 is cylindrical, that is, the optical fiber 100 is cylindrical. The diameter of the fiber core 110 is 100 micrometers to 2 millimeters, that is, the diameter of the optical fiber 100 is 100 micrometers to 2 millimeters. For example, it can be 100 micrometers, 200 micrometers, 500 micrometers, 800 micrometers, 1 millimeter, 1.5 millimeters, 1.8 millimeters, 2 millimeters, etc. This helps to reduce problems such as fiber breakage during the manufacturing process due to the fiber core 110 being too small, or low mechanical strength due to the small diameter, making wiring and assembly difficult in practical applications. At the same time, it also helps to avoid problems such as internal pore collapse and decreased light transmittance during the manufacturing process due to the fiber core 110 being too large, thereby affecting the sensing performance of the sensor when the optical fiber 100 is used in a gas sensor. Preferably, the diameter of the fiber core 110 is 400 micrometers to 600 micrometers, and more preferably 500 micrometers. Traditional silica optical fibers rely on the refractive index difference between the core and cladding to achieve total internal reflection transmission of optical signals. The two layers have different coefficients of thermal expansion, and interlayer stress is easily generated when the temperature changes, leading to optical path misalignment and signal fluctuations, which requires high coupling alignment accuracy. In contrast, the optical fiber 100 with the aforementioned diameter has a large effective light transmission cross-sectional area and a wide alignment tolerance range during laser coupling. Optical path alignment can be completed without a high-precision multi-dimensional fine-tuning frame, which significantly reduces the operational difficulty and instrument cost of on-site assembly.
[0032] In some embodiments, the length of the fiber core 110 is 1 cm to 10 cm, that is, the length of the optical fiber 100 is 1 cm to 10 cm. For example, it can be 1 cm, 2 cm, 3 cm, 4 cm, 5 cm, 6 cm, 7 cm, 8 cm, 9 cm, 10 cm, etc. This facilitates the docking and assembly of the optical fiber 100 with the optical path when it is used in a gas sensor, while avoiding cracking problems caused by uneven stress distribution during the manufacturing process due to the excessive length of the fiber core 110.
[0033] Traditional optical fibers using aerogel materials, such as hollow liquid-core optical fibers with a hollow tubular matrix and relying on the liquid inside the tube for light transmission, and aerogel as the tube wall support layer, achieve total internal reflection by utilizing the refractive difference between the liquid core layer and the tube wall. Gas only contacts the tube wall surface and cannot enter the core layer, making them only suitable for liquid phase detection. Compared to these traditional optical fibers using aerogel materials, the optical fiber 100 of this invention uses silica aerogel as the fiber core 110. The silica aerogel as a whole simultaneously performs both light transmission and gas enrichment functions, making it more suitable for gas sensors, such as dry gas Raman sensors, and further improving the sensitivity of gas sensors using the optical fiber 100 of this invention.
[0034] Meanwhile, the optical fiber 100 provided by the present invention integrates optical transmission and gas enrichment functions into the fiber core 110, eliminating the need for an external independent gas chamber. When applied to optical fiber gas sensors, it helps to significantly reduce the size of the optical fiber sensor probe, making it easier to deploy and install in limited spaces such as narrow pipelines and enclosed equipment, thus reducing the difficulty of on-site deployment.
[0035] Secondly, the present invention provides a method for preparing an optical fiber, comprising: S100, silicon source, catalyst, stress modifier, first solvent and water are mixed and then treated to obtain the precursor.
[0036] S200. The precursor is placed in a tubular mold and subjected to gelation treatment to obtain a wet gel fiber core preform.
[0037] S300. The wet gel fiber core preform is subjected to aging treatment to obtain a wet gel fiber core.
[0038] S400. The wet gel fiber core is subjected to supercritical carbon dioxide drying treatment to obtain the optical fiber.
[0039] The silicon source is selected from at least one of tetramethoxysilane and tetraethyl orthosilicate; the catalyst is selected from at least one of ammonia, an aqueous solution of ethylamine, and an aqueous solution of monomethylamine; the stress modifier is selected from at least one of N,N-dimethylformamide and N,N-dimethylacetamide; and the first solvent is selected from at least one of methanol and anhydrous ethanol.
[0040] The mass ratio of the silicon source, the catalyst, the stress modifier, the first solvent, and the water is (31 to 34 parts): (0.21 to 0.3 parts): (1.19 to 1.63 parts): (71.78 to 93.03 parts): (22.02 to 28.17 parts).
[0041] The optical fiber fabrication method provided by this invention involves integrally molding the optical fiber from silica aerogel. By using a silica aerogel core as the light guide body, and utilizing the high specific surface area and suitable refractive index of silica aerogel, the optical transmission and gas enrichment functions are completed in one piece. This avoids the interface loss of light between the silica aerogel and the light guide body, and improves the sensitivity of gas sensors using optical fibers.
[0042] Traditional methods for preparing aerogels involve a combination of sol-gel and atmospheric pressure drying. The resulting aerogels are extremely brittle and prone to shrinkage fracture and pore collapse when forming columnar structures of suitable diameter and length, making it difficult to form long-sized structures. Therefore, when aerogels are used in optical fibers, they are often made into blocks, films, or powders and used only as spectral enhancement substrates or coatings. Compared with traditional methods for preparing aerogels, the optical fiber preparation method provided by this invention involves mixing a silicon source, catalyst, stress modifier, first solvent, and water in a specific ratio to obtain a precursor. The precursor is then gelled in a tubular mold, followed by aging treatment and supercritical carbon dioxide drying to obtain a monolithically formed cylindrical silica aerogel material with suitable length and diameter. This method overcomes the limitations of traditional aerogels, which can only exist in short-sized blocks, thin films, or packaged forms, providing a feasible process path for the large-scale preparation and engineering application of aerogel optical fibers. Simultaneously, this silica aerogel material serves as a light guide, utilizing its high transmittance, porosity, and suitable refractive index to integrate light transmission and gas enrichment functions, avoiding interfacial loss between the silica aerogel and the light guide, and improving the sensitivity of gas sensors using optical fibers.
[0043] Meanwhile, traditional applications of aerogels in fiber optic sensors typically involve attaching the aerogel to the surface or interior of a quartz fiber as a coating, thin film, or filler. The quartz fiber is responsible for optical signal transmission, while the aerogel only performs the single function of gas adsorption. This process is complex, requiring separate fabrication of quartz and aerogel before composite formation. The abrupt change in refractive index at the quartz-aerogel interface causes additional scattering loss, reducing the signal-to-noise ratio of the sensing signal when the fiber is used in the sensor. In contrast to these traditional fabrication processes, the fiber fabrication method provided by this invention utilizes silica aerogel in a one-step molding process to obtain a single-material fiber integrating optical transmission and gas molecule enrichment functions. This eliminates the interfacial optical losses, thermodynamic mismatch problems, and film delamination risks inherent in multilayer composite structures. Furthermore, it eliminates multiple steps such as quartz substrate preparation, coating, and interface sealing, effectively reducing production processes and manufacturing costs.
[0044] In some embodiments, the optical fiber fabrication method is used to fabricate the optical fiber 100 as described above.
[0045] In some embodiments, the weight parts of the silicon source, the catalyst, the stress modifier, the first solvent, and the water are respectively: The silicon source: 31 to 34 parts; the catalyst: 0.21 to 0.3 parts; the stress modifier: 1.19 to 1.63 parts; the first solvent: 71.78 to 93.03 parts; the water: 22.02 to 28.17 parts.
[0046] The catalyst catalyzes the hydrolysis-condensation reaction to generate a three-dimensional silica network framework. By controlling the amount of catalyst, the gelation rate can be appropriately slowed down, which is beneficial for the precursor to be fully and uniformly gelled in the tubular mold. This avoids uneven fiber density caused by premature local gelation and cracking problems in the subsequent supercritical carbon dioxide drying process.
[0047] In the sol-gel system, the stress modifier is uniformly dispersed within the gel during the gelation process. This regulates the solvent evaporation rate and surface tension within the pores during subsequent supercritical carbon dioxide drying, balancing the capillary forces generated during the process. This alleviates the shrinkage and breakage problems caused by stress concentration in the wet gel fiber core during supercritical carbon dioxide drying, making it a key component in forming the optical fiber 100 of suitable length and diameter. Simultaneously, the stress modifier participates in regulating the polycondensation process of the silicon source, refining the pore structure within the aerogel. This facilitates the formation of uniformly sized nanopores, reducing light scattering in the prepared optical fiber 100 and improving its light transmittance.
[0048] The pore size, density, and other properties of the optical fiber 100 are mainly regulated by the silicon source, water, catalyst, stress modifier, and the first solvent. By controlling the mass ratio of the silicon source, catalyst, stress modifier, first solvent, and water to (31 to 34 parts): (0.21 to 0.3 parts): (1.19 to 1.63 parts): (71.78 to 93.03 parts): (22.02 to 28.17 parts), the water content is appropriate, avoiding excessively large pore size and low pore density due to insufficient hydrolysis of the silicon source, and avoiding excessively small pore size and high pore density due to excessive hydrolysis. This promotes sufficient hydrolysis of the silicon source, forming channels with suitable pore size and density. The catalyst regulates the pH value of the precursor, thereby regulating the growth of silica nanoparticles. The catalyst content is appropriate, avoiding excessively low catalyst content. The slow hydrolysis process results in an insufficient number and excessively large size of primary silica nanoparticles, leading to excessively large pore sizes and uneven pore distribution. This also avoids the violent condensation reaction caused by an excessively high proportion of the catalyst, which would otherwise result in rapid agglomeration of the primary silica particles, causing excessively large pore sizes and uneven pore distribution. The stress modifier is used to stabilize the pore structure during the supercritical carbon dioxide drying process. An appropriate proportion of the stress modifier helps prevent pore collapse and reduced pore size due to insufficient proportion and significant capillary shrinkage during supercritical carbon dioxide drying, and also avoids phase separation and uneven pore distribution in the precursor due to an excessively high proportion. The proportion of the silicon source determines the total solid phase of the gel, providing the basic density of the optical fiber 100 and providing a basis for the regulation of the aforementioned components.
[0049] In some embodiments, the silicon source, catalyst, stress modifier, first solvent, and water are mixed at 20°C to 30°C (e.g., 20°C, 25°C, 30°C, etc.), and the pH value of the precursor is 7.5 to 8.5, for example, 7.5, 7.8, 8.0, 8.2, 8.5, etc. The catalyst is an alkaline catalyst. The addition of the catalyst keeps the pH value of the precursor within the above-mentioned mild alkaline range, thereby further regulating the hydrolysis and condensation reaction rate of the silicon source. This is beneficial for the uniform growth of primary silica particles at the nanoscale, constructing a fine and uniform nanoporous structure. At the same time, the precursor being within the above-mentioned mild alkaline range helps to moderately delay the gelation process, ensuring that the precursor gels fully and uniformly within the tubular mold, avoiding uneven fiber density caused by localized premature gelation and cracking problems during subsequent supercritical carbon dioxide drying.
[0050] In some embodiments, the water is selected from at least one of distilled water, deionized water, recycled water, pure water, and ultrapure water.
[0051] In some embodiments, when the catalyst is selected from at least one of ammonia, an aqueous solution of ethylamine, and an aqueous solution of monomethylamine, the ammonia is ammonia with a mass fraction of 24% to 26% (e.g., 24%, 25%, 26%), the aqueous solution of ethylamine is an aqueous solution of ethylamine with a mass fraction of 24% to 26% (e.g., 24%, 25%, 26%), and the aqueous solution of monomethylamine is an aqueous solution of monomethylamine with a mass fraction of 24% to 26% (e.g., 24%, 25%, 26%).
[0052] In some embodiments, step S100 includes: S110. The silicon source, the stress modifier, and the first solvent undergo a first mixing treatment to obtain a first mixture. S120. The first mixture, the catalyst, and the water undergo a second mixing treatment to obtain the precursor.
[0053] In some embodiments, the stress modifier and the first solvent may be mixed first, and then mixed with the silicon source. The first mixing process may be a stirring process to fully disperse the silicon source in the first mixture, which is a transparent solution. The first mixing process may last from 6 minutes to 10 minutes, for example, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, etc., and the first mixing process may last from 20°C to 30°C, for example, 20°C, 25°C, 30°C, etc.
[0054] In some embodiments, the second mixing process can be a stirring process, and the precursor is a transparent solution. The duration of the second mixing process can be from 45 seconds to 60 seconds, for example, 45 seconds, 50 seconds, 55 seconds, 60 seconds, etc., and the temperature of the second mixing process can be from 20°C to 30°C, for example, 20°C, 25°C, 30°C, etc.
[0055] In some embodiments, the inner diameter of the tubular mold is 100 micrometers to 2 millimeters, for example, it can be 100 micrometers, 200 micrometers, 500 micrometers, 800 micrometers, 1 millimeter, 1.5 millimeters, 2 millimeters, etc.; the length of the tubular mold is 1 centimeter to 10 centimeters, for example, it can be 1 centimeter, 2 centimeters, 5 centimeters, 8 centimeters, 10 centimeters, etc., so as to obtain the optical fiber 100 with a suitable diameter and a suitable length.
[0056] In some embodiments, the tubular mold is made of a chemically inert and smooth polymer material. Such materials have low surface energy and extremely weak adhesion to the silica wet gel, preventing the tubular mold from reacting with the precursor while facilitating the detachment of the wet gel fiber core preform from the tubular mold, thereby obtaining a complete wet gel fiber core preform. The material of the tubular mold is selected from at least one of polytetrafluoroethylene, polypropylene, and polyethylene.
[0057] In some embodiments, the precursor is injected into the tubular mold, the tubular mold is sealed, and the gelation process is allowed to complete. By sealing the tubular mold, the gelation process is maintained in a stable liquid phase environment, preventing solvent evaporation and the entry of outside air during the gelation process, which could lead to uneven precursor concentration and premature surface gelation within the tubular mold. This facilitates the uniform molding of the wet gel fiber core preform along the length of the tubular mold and prevents uneven internal pore distribution and localized cracking of the wet gel fiber core preform during the molding process.
[0058] In some embodiments, the tubular mold is a hollow cylinder and a plug can be used to seal at least one end of the tubular mold. The plug is used to seal the end of the tubular mold that is connected to the outside after the precursor is injected into the tubular mold. For example, when one end of the tubular mold is connected to the outside, the plug is placed at that end; when both ends of the tubular mold are connected to the outside, the plug is placed at both ends of the tubular mold.
[0059] In some embodiments, the material of the plug may be the same as that of the tubular mold, for example, it may be selected from at least one of polytetrafluoroethylene, polypropylene and polyethylene; or, the plug may be made of hot melt adhesive material to seal the tubular mold by hot melting; or, the plug may be made of transparent waterproof tape.
[0060] In some embodiments, an elastic sealing ring may be used to assist the plug in sealing the tubular mold.
[0061] In some embodiments, the radial diameter and axial length of the produced optical fiber can be controlled by replacing the tubular mold with different inner diameters and lengths. The entire core fabrication equipment of the optical fiber fabrication method does not require modification or upgrade, and the process is highly flexible. Based on the adjustable design of the tubular mold, optical fibers of different thicknesses and lengths can be flexibly fabricated according to the actual detection space and optical path matching requirements. Fine-gauge optical fibers are suitable for in-situ detection in confined spaces such as narrow sealed cavities and microcapillaries, while large-diameter optical fibers can obtain a larger light-transmitting area, which is beneficial to improving optical path coupling fault tolerance and optical signal output intensity. They are suitable for different application requirements such as laboratory micro-detection and continuous monitoring of industrial pipelines. The optical fiber fabrication method provided by this invention is compatible with the production of optical fibers of various shapes and sizes, and has a wider range of applications.
[0062] In some embodiments, the gelation treatment time is greater than or equal to 10 minutes and less than or equal to 10 hours. For example, it can be 10 minutes, 20 minutes, 30 minutes, 1 hour, 2 hours, 3 hours, 5 hours, 6 hours, 8 hours, 10 hours, etc.
[0063] In some embodiments, the temperature of the gelation treatment is greater than or equal to 20°C and less than or equal to 40°C. For example, it can be 20°C, 25°C, 30°C, 35°C, 40°C, etc.
[0064] The duration of the gelation treatment is determined by the gelation temperature, the mass ratio of each component in the precursor, and the inner diameter of the tubular mold. The gelation time and temperature are controlled within the above ranges, in conjunction with the mass ratio of each component in the precursor, so as to facilitate the integral molding of the wet gel fiber core preform in the tubular mold. Specifically, due to the large aspect ratio of the tubular mold, the precursor needs sufficient time to spread, wet, and expel air bubbles after being injected into the tubular mold. If the gelation time is too short, the precursor will solidify before fully filling the mold, which can easily cause uneven density along the length of the resulting wet gel fiber core preform, resulting in local structural defects. On the other hand, the formed silica aerogel is used as the fiber core of the optical fiber as a light transmission medium, and the uniformity of the internal pore structure is required to be significantly higher than that of block aerogel. By moderately slowing down the gelation process, the wet gel fiber core preform can be integrally formed after an appropriate amount of time. This is beneficial for the siloxane condensation reaction to proceed under quasi-static conditions, allowing the primary silica particles to nucleate slowly and grow uniformly. This results in the construction of a uniform nanoporous framework along the axial direction and cross-section inside the wet gel fiber core preform, avoiding internal stress concentration, effectively preventing the wet gel fiber core preform from bending or breaking during subsequent preparation, and ensuring the light transmission performance of the optical fiber 100.
[0065] In some embodiments, after the gelation process is completed, the plugs at both ends of the tubular mold can be removed, one end of the tubular mold can be fixed, and an axial thrust can be applied from the other end using a push rod that matches the inner diameter of the tubular mold, so that the wet gel fiber core preform slides out smoothly along the axial direction of the tubular mold.
[0066] In some embodiments, the tubular mold may have a detachable structure. After the gelation process is completed, the tube wall of the tubular mold is disassembled and the wet gel fiber core preform is taken out.
[0067] In some embodiments, the demolding process of the wet gel fiber core preform can be carried out at room temperature, with the operation kept stable and continuous, avoiding sudden pulling or impact operations, so that the wet gel fiber core preform slides out smoothly along the axial direction of the tubular mold, preventing the wet gel fiber core preform from bending or breaking.
[0068] In some embodiments, step S300 includes: S310. The wet gel fiber core preform is placed in a second solvent and aged at an aging temperature for a specified time to obtain the wet gel fiber core.
[0069] In some embodiments, the second solvent is selected from solvents that are completely miscible with water, have low surface tension, and are miscible with supercritical carbon dioxide, so as to fully displace the moisture in the wet gel fiber core preform during the aging process and ensure that pore collapse does not occur during the supercritical carbon dioxide drying process. The second solvent is selected from at least one of anhydrous ethanol, isopropanol, and methanol.
[0070] In some embodiments, the aging temperature is 20°C to 30°C, for example, 20°C, 25°C, 30°C, etc.; the aging time is 24 hours to 96 hours, for example, 24 hours, 36 hours, 48 hours, 60 hours, 72 hours, 84 hours, 96 hours, etc. Depending on the second solvent, the aging time can be adjusted accordingly within the above range. For example, compared to anhydrous ethanol, methanol has stronger permeability, a faster replacement rate, higher volatility, and relatively greater toxicity, so the aging time can be appropriately shortened; isopropanol has a higher surface tension than anhydrous ethanol and slower replacement kinetics, so the aging time can be appropriately extended and the replacement frequency of the second solvent increased. Controlling the aging time and aging temperature within the aforementioned ranges helps to strengthen the skeleton toughness of the wet gel fiber core and reduce the probability of breakage during transport and supercritical carbon dioxide drying. Simultaneously, under mild temperature conditions, the moisture inside the pores of the wet gel fiber core is completely removed, leaving only the second solvent. This prevents the high surface tension of residual water from damaging the nanoporous structure during subsequent supercritical carbon dioxide drying, thus preventing problems such as pore collapse and decreased light transmittance in the resulting optical fiber 100.
[0071] In some embodiments, the second solvent is replaced three times or more during the aging process, or the second solvent is replaced every 8 hours during the aging process, in order to promote further cross-linking and densification of the silica gel network, improve the self-skeleton strength of the wet gel fiber core, and the repeated replacement of the second solvent is more conducive to removing unreacted tetramethoxysilane, moisture and reaction byproducts remaining in the gel pores, so that all the medium in the pores of the wet gel fiber core is replaced with the second solvent.
[0072] In some embodiments, step S400 includes: S410. In supercritical carbon dioxide, the wet gel fiber core is dried under drying pressure and temperature for a certain time to obtain the optical fiber 100.
[0073] In some embodiments, supercritical carbon dioxide has better diffusion ability than liquid carbon dioxide and can easily penetrate into the nanoporous structure of the wet gel fiber core, thus facilitating the full removal of the second solvent from the wet gel fiber core.
[0074] In some embodiments, the drying pressure is 8 MPa to 9 MPa, for example, 8 MPa, 8.5 MPa, 9 MPa, etc.; the drying temperature is 35°C to 40°C, for example, 35°C, 36°C, 38°C, 40°C, etc.; the drying time is greater than or equal to 2.5 hours and less than or equal to 6 hours, for example, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 5 hours, 6 hours, etc.
[0075] In some embodiments, the supercritical carbon dioxide drying process is carried out in an autoclave. The pressurization rate to reach the drying pressure is 0.5 MPa / min to 1 MPa / min, for example, it can be 0.5 MPa / min, 0.6 MPa / min, 0.8 MPa / min, 0.9 MPa / min, 1 MPa / min, etc. By controlling the pressurization rate, while taking into account the operating efficiency of the equipment, the process of carbon dioxide entering the nanopores of the wet gel fiber core is made more gradual, avoiding the formation of violent pressure shocks and effectively protecting the integrity of the skeleton of the obtained optical fiber 100. If a higher pressurization rate is used, for example, 2 MPa / min to 3 MPa / min or higher for rapid pressurization, the high-speed carbon dioxide gas flow can easily cause mechanical erosion damage to the surface nanonetwork of the wet gel fiber core; at the same time, the compression heat caused by rapid compression will cause uneven temperature distribution in the autoclave, which is not conducive to the uniform formation of a stable supercritical fluid environment in the autoclave.
[0076] In some embodiments, after the supercritical carbon dioxide drying treatment is completed, the depressurization rate is greater than 0 MPa / h and less than or equal to 0.5 MPa / h, for example, it can be 0.1 MPa / h, 0.2 MPa / h, 0.3 MPa / h, 0.4 MPa / h, 0.5 MPa / h, etc. By controlling the depressurization rate, it is beneficial to balance the internal and external pressures of the nanopores of the optical fiber 100 during the depressurization process, which protects the optical fiber 100 and avoids problems such as breakage of the optical fiber 100 and collapse of the pore structure caused by excessive internal and external pressures of the nanopores and rapid carbon dioxide overflow due to excessive depressurization rate.
[0077] In some embodiments, the specific steps of the supercritical carbon dioxide drying process are as follows: The wet gel fiber core is placed inside an autoclave. Compared with the conventional supercritical carbon dioxide drying process, this process adopts a dynamic circulation supercritical drying method to accelerate the solvent replacement rate inside the pores of the wet gel fiber core. The delivery pump adopts a constant pressure working mode, and the pressure inside the autoclave can be maintained in the range of 8.0 MPa to 9.0 MPa, preferably 8.5 MPa; the heating temperature of the autoclave body is controlled in the range of 35℃ to 40℃, preferably 36℃, so that the carbon dioxide inside the autoclave reaches a supercritical state; the carbon dioxide mixed gas carrying the second solvent is continuously discharged from the exhaust valve, and the total replacement time is not less than 2.5 hours, preferably more than 3 hours, to ensure that the second solvent inside the pores of the wet gel fiber core is completely removed; after the second solvent replacement is completed, the autoclave inlet valve is closed, the exhaust flow rate of the exhaust valve is reduced, and the pressure relief rate is controlled within 0.5 MPa per hour to slowly release the pressure inside the autoclave; after the pressure inside the autoclave drops to atmospheric pressure, the optical fiber 100 is taken out.
[0078] The optical fiber preparation method provided by this invention has good parameter adjustment margin. By adjusting the precursor weight fraction, aging treatment time, and supercritical drying temperature and pressure parameters, the pore structure of the obtained optical fiber can be controlled within a certain range. When the prepared optical fiber is applied to the detection of small molecule inorganic gases such as methane and carbon dioxide, the optical fiber can be controlled to have a smaller pore size to increase the specific surface area and increase the adsorption sites for small molecules; when the prepared optical fiber is applied to the detection of volatile organic macromolecular gases such as benzene and formaldehyde, the optical fiber can be controlled to have a larger pore size structure to reduce gas diffusion resistance and accelerate the adsorption response speed.
[0079] The optical fiber preparation method provided by this invention uses common chemical raw materials as the precursor components, without any highly corrosive, toxic, or other high-risk reagents, resulting in lower safety risks during raw material storage and on-site operations. The supercritical carbon dioxide drying process eliminates the emission of organic solvents, allows for the recycling and reuse of carbon dioxide, minimizes environmental impact, and reduces the investment cost of supporting exhaust gas treatment equipment.
[0080] The optical fiber fabrication method provided by this invention involves treating the wet gel fiber core with supercritical carbon dioxide to form an optical fiber with a complete structure, uniform pores, and light transmission characteristics. Compared with the traditional method of removing residual impurities and improving the density of the nanoparticle skeleton by high-temperature heat treatment of aerogel, the optical fiber fabrication method provided by this invention uses the aging treatment in combination with the supercritical carbon dioxide drying treatment, which more effectively removes residual solvents and other impurities. This method can directly meet the requirements for application in gas sensors (such as dry gas Raman sensors), simplifies the process flow, and shortens the fabrication cycle. At the same time, it avoids problems such as bending and breakage caused by thermal stress concentration in the optical fiber due to high-temperature heat treatment, and also avoids damage to the optical fiber skeleton structure and optical performance caused by pore shrinkage and changes in aperture due to high-temperature treatment.
[0081] In some embodiments, after the supercritical carbon dioxide drying treatment, the resulting optical fiber 100 only needs to have any trace debris removed from its surface. It can then be stored in a sealed container in a constant-temperature drying environment (e.g., a drying cabinet) at 20°C to 25°C and humidity below 20%. This prevents long-term contact with moisture in the air, which could cause the silica aerogel framework to collapse, thus preserving the performance of the optical fiber 100 for a longer period and facilitating its subsequent assembly into a gas sensor. The optical fiber 100 exhibits good storage stability and can be kept in stock for extended periods. It eliminates the need for temporary preparation when replacing equipment in the field, significantly reducing the cost of consumables and the frequency of on-site maintenance in industrial gas monitoring scenarios.
[0082] The technical solution of the present invention will be further described in detail below with reference to specific embodiments.
[0083] Example 1 like Figure 2 As shown, the optical fiber fabrication method provided in this embodiment includes the following steps: like Figure 2 As shown in (a), 1 is a mixture of methanol, DMF, and tetramethoxysilane, and 2 is a mixture of 25wt% ammonia solution and deionized water. (1) Preparation of precursor: by weight, 33 parts of tetramethoxysilane, 82 parts of methanol, 1.4 parts of N,N-dimethylformamide (DMF), 0.26 parts of 25wt% ammonia solution, and 20 parts of deionized water. After premixing methanol and DMF, tetramethoxysilane was added and magnetically stirred for 8 minutes; then 25wt% ammonia solution and deionized water were added dropwise and stirred rapidly for 50 seconds to obtain a transparent hydrolyzed sol, which is the precursor.
[0084] like Figure 2As shown in (b), 11 represents a tubular mold. (2) Gel molding: The prepared precursor solution is injected into a polytetrafluoroethylene tubular mold with an inner diameter of 500 μm. The two ends of the mold are sealed with matching plugs. The gelation reaction is completed after standing at room temperature for 2.5 hours. After demolding, a complete wet gel optical fiber preform is obtained.
[0085] like Figure 2 As shown in (c), 12 represents the second solvent. (3) Aging and replacement: The wet gel fiber preform is completely immersed in anhydrous ethanol and aged at room temperature. The anhydrous ethanol is replaced every 8 hours for a total of five times to completely remove the moisture and unreacted substances from the wet gel fiber preform and obtain the wet gel fiber core.
[0086] like Figure 2 As shown in (d), 13 is a carbon dioxide cylinder that provides carbon dioxide gas source, 14 is a booster pump, 15 is a carbon dioxide inlet control valve, 16 is a thermometer, 17 is a pressure gauge for the autoclave, and 18 is a pressure relief control valve. (4) Supercritical drying: The wet gel fiber core is placed in the autoclave, and carbon dioxide is introduced. The pressure is increased to 8.5 MPa at a rate of 0.75 MPa / min, and the temperature is increased to 36°C at the same time, so that the carbon dioxide reaches the supercritical state. The constant pressure and temperature replacement is maintained for 3 hours using a dynamic circulation mode. Fresh supercritical carbon dioxide is continuously introduced throughout the process, and the mixed gas carrying anhydrous ethanol is continuously discharged. After the replacement is completed, the inlet valve is closed, and the pressure is slowly released to atmospheric pressure at a rate of 0.5 MPa / h. The optical fiber is then removed.
[0087] Example 2 This embodiment is similar to Embodiment 1, except that: in the precursor of step (1), by weight parts: 31 parts of tetramethoxysilane, 71.78 parts of methanol, 1.19 parts of N,N-dimethylformamide (DMF), 0.21 parts of 25wt% ammonia solution, and 22.02 parts of deionized water.
[0088] Example 3 This embodiment is similar to Embodiment 1, except that: in the precursor of step (1), by weight parts: 33 parts of tetramethoxysilane, 93.03 parts of methanol, 1.63 parts of N,N-dimethylformamide (DMF), 0.3 parts of 25wt% ammonia solution, and 28.17 parts of deionized water.
[0089] Example 4 The optical fiber fabrication method provided in this embodiment includes the following steps: (1) Preparation of precursor: By weight, 33 parts of tetraethyl orthosilicate, 82 parts of anhydrous ethanol, 1.4 parts of N,N-dimethylacetamide, 0.26 parts of 24wt% ethylamine aqueous solution, and 20 parts of deionized water. After premixing anhydrous ethanol and N,N-dimethylacetamide, add tetraethyl orthosilicate and stir magnetically for 6 minutes; then add 24wt% ethylamine aqueous solution and deionized water dropwise and stir rapidly for 45 seconds to obtain a transparent hydrolyzed sol, which is the precursor.
[0090] (2) Gel molding: The prepared precursor solution is injected into a polytetrafluoroethylene tubular mold with an inner diameter of 100 μm. The two ends of the mold are sealed with matching plugs. The gelation reaction is completed after standing at 20°C for 10 minutes. After demolding, a complete wet gel optical fiber preform is obtained.
[0091] (3) Aging and replacement: The wet gel fiber preform is completely immersed in methanol and aged at 20°C. The methanol is replaced every 6 hours for a total of 4 times to completely remove the moisture and unreacted substances from the wet gel fiber preform and obtain the wet gel fiber core.
[0092] (4) Supercritical drying: The wet gel fiber core is placed in an autoclave, and carbon dioxide is introduced. The pressure is increased to 8 MPa at a rate of 0.5 MPa / min, while the temperature is increased to 35°C to bring the carbon dioxide to a supercritical state. A dynamic circulation mode is used to maintain constant pressure and temperature for 2.5 hours of replacement. Fresh supercritical carbon dioxide is continuously introduced throughout the process, while a mixed gas carrying methanol is continuously discharged. After replacement, the inlet valve is closed, and the pressure is slowly released to atmospheric pressure at a rate of 0.25 MPa / h. The finished optical fiber is then removed.
[0093] Example 5 The optical fiber fabrication method provided in this embodiment includes the following steps: (1) Preparation of precursor: by weight, 33 parts of tetramethoxysilane, 82 parts of methanol, 1.4 parts of N,N-dimethylformamide, 0.26 parts of 26wt% monomethylamine aqueous solution, and 20 parts of deionized water. After premixing methanol and N,N-dimethylformamide, tetramethoxysilane was added and the mixture was magnetically stirred for 10 minutes; then 26wt% monomethylamine aqueous solution and deionized water were added dropwise and the mixture was stirred rapidly for 60 seconds to obtain a transparent hydrolyzed sol, which is the precursor.
[0094] (2) Gel molding: The prepared precursor solution is injected into a polytetrafluoroethylene tubular mold with an inner diameter of 2 mm. The two ends of the mold are sealed with matching plugs. The gelation reaction is completed after standing at 30°C for 10 hours. After demolding, a complete wet gel optical fiber preform is obtained.
[0095] (3) Aging and replacement: The wet gel fiber preform is completely immersed in isopropanol and aged at 30°C. The isopropanol is replaced every 8 hours for a total of 12 times to completely remove the moisture and unreacted substances from the wet gel fiber preform and obtain the wet gel fiber core.
[0096] (4) Supercritical drying: The wet gel fiber core is placed in an autoclave, and carbon dioxide is introduced to increase the pressure to 9 MPa at a rate of 1 MPa / min, while the temperature is increased to 40°C to bring the carbon dioxide to a supercritical state. A dynamic circulation mode is used to maintain constant pressure and temperature for 6 hours of replacement, with fresh supercritical carbon dioxide continuously introduced and a mixed gas carrying methanol continuously discharged throughout the process. After replacement, the inlet valve is closed, and the pressure is slowly released to atmospheric pressure at a rate of 0.4 MPa / h, and the finished optical fiber is taken out.
[0097] Comparative Example 1 The optical fiber fabrication method provided in this comparative example includes the following steps: (1) Preparation of precursor: by weight, 29 parts of tetramethoxysilane, 70 parts of methanol, 1.0 part of N,N-dimethylformamide (DMF), 0.18 parts of 22wt% ammonia solution, and 20 parts of deionized water. After premixing methanol and DMF, add tetramethoxysilane and stir magnetically for 5 minutes; then add 22wt% ammonia solution and deionized water dropwise and stir rapidly for 40 seconds to obtain a transparent hydrolyzed sol, which is the precursor.
[0098] (2) Gel molding: The prepared precursor solution is injected into a polytetrafluoroethylene tubular mold with an inner diameter of 60 μm. The two ends of the mold are sealed with matching plugs. The gelation reaction is completed after standing at 20°C for 1.5 hours. After demolding, a complete wet gel optical fiber preform is obtained.
[0099] (3) Aging and replacement: The wet gel fiber preform is completely immersed in anhydrous acetone and aged at 15°C. The anhydrous acetone is replaced every 8 hours for a total of five times to remove moisture and unreacted substances from the wet gel fiber preform and obtain the wet gel fiber core.
[0100] (4) Supercritical drying: The wet gel fiber core was placed in an autoclave, and carbon dioxide was introduced. The pressure was increased to 9 MPa at a rate of 0.4 MPa / min, while the temperature was increased to 31°C to bring the carbon dioxide to a supercritical state. A dynamic circulation mode was used to maintain constant pressure and temperature for 2 hours of replacement. Fresh supercritical carbon dioxide was continuously introduced throughout the process, and a mixed gas carrying anhydrous acetone was continuously discharged. After replacement, the inlet valve was closed, and the pressure was slowly released to atmospheric pressure at a rate of 0.5 MPa / h. The optical fiber was then removed.
[0101] Comparative Example 2 The optical fiber fabrication method provided in this comparative example includes the following steps: (1) Preparation of precursor: by weight, 38 parts of tetramethoxysilane, 95 parts of methanol, 1.8 parts of N,N-dimethylformamide (DMF), 0.4 parts of 30wt% ammonia solution, and 30 parts of deionized water. After premixing methanol and DMF, add tetramethoxysilane and stir magnetically for 12 minutes; then add 30wt% ammonia solution dropwise and stir rapidly for 80 seconds to obtain a transparent hydrolyzed sol, which is the precursor.
[0102] (2) Gel molding: The prepared precursor solution is injected into a polytetrafluoroethylene tubular mold with an inner diameter of 3 mm. The two ends of the mold are sealed with matching plugs. The gelation reaction is completed after standing at 35°C for 12 hours. After demolding, a complete wet gel optical fiber preform is obtained.
[0103] (3) Aging and replacement: The wet gel fiber preform is completely immersed in anhydrous formamide and aged at room temperature. The anhydrous formamide is replaced every 8 hours for a total of five times to completely remove the moisture and unreacted substances from the wet gel fiber preform and obtain the wet gel fiber core.
[0104] (4) Supercritical drying: The wet gel fiber core was placed in an autoclave, and carbon dioxide was introduced. The pressure was increased to 7.4 MPa at a rate of 1.5 MPa / min, while the temperature was increased to 45°C to bring the carbon dioxide to a supercritical state. A dynamic circulation mode was used to maintain constant pressure and temperature for 8 hours of replacement, with fresh supercritical carbon dioxide continuously introduced and a mixed gas carrying anhydrous formamide continuously discharged throughout the process. After replacement, the inlet valve was closed, and the pressure was slowly released to atmospheric pressure at a rate of 0.5 MPa / h. The optical fiber was then removed.
[0105] Comparative Example 3 This comparative example is similar to Example 1, except that step (4) uses high-temperature heat treatment instead of supercritical carbon dioxide drying to obtain optical fiber. The temperature of the high-temperature heat treatment is 180°C, and the time of the high-temperature heat treatment is 3 hours.
[0106] The optical fibers obtained in the above embodiments and comparative examples were subjected to performance tests. Among them, the natural fracture surface and the whole sample were observed by field emission scanning electron microscopy after gold sputtering treatment. The results are shown in Table 1.
[0107] Specific surface area, total pore volume at a single point, and average pore size were obtained using the nitrogen adsorption-desorption (BET) method, and the results are shown in Table 2. The BET method testing procedure was as follows: Equal amounts of optical fiber samples were taken and pretreated under vacuum at 120℃ for 6 hours to remove adsorbed water vapor and impurities from the sample pores. A 77K nitrogen adsorption-desorption analyzer was used to quantitatively test the pore structure. Specific surface area was calculated based on the BET model, and pore size distribution and average pore size were calculated using the BJH model. The results are shown in Table 2.
[0108] The light loss per unit length and the visible light transmittance were obtained by using a simplified visible light optical path test, and the results are shown in Table 2.
[0109] The refractive index of the optical fiber was obtained using the laser beam deflection method. The specific process is as follows: A 532nm laser beam was perpendicularly incident on the aerogel sample. After passing through the sample, the beam was deflected, forming a deflected spot on the receiving screen. The original spot position without the sample and the deflected spot position after the sample was placed were recorded. The spot deflection distance d and the distance L from the sample to the receiving screen were measured. Combined with the sample thickness, the equivalent refractive index n of the sample was calculated based on Snell's law of refraction and the geometric relationship of the optical path.
[0110] Since the optical fibers obtained in the embodiments and comparative examples have no solid cladding layer, and the outer medium is air, the refractive index of air is n. air =1.00, substituting the air refractive index and the refractive index of the optical fiber obtained by the laser beam deflection method into the following formula:
[0111] The numerical aperture NA can then be obtained, and the results are shown in Table 2.
[0112] Table 1. SEM test results of the optical fibers in the examples and comparative examples.
[0113] Depend on Figures 3a to 3d As shown in Table 1, the optical fiber obtained in this embodiment of the invention, when observed with field emission scanning electron microscopy (SEM) on its natural fracture surface, exhibits no through-cracks, a continuous and interconnected three-dimensional nanoporous network, uniformly dispersed nanoparticles, and no large-area collapse of pores. Among these, [the following information is missing from the original text]. Figure 3a As can be seen, the optical fiber obtained in Embodiment 1 of the present invention has a regular circular cross-section, is a one-piece homogeneous solid structure, without delamination or coating, has continuous and complete fiber formation, and has no large axial through-cracks. Only a few slight mechanical tearing traces caused by breaking and sampling are present at the edge of the cross-section. Figure 3b It can be seen that the natural fracture surface of the optical fiber obtained in Example 1 of the present invention is generally uniform and flat, without large areas of dense solid regions or pore collapse defects, with only a small amount of scattered detached nanoparticles, and no deep penetrating microcracks. Figure 3c As can be seen, the optical fiber obtained in Example 1 of this invention is composed of interconnected silica nanoparticles forming a large-scale, continuous, interwoven network of channels, without large-area isolated closed-pore regions. Figure 3dAs can be seen, the silica nanoparticles in the optical fiber obtained in Example 1 of this invention are uniform in size, and a large number of 3-5 nanometer mesopores are formed between the silica nanoparticles. Only a small amount of silica nanoparticles are slightly aggregated locally, without blocking the channel connectivity. The above SEM test results intuitively prove that the optical fiber preparation method provided by this invention effectively avoids problems such as pore shrinkage and collapse. The prepared optical fiber has a complete, crack-free, and fully interconnected three-dimensional nanoporous framework. Comparative Example 1 uses anhydrous acetone as the solvent for aging treatment. Due to the high volatility of anhydrous acetone, the prepared optical fiber shows obvious cracks in many places, and local pore collapse and obvious nanoparticle aggregation occur, resulting in poor continuity of the porous network inside the optical fiber. Comparative Example 2 uses anhydrous formamide as the solvent for aging treatment. The intermolecular hydrogen bonding of anhydrous formamide is too strong, which easily generates uneven stress distribution during the aging treatment, resulting in uneven shrinkage of the pores inside the prepared optical fiber and the generation of local slight cracks.
[0114] Table 2 shows the BET and optical performance test results of the optical fibers in the examples and comparative examples.
[0115] Depend on Figures 4 to 5 As shown in Table 2, the optical fiber provided by this invention has a high specific surface area, a high total single-point aperture volume, and a suitable average aperture. It also possesses a suitable refractive index and low optical loss. It can stably achieve total internal reflection light guiding by relying on the refractive index difference between the optical fiber and air, while simultaneously achieving global gas diffusion sensing through the interconnected pores within the silica gel. Among these, [the following information is missing from the original text]. Figure 4 It can be seen that the nitrogen adsorption-desorption isotherm of the optical fiber provided in Example 1 of this invention exhibits a typical type IV isotherm, with a clear H1 hysteresis loop in the medium-high pressure range. This proves that the internal structure of the optical fiber in Example 1 is mainly composed of interconnected mesopores, without a large number of closed dead pores, which perfectly matches the morphology of the three-dimensional interconnected nanoporous network observed by scanning electron microscopy. Figure 5The average aperture of the optical fiber obtained in Example 1 was consistent with its SEM observation results. The optical fiber fabrication method provided by this invention produces an optical fiber with a high specific surface area and suitable mesopore size, providing sufficient adsorption sites for gas while ensuring rapid gas diffusion within the pores. This indicates that the optical fiber fabrication method provided by this invention can completely preserve the porous framework inside the optical fiber, avoiding large-area pore collapse and channel blockage. As shown in Table 2, Examples 1 to 5 and Comparative Examples 1 to 2, by controlling the mass ratio of silicon source, catalyst, stress modifier, first solvent, and water to (31 to 34 parts): (0.21 to 0.3 parts): (1.19 to 1.63 parts): (71.78 to 93.03 parts): (22.02 to 28.17 parts), it is more advantageous to obtain an optical fiber with a higher specific surface area, higher total pore volume at a single point, a more suitable average aperture, a more suitable refractive index, and lower optical loss.
[0116] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. An optical fiber, characterized in that, include: The fiber core is made of silica aerogel. The specific surface area of the fiber core is 800 m². 2 / g to 900m 2 / g, wherein the refractive index of the fiber core is 1.03 to 1.
05.
2. The optical fiber as described in claim 1, characterized in that, The optical fiber further includes a cladding layer, which covers the surface of the fiber core, and the cladding layer is air; The optical fiber has a numerical aperture of 0.26 to 0.32 and a fiber core optical loss per unit length of 0.15 dB / cm to 0.19 dB / cm.
3. The optical fiber as described in any one of claims 1 or 2, characterized in that, The total pore volume at a single point in the fiber core is 0.7 cm. 3 / g to 0.85cm 3 / g, the average pore size of the fiber core is 3.5nm to 4nm.
4. A method for fabricating an optical fiber, characterized in that, include: A silicon source, catalyst, stress modifier, first solvent, and water are mixed and then treated to obtain a precursor. The precursor is gelled in a tubular mold to obtain a wet gel fiber core preform. The wet gel fiber core preform is subjected to aging treatment to obtain a wet gel fiber core; The wet gel fiber core is subjected to supercritical carbon dioxide drying to obtain the optical fiber; Wherein, the silicon source is selected from at least one of tetramethoxysilane and tetraethyl orthosilicate, the catalyst is selected from at least one of ammonia, an aqueous solution of ethylamine and an aqueous solution of monomethylamine, the stress modifier is selected from at least one of N,N-dimethylformamide and N,N-dimethylacetamide, and the first solvent is selected from at least one of methanol and anhydrous ethanol. The mass ratio of the silicon source, the catalyst, the stress modifier, the first solvent, and the water is (31 to 34 parts): (0.21 to 0.3 parts): (1.19 to 1.63 parts): (71.78 to 93.03 parts): (22.02 to 28.17 parts).
5. The method for preparing optical fiber as described in claim 4, characterized in that, The gelation treatment time is greater than or equal to 10 minutes, and the gelation treatment time is less than or equal to 10 hours; The gelation treatment temperature is greater than or equal to 20°C, and the gelation treatment temperature is less than or equal to 40°C.
6. The method for preparing an optical fiber as described in any one of claims 4 or 5, characterized in that, The inner diameter of the tubular mold is 100 micrometers to 2 millimeters, and the length of the tubular mold is 1 centimeter to 10 centimeters; The tubular mold is made of at least one of polytetrafluoroethylene, polypropylene, and polyethylene.
7. The method for preparing optical fiber as described in claim 4, characterized in that, The steps for obtaining the wet gel fiber core by aging the wet gel fiber core preform include: The wet gel fiber core preform is obtained by aging in a second solvent at an aging temperature and for an aging time. The second solvent is selected from at least one of anhydrous ethanol, isopropanol and methanol, the aging temperature is 20°C to 30°C, and the aging time is 24 hours to 96 hours.
8. The method for preparing optical fiber as described in claim 7, characterized in that, In the aging process, the second solvent is replaced three times or more.
9. The method for preparing optical fiber as described in claim 4, characterized in that, The step of obtaining the optical fiber by subjecting the wet gel fiber core to supercritical carbon dioxide drying includes: The wet gel fiber core is dried under supercritical carbon dioxide for a specified time under drying pressure and temperature to obtain the optical fiber. The drying pressure is 8 MPa to 9 MPa, the drying temperature is 35°C to 40°C, and the drying time is greater than or equal to 2.5 hours and less than or equal to 6 hours.
10. The method for fabricating optical fiber as described in claim 9, characterized in that, The rate of pressure increase to achieve the drying pressure is from 0.5 MPa / min to 1 MPa / min; After the supercritical carbon dioxide drying process is completed, the pressure relief rate is greater than 0 MPa / h and less than or equal to 0.5 MPa / h.