A silica carrier and its preparation method

By using a specific ratio of fumed silica, silica gel aqueous solution, and ethanol for spray drying and calcination, the problem of balancing the mechanical strength and specific surface area of ​​silica carriers was solved, and a potassium-based low-temperature solid adsorbent material was prepared, achieving efficient CO2 capture and stability, suitable for industrial production.

CN123105668APending Publication Date: 2026-11-17HUANENG CHONGQING LUOWEN POWER CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611368823.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-04
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing silica carriers have low mechanical strength and are prone to pore collapse, which makes it easy for gaseous silica to be blown away and difficult to achieve the desired specific surface area, thus affecting the ease of operation and adsorption performance of potassium-based adsorbents.

Method used

A silica carrier was prepared by mixing fumed silica, silica gel aqueous solution and ethanol in a specific ratio, and then by spray drying and calcination. Silica gel was used as a binder to enhance mechanical strength, and ethanol was used as a dispersion medium to protect the pore structure. Combined with reasonable calcination temperature and time, the stability and specific surface area of ​​the carrier were ensured.

Benefits of technology

A silica support with high mechanical strength, high specific surface area and stable pore structure was prepared for the preparation of potassium-based low-temperature solid adsorbent materials, which improved CO2 capture performance and ease of operation, making it suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
Patent Text Reader

Abstract

This invention discloses a silica support and its preparation method. The method introduces an aqueous silica gel solution as a binder. During calcination, the silica gel forms an inorganic network that tightly bonds nano-sized fumed silica particles, significantly improving the mechanical strength of the support and overcoming the problem of fumed silica easily "blowing away" and causing operational inconvenience. Simultaneously, ethanol is used instead of traditional water solvent as the dispersion medium. During spray drying, ethanol's high volatility and low surface tension allow for gentle and rapid removal, greatly reducing the capillary force of solvent evaporation and its damaging effect on the pores. Combined with a controllable calcination process, the silica gel is fully converted into a stable silica framework, further improving the structural stability of the support and avoiding defects such as pore collapse and a sharp drop in specific surface area caused by excessive sintering. This invention relies on the synergistic effect of "silica gel reinforcement, ethanol pore protection, and calcination shaping" to obtain a silica support with high mechanical strength, high specific surface area, and a stable pore structure, providing a reliable foundation for the preparation of high-performance adsorbents.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of carbon dioxide capture technology and relates to a silica carrier and its preparation method. Background Technology

[0002] With the increasing severity of the global greenhouse effect, carbon dioxide (CO2) capture, utilization, and storage (CCUS) technology has become a key means of mitigating climate change. Among the many technical approaches, solid-state adsorption has become a research hotspot in the field of low-temperature CO2 capture due to its significant advantages such as low energy consumption, non-corrosiveness, and recyclability. Silica, due to its large specific surface area, tunable pore size, and good chemical stability, is often used as a carrier for potassium-based adsorbents. In particular, fumed silica, with its nanoscale particle characteristics, possesses an extremely high geometric specific surface area, providing ample loading sites for potassium-based active components, thereby significantly improving adsorption performance.

[0003] However, fumed silica as a carrier has significant drawbacks. Its fine particles and low mechanical strength make it prone to "blowing away" during subsequent impregnation, sieving, and filling operations, leading to operational inconvenience and material loss. Furthermore, when using fumed silica alone, its microporous structure exhibits poor stability, easily collapsing during drying and calcination. This not only affects the dispersibility of the active components but also weakens the cyclic stability of the adsorbent.

[0004] To address these issues, existing technologies often employ methods such as adding binders or high-temperature sintering to enhance mechanical strength. However, this frequently leads to a significant decrease in the specific surface area of ​​the support, sacrificing core adsorption performance. Furthermore, traditional processes often use water as a solvent; the stress generated during water evaporation can damage the pore structure of the support, resulting in reduced pore volume and specific surface area. Therefore, existing potassium-based adsorbent supports generally suffer from a trade-off between specific surface area and mechanical strength, severely limiting their industrial application. Developing a silica support that retains the advantages of a large specific surface area of ​​fumed silica while possessing good mechanical strength and pore structure stability, and offering ease of operation, has become a pressing technical challenge. Summary of the Invention

[0005] To address the problems existing in the prior art, the present invention provides a silica support and its preparation method, thereby solving the technical problem that the prior art is unable to effectively maintain its high specific surface area and stable pore structure while improving the mechanical strength of the fumed silica support, resulting in a trade-off between adsorption performance and operational stability.

[0006] This invention is achieved through the following technical solution: A method for preparing a silica support includes the following steps: Fumed silica, silica gel aqueous solution and ethanol are mixed and stirred to obtain a mixed slurry; The mixed slurry was spray-dried to obtain precursor powder; The precursor powder was calcined to obtain a silica carrier.

[0007] Optionally, the mass ratio of the fumed silica, silica gel aqueous solution, and ethanol is 10:0.5:89.5.

[0008] Optionally, the fumed silica has a particle size of 10-50 nm and a specific surface area of ​​200-400 m². 2 / g; the SiO2 content in the silica gel aqueous solution is 28%~32%.

[0009] Optionally, the inlet air temperature of the spray dryer is 200~300℃, and the outlet air temperature is 80~120℃.

[0010] Optionally, in step 3, the calcination is carried out in an air atmosphere at a temperature of 600°C for a constant temperature calcination time of 5-6 hours.

[0011] A silica support is prepared by the method described above.

[0012] A method for preparing a potassium-based low-temperature solid adsorbent material, which is obtained by using the aforementioned silica support, includes the following steps: The silica carrier was added to a potassium carbonate aqueous solution for impregnation treatment; The impregnated mixture is dried to obtain a solid powder; The solid powder is sieved to obtain the potassium-based low-temperature solid adsorbent material.

[0013] Optionally, the mass concentration of the potassium carbonate aqueous solution is 10%~20%; the solid-liquid mass ratio of the silica carrier to the potassium carbonate aqueous solution is 1:(1~2).

[0014] Optionally, the impregnated mixture is dried to obtain a solid powder, wherein the drying temperature is 80~100℃ and the drying time is 12~24 hours; The solid powder is sieved to obtain a potassium-based low-temperature solid adsorbent material, wherein the sieve used for sieving is 80-100 mesh.

[0015] A potassium-based low-temperature solid adsorbent material is prepared by the method described above.

[0016] Compared with the prior art, the present invention has the following beneficial technical effects: This invention discloses a method for preparing a silica carrier. This method effectively solves the technical challenge of simultaneously achieving optimal mechanical strength, specific surface area, and pore structure in existing technologies by synergistically utilizing a specific raw material system and key process steps. Specifically, the method first introduces a silica aqueous solution as a binder into the raw materials. During subsequent calcination, the silica forms a robust inorganic network structure, tightly binding the nanoscale fumed silica particles, thereby significantly improving the macroscopic mechanical strength of the final carrier and fundamentally overcoming the defects of fumed silica powder being easily "blown away" and inconvenient to handle. Secondly, this method uses ethanol as a dispersion medium instead of the traditional water solvent. In the subsequent spray drying step, ethanol, with its low surface tension and high volatility, can be quickly and gently removed from the slurry, greatly reducing the damage to the fragile pore structure between nanoparticles caused by capillary forces generated by solvent evaporation, thus maximizing the preservation of the inherent high specific surface area and abundant pore volume of fumed silica. Finally, through a controlled calcination process, not only is the silica binder fully transformed into a stable silica framework, further enhancing the overall structural stability of the carrier, but the pore collapse and sharp decrease in specific surface area caused by excessively high temperature or prolonged calcination are also avoided. In summary, this invention, through the synergistic effect of "silica reinforcement, ethanol pore protection, and calcination shaping," successfully prepares a silica carrier possessing high mechanical strength, high specific surface area, and a stable pore structure, laying a solid foundation for the preparation of high-performance adsorbents.

[0017] Furthermore, the mass ratio of fumed silica, silica gel aqueous solution, and ethanol is 10:0.5:89.5. Under this ratio, a small amount of silica gel aqueous solution can fully exert its binding effect to improve the mechanical strength of the carrier, without causing pore blockage or significant reduction in specific surface area due to excessive addition of binder. The high proportion of ethanol can fully disperse the fumed silica particles, reduce the viscosity of the system, and the solvent evaporates quickly during the spray drying process, reducing the damage to the pore structure caused by drying stress. This avoids the loss of fumed silica powder by blowing it away, and ensures that the carrier retains a high specific surface area and pore volume, providing sufficient sites for loading active components.

[0018] Furthermore, the fumed silica has a particle size of 10-50 nm and a specific surface area of ​​200-400 m². 2 / g; The SiO2 content in the silica aqueous solution is 28%~32%. The specific particle size and high specific surface area of ​​fumed silica can provide abundant original pore structure and loading sites. The silica aqueous solution has suitable bonding activity within this SiO2 content range. It can effectively bond between particles to improve the overall strength of the carrier, and will not overfill the pores due to excessive silica sol solid content. It can synergistically take into account the high specific surface area, pore unobstructedness and mechanical strength of the carrier, and lay the carrier foundation for the subsequent preparation of high-performance potassium-based adsorbent materials.

[0019] Furthermore, the inlet air temperature of the spray dryer is 200~300℃, and the outlet air temperature is 80~120℃. The inlet air temperature ensures that the ethanol solvent can evaporate quickly, avoiding the slow evaporation of solvent inside the slurry droplets, which would cause particle agglomeration and pore blockage. The outlet air temperature is controlled within a reasonable range, which can not only remove the solvent to obtain the dried precursor powder, but also prevent the excessive temperature from causing excessive sintering on the precursor surface and premature collapse of the pore structure. This ensures that the precursor powder maintains a loose and porous microstructure, which is beneficial for obtaining a silica carrier with a stable pore structure after subsequent calcination.

[0020] Furthermore, in step 3, calcination is carried out in an air atmosphere at a temperature of 600°C for 5-6 hours. The air atmosphere can effectively remove residual organic components such as ethanol from the precursor. The calcination temperature of 600°C combined with 5-6 hours of constant temperature allows the silica component to fully crosslink and solidify, significantly improving the compressive strength and structural stability of the silica carrier. At the same time, it avoids the problems of particle sintering and a sharp decrease in specific surface area caused by excessively high calcination temperatures. Sufficient constant temperature time ensures uniform carrier structural performance and avoids insufficient carrier strength and pore structure damage during cycling due to insufficient calcination.

[0021] Meanwhile, this invention also discloses a method for preparing potassium-based low-temperature solid adsorbent materials, which are prepared using the aforementioned silica support. Utilizing the stable pore structure and abundant loading sites of the silica support, the impregnation process allows the active component of potassium carbonate to enter the pores and surface of the support. After drying to remove moisture from the system and sieving to remove agglomerated particles, a uniformly sized adsorbent material is obtained. This process is simple and controllable, fully leveraging the performance advantages of the support to prepare a solid adsorbent material suitable for low-temperature CO2 capture, and is suitable for industrial-scale preparation.

[0022] Furthermore, the mass concentration of the potassium carbonate aqueous solution is 10%~20%; the solid-liquid mass ratio of the silica support to the potassium carbonate aqueous solution is 1:(1~2). This concentration range of the potassium carbonate aqueous solution can ensure sufficient loading of active components to achieve a high CO2 adsorption capacity, while preventing potassium carbonate from agglomerating and clogging pores on the support surface due to excessive concentration. Controlling the solid-liquid ratio within this range can ensure that the support is fully wetted during the impregnation process, achieving uniform dispersion of active components, while avoiding the problems of increased energy consumption and loss of active components in subsequent drying due to excessive liquid, thus balancing adsorption performance and the economic efficiency of the preparation process.

[0023] Furthermore, the impregnated mixture is dried to obtain a solid powder, wherein the drying temperature is 80~100℃ and the drying time is 12~24 hours; the solid powder is then sieved to obtain a potassium-based low-temperature solid adsorbent material, wherein the sieve used for sieving is 80~100 mesh. This drying condition can slowly and fully remove the internal moisture of the impregnated material, avoiding local agglomeration of active components and damage to the carrier pore structure by water vapor stress caused by excessively high drying temperature or speed; after sieving through an 80-100 mesh sieve, large agglomerates are removed, resulting in adsorbent material particles with uniform particle size, improving the fluidity of the adsorbent material filling, reducing bed pressure drop, and making it more suitable for the filling and use requirements of industrial adsorption devices. Attached Figure Description

[0024] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0025] Figure 1 The N2 adsorption curve of the silica support in Example 1; Figure 2 This is the breakthrough curve of the adsorbent in Example 2. Detailed Implementation

[0026] To enable those skilled in the art to understand the features and effects of the present invention, the terms and expressions used in the specification and claims are explained and defined in general below. Unless otherwise specified, all technical and scientific terms used herein have the ordinary meaning understood by those skilled in the art regarding the present invention, and in case of conflict, the definitions in this specification shall prevail.

[0027] The theories or mechanisms described and disclosed herein, whether right or wrong, should not in any way limit the scope of the invention, that is, the contents of the invention can be implemented without being limited by any particular theory or mechanism.

[0028] In this document, all features defined by numerical ranges or percentage ranges, such as numerical values, quantities, contents, and concentrations, are for the sake of brevity and convenience only. Accordingly, descriptions of numerical ranges or percentage ranges should be considered as covering and specifically disclosing all possible sub-ranges and individual numerical values ​​(including integers and fractions) within those ranges.

[0029] In this article, unless otherwise specified, “contains,” “includes,” “containing,” “has,” or similar terms cover the meanings of “composed of” and “mainly composed of,” for example, “A contains a” covers the meanings of “A contains a and others” and “A contains only a.”

[0030] For the sake of brevity, not all possible combinations of the technical features in each implementation scheme or embodiment are described herein. Therefore, as long as there is no contradiction in the combination of these technical features, the technical features in each implementation scheme or embodiment can be combined arbitrarily, and all possible combinations should be considered within the scope of this specification.

[0031] The purpose of this invention is to overcome the shortcomings of existing technologies, such as low mechanical strength of silica carriers, easy collapse of pores, easy blowing away of fumed silica, and poor carbon capture effect of potassium-based adsorbents. This invention provides a silica carrier with a simple preparation process and controllable cost, as well as its preparation method. At the same time, it provides potassium-based low-temperature solid adsorbent materials based on this carrier, achieving a balance between specific surface area and mechanical strength, and improving carbon capture performance and ease of operation.

[0032] Specifically, a method for preparing a silica support includes the following steps: Step 1: Take fumed silica, silica gel (30% aqueous solution), and ethanol in a mass ratio of 10:0.5:89.5, and set aside; wherein the fumed silica is nano-sized fumed silica with a particle size of 10~50nm and a specific surface area of ​​200~400m². 2 / g; the silica gel (30% aqueous solution) is industrial grade silica sol with a SiO2 content of 28%~32%; the ethanol is industrial grade anhydrous ethanol with a purity ≥99.5%.

[0033] Step 2: Add the fumed silica, silica gel (30% aqueous solution) and ethanol from Step 1 to a mixing container, and stir at 200-300 r / min for 30-60 min at room temperature (20-25℃) until the mixture is homogeneous and free of obvious precipitation and agglomeration, thus obtaining a mixed slurry.

[0034] Step 3: The mixed slurry obtained in Step 2 is fed into a spray dryer for spray drying. The spray drying parameters are controlled as follows: inlet air temperature 200~300℃, outlet air temperature 80~120℃, feed rate 5~10mL / min, and atomization pressure 0.2~0.4MPa, to obtain the dried precursor powder. During the spray drying process, ethanol evaporates rapidly, which can effectively avoid the stress damage caused by the evaporation of traditional water solvents and initially preserve the pore structure.

[0035] Step 4: The precursor powder obtained in Step 3 is fed into a muffle furnace and heated to 600°C at a heating rate of 5~10°C / min in an air atmosphere. It is then calcined at 600°C for 5~6 hours. After calcination, it is naturally cooled to room temperature to obtain a silica support.

[0036] This invention also discloses a silica support prepared by the above method, wherein the silica support has a specific surface area of ​​180-350 m². 2 / g, pore volume 0.8-1.5cm 3 / g, compressive strength ≥15MPa, bulk density 0.3-0.5g / cm³ 3 There was no obvious "blowing away" phenomenon, and subsequent operations were convenient; In addition, the present invention also discloses a method for preparing a potassium-based low-temperature solid adsorbent material based on the above-mentioned silica support, comprising the following steps: Prepare a potassium carbonate aqueous solution with a mass concentration of 10%~20% for later use; the potassium carbonate is analytical grade with a purity ≥99%.

[0037] The silica carrier prepared above was added to a potassium carbonate aqueous solution at a solid-liquid mass ratio of 1:(1~2). The solution was stirred at room temperature for 2~4 hours to impregnate the silica carrier so that the potassium carbonate was uniformly loaded on the surface and in the pores of the silica carrier.

[0038] The impregnated mixture is dried at 80~100℃ for 12~24 hours to remove moisture, and the dried solid powder is obtained.

[0039] The dried solid powder is passed through an 80-100 mesh sieve to remove agglomerated particles, thus obtaining a potassium-based low-temperature solid adsorbent material.

[0040] The present invention also discloses a potassium-based low-temperature solid adsorbent material based on the above-mentioned silica carrier prepared by the above method. The potassium-based low-temperature solid adsorbent material has a CO2 adsorption capacity ≥2.2mmol / g under low temperature conditions (25-80℃), and after 5 adsorption-desorption cycles, the adsorption capacity retention rate is ≥90%, which has good carbon capture effect and cycle stability, and can meet the industrial low-temperature carbon capture requirements.

[0041] This invention employs a system of fumed silica:silica gel (30% aqueous solution):ethanol with a mass ratio of 10:0.5:89.5. Silica gel, as a binder, can effectively improve the mechanical strength of the carrier without significantly reducing the specific surface area. Ethanol, as a solvent, can avoid pore collapse caused by water evaporation stress. The three work synergistically to achieve a balance between a large specific surface area, good mechanical strength, and stable pore structure of the carrier, thus solving the technical problem of balancing the specific surface area and mechanical strength of traditional carriers.

[0042] This invention combines spray drying with constant-temperature calcination at 600℃. Spray drying can quickly remove solvents and retain the pore structure, while calcination can further enhance the mechanical strength and structural stability of the carrier, while avoiding the significant decrease in specific surface area caused by high-temperature calcination. The entire preparation process is simple, continuous and operable, suitable for large-scale industrial production, and the cost is controllable. Compared with complex processes such as supercritical drying, it is more practical and economical.

[0043] The silica support prepared by this invention effectively solves the problem of fumed silica being easily "blown away," and subsequent impregnation, filling, and other operations are convenient with low material loss. Based on this support, the potassium-based low-temperature solid adsorbent material achieves efficient CO2 capture under low-temperature conditions thanks to the support's sufficient loading sites and stable pore structure. Its adsorption capacity and cycle stability are superior to existing similar adsorbent materials, and the preparation process has no harmful gas emissions, making it green and environmentally friendly, thus making up for the shortcomings of existing potassium-based adsorbent supports with poor performance.

[0044] Meanwhile, this invention abandons traditional water solvents and uses ethanol as the main solvent. By taking advantage of the fast evaporation rate and low evaporation stress of ethanol, it effectively avoids the damage to the carrier pores caused by the stress generated by water evaporation during the drying process, and preserves the pore structure of the carrier to the maximum extent. This provides sufficient space for the loading of active components and CO2 adsorption, and solves the technical pain point of easy pore collapse in the preparation of traditional carriers.

[0045] The present invention will be further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Furthermore, it should be understood that after reading the teachings of this invention, those skilled in the art can make various alterations or modifications to the invention, and these equivalent forms also fall within the scope defined by the appended claims.

[0046] The following examples use instruments and equipment conventional in the art. Experimental methods in the following examples, unless otherwise specified, are generally performed under conventional conditions or as recommended by the manufacturer. All raw materials used in the following examples are conventional commercially available products with specifications conventional in the art. In this specification and the following examples, unless otherwise specified, "%" refers to weight percentage, "parts" refers to parts by weight, and "ratio" refers to weight proportion.

[0047] Example 1 The preparation of a silica support includes the following steps: Raw material selection: Take 100g of fumed silica (particle size 20~30nm, specific surface area 300m²) at a mass ratio of 10:0.5:89.5. 2 / g), silica gel (30% aqueous solution) 5g (SiO2 content 30%), anhydrous ethanol 895g (purity 99.7%).

[0048] Mixing: Add the above raw materials to a beaker and stir at 250 r / min for 45 min at 25℃ to obtain a uniform and transparent slurry without obvious sedimentation and clumping.

[0049] Spray drying: The mixed slurry is fed into a spray dryer, with the inlet air temperature set to 250℃, the outlet air temperature to 100℃, the feed rate to 8mL / min, and the atomization pressure to 0.3MPa, to obtain a white precursor powder.

[0050] Calcination: The precursor powder was fed into a muffle furnace and heated to 600°C at a heating rate of 8°C / min in an air atmosphere. The mixture was then calcined at a constant temperature for 5.5 hours and allowed to cool naturally to room temperature to obtain a silica support.

[0051] Figure 1 The nitrogen adsorption-desorption isotherm of the silica support in Example 1 exhibits typical Type IV isotherm characteristics, accompanied by a Type H1 hysteresis loop. In the lower relative pressure (P / P0) range (0-0.4), the adsorption amount increases slowly with increasing pressure, indicating the presence of microporous or small mesoporous structures in the material. As the relative pressure further increases (0.6-1.0), the adsorption amount increases sharply, indicating that the material has a well-developed mesoporous or macroporous structure with a relatively concentrated pore size distribution. The adsorption and desorption branches form a distinct hysteresis loop in the medium to high relative pressure range, reflecting the good connectivity and openness of the pore structure, which is conducive to the rapid diffusion and mass transfer of gas molecules. This isotherm morphology confirms that the prepared silica support possesses the synergistic advantages of high specific surface area and suitable pore structure, laying a good physical foundation for subsequent loading of active components and providing efficient carbon dioxide adsorption performance.

[0052] Performance testing: The specific surface area of ​​this silica carrier is 280 m². 2 / g, pore volume 1.2cm 3 / g, compressive strength 18MPa, bulk density 0.4g / cm³ 3 There is no obvious "blowing" phenomenon when it is poured, and it is easy to operate.

[0053] Example 2 The preparation of a potassium-based low-temperature solid adsorbent material includes the following steps: Preparation of potassium carbonate aqueous solution: Take 100g of analytical grade potassium carbonate, add 400g of deionized water, stir to dissolve, and obtain a potassium carbonate aqueous solution with a mass concentration of 20%.

[0054] Impregnation: Take 100g of the silica carrier prepared in Example 1 and add it to 150g of the above potassium carbonate aqueous solution. Stir at 25°C for 3 hours to ensure uniform loading of potassium carbonate.

[0055] Drying: Place the impregnated mixture in an oven and dry at 90°C for 18 hours to remove moisture and obtain a solid powder.

[0056] Sieving: The dried solid powder is passed through a 90-mesh sieve to remove agglomerated particles, thus obtaining potassium-based low-temperature solid adsorbent material.

[0057] Figure 2 The image shows the CO2 breakthrough curve of the potassium-based solid adsorbent in Example 2 under dynamic conditions, reflecting its adsorption and desorption performance for carbon dioxide. In the initial stage from 0 to 7 minutes, the outlet CO2 concentration remained stable at around 10%, indicating that the adsorbent had not yet begun effective adsorption or was in a pretreatment equilibrium state. From the 7th minute onwards, the concentration rapidly decreased, reaching its lowest point (approximately 1%) at about 12 minutes, indicating that the adsorbent efficiently captured CO2 from the gas stream during this stage, demonstrating excellent adsorption kinetics. Subsequently, the concentration gradually recovered, returning to near the initial level (approximately 9.5%) by the 30th minute, indicating that the adsorbent had approached saturation and entered the desorption or breakthrough stage. The entire curve exhibits a typical "V"-shaped breakthrough characteristic, confirming that the adsorbent has a fast adsorption response rate, high adsorption capacity, and good reversibility, making it suitable for CO2 capture applications under low-temperature and dynamic operating conditions.

[0058] The potassium-based solid adsorbent prepared in this embodiment has a CO2 adsorption capacity of 2.4 mmol / g under the conditions of 50°C, 10% CO2 concentration, and the remainder being nitrogen. After 5 adsorption-desorption cycles, the adsorption capacity is 2.2 mmol / g, with a retention rate of 91.7%, demonstrating good carbon capture effect and cycle stability, which meets the requirements for industrial applications.

[0059] Comparative Example 1 Without adding silica gel (30% aqueous solution), the proportions of the remaining raw materials and the preparation process are the same as in Example 1, to prepare silica carriers and potassium-based adsorbent materials.

[0060] Test results: The carrier's compressive strength is only 8 MPa, making it easily blown away; its specific surface area is 290 m². 2 / g; the CO2 adsorption capacity of the adsorbent material is 2.2 mmol / g, and the retention rate is 80% after 5 cycles.

[0061] Comparative Example 2 Water was used instead of ethanol as the solvent, and the proportions of the remaining raw materials and the preparation process were the same as in Example 1, to prepare silica carriers and potassium-based adsorbent materials.

[0062] Test results: The carrier pore volume is only 0.6 cm³. 3 / g, specific surface area 150m² 2 / g; the CO2 adsorption capacity of the adsorbent material is 1.9 mmol / g, and the retention rate is 78% after 5 cycles, with obvious pore collapse phenomenon.

[0063] Comparative Example 3 The calcination temperature was changed to 500℃, and the proportions of the remaining raw materials and the preparation process were the same as in Example 1, to prepare silica carriers and potassium-based adsorbent materials.

[0064] Test results: Carrier compressive strength 12MPa, specific surface area 250m² 2 / g; the CO2 adsorption capacity of the adsorbent material is 2.3 mmol / g, and the retention rate is 85% after 5 cycles.

[0065] The experimental results of Examples 1 and 2 and Comparative Examples 1-3 show that the silica support prepared by the present invention using a specific raw material ratio, ethanol solvent and calcination process at 600℃ is superior to the control group in terms of mechanical strength, pore structure stability and specific surface area. The carbon capture effect and cycle stability of the potassium-based adsorbent material based on this support are also significantly improved, which fully demonstrates the technical advantages of the present invention.

[0066] Example 3 The preparation of a silica support includes the following steps: Raw material selection: 100g of fumed silica (particle size 10nm, specific surface area 200m²) was selected according to a mass ratio of 10:0.5:89.5. 2 / g), silica gel (30% aqueous solution) 5g (SiO2 content 28%), anhydrous ethanol 895g (purity 99.5%).

[0067] Mixing: Add the above raw materials to a mixing container and stir at 200 r / min for 60 min at 20℃ to obtain a homogeneous slurry without obvious sedimentation or agglomeration.

[0068] Spray drying: The mixed slurry is fed into a spray dryer, with the inlet air temperature set to 200℃, the outlet air temperature to 80℃, the feed rate to 5mL / min, and the atomization pressure to 0.2MPa, to obtain a white precursor powder.

[0069] Calcination: The precursor powder was fed into a muffle furnace and heated to 600°C at a heating rate of 5°C / min in an air atmosphere. The mixture was then calcined at a constant temperature for 6 hours and allowed to cool naturally to room temperature to obtain a silica support.

[0070] Performance testing: The specific surface area of ​​this silica carrier is 185 m². 2 / g, pore volume 0.85cm 3 / g, compressive strength 16MPa, bulk density 0.32g / cm³ 3 There is no obvious "blowing" phenomenon when it is poured, and it is easy to operate.

[0071] Example 4 The preparation of a silica support includes the following steps: Raw material selection: 100g of fumed silica (particle size 50nm, specific surface area 400m²) was selected at a mass ratio of 10:0.5:89.5. 2 / g), silica gel (30% aqueous solution) 5g (SiO2 content 32%), anhydrous ethanol 895g (purity 99.8%).

[0072] Mixing: Add the above raw materials to a mixing container and stir at 300 r / min for 30 min at 25℃ to obtain a homogeneous slurry without obvious sedimentation or agglomeration.

[0073] Spray drying: The mixed slurry is fed into a spray dryer, with the inlet air temperature set at 300℃, the outlet air temperature at 120℃, the feed rate at 10mL / min, and the atomization pressure at 0.4MPa, to obtain a white precursor powder.

[0074] Calcination: The precursor powder was fed into a muffle furnace and heated to 600°C at a heating rate of 10°C / min in an air atmosphere. The mixture was then calcined at a constant temperature for 5 hours and allowed to cool naturally to room temperature to obtain a silica support.

[0075] Performance testing: The specific surface area of ​​this silica carrier is 340 m². 2 / g, pore volume 1.45 cm³ 3 / g, compressive strength 17MPa, bulk density 0.48 g / cm³ 3 There is no obvious "blowing" phenomenon when it is poured, and it is easy to operate.

[0076] Example 5 The preparation of a potassium-based low-temperature solid adsorbent material includes the following steps: Preparation of potassium carbonate aqueous solution: Take 100g of analytical grade potassium carbonate, add 900g of deionized water, stir to dissolve, and obtain a potassium carbonate aqueous solution with a mass concentration of 10%.

[0077] Impregnation: Take 100g of the silica carrier prepared in Example 3 and add it to 100g of the above potassium carbonate aqueous solution (solid-liquid mass ratio 1:1). Stir at room temperature for 4 hours to ensure uniform loading of potassium carbonate.

[0078] Drying: Place the impregnated mixture into an oven and dry at 80°C for 24 hours to remove moisture and obtain a dried solid powder.

[0079] Sieving: The dried solid powder is passed through an 80-mesh sieve to remove agglomerated particles, thus obtaining potassium-based low-temperature solid adsorbent material.

[0080] Performance testing: Under conditions of 25℃, CO2 concentration of 10%, and the remainder being nitrogen, the CO2 adsorption capacity of this adsorbent material is 2.25 mmol / g; after 5 adsorption-desorption cycles, the adsorption capacity is 2.05 mmol / g, with a retention rate of 91.1%, demonstrating good carbon capture effect and cycle stability.

[0081] Example 6 The preparation of a potassium-based low-temperature solid adsorbent material includes the following steps: Preparation of potassium carbonate aqueous solution: Take 200g of analytical grade potassium carbonate, add 800g of deionized water, stir to dissolve, and obtain a potassium carbonate aqueous solution with a mass concentration of 20%.

[0082] Impregnation: Take 100g of the silica carrier prepared in Example 4 and add it to 200g of the above potassium carbonate aqueous solution (solid-liquid mass ratio 1:2). Stir at room temperature for 2 hours to ensure uniform loading of potassium carbonate.

[0083] Drying: Place the impregnated mixture into an oven and dry at 100°C for 12 hours to remove moisture and obtain a dried solid powder.

[0084] Sieving: The dried solid powder is passed through a 100-mesh sieve to remove agglomerated particles, thus obtaining potassium-based low-temperature solid adsorbent material.

[0085] Performance testing: Under conditions of 80℃, CO2 concentration of 10%, and the remainder being nitrogen, the CO2 adsorption capacity of this adsorbent material is 2.3 mmol / g; after 5 adsorption-desorption cycles, the adsorption capacity is 2.1 mmol / g, with a retention rate of 91.3%, demonstrating good carbon capture effect and cycle stability.

[0086] The silica support prepared by this invention retains the large specific surface area advantage of fumed silica while enhancing its mechanical strength through the bonding effect of silica gel and a specific calcination process. Furthermore, the use of ethanol as a solvent prevents pore collapse, solving the problems of easy blowing and inconvenient handling associated with traditional fumed silica. Subsequent impregnation and filling operations are convenient, with low material loss and strong practicality. In addition, the potassium-based low-temperature solid adsorbent material based on this silica support provides ample loading sites for potassium carbonate due to the support's large specific surface area and stable pore structure, resulting in uniform dispersion of the active component and significantly improving CO2 adsorption capacity and cycle stability under low-temperature conditions. This meets the low-temperature carbon capture requirements of industrial flue gas, chemical tail gas, and other scenarios, and has broad prospects for industrial application.

[0087] The preparation process of this invention is simple, continuous, and operable, with readily available and cost-controllable raw materials. The entire process produces no harmful gas emissions, making it environmentally friendly. Compared to existing complex preparation processes, it is more suitable for large-scale industrial production, effectively reducing carbon capture costs and promoting the industrial application of CCUS technology. Compared to existing silica-based adsorbent preparation processes, this invention does not require complex surface modification or supercritical drying equipment. The optimization of carrier performance can be achieved solely through conventional spray drying and calcination processes, resulting in low equipment investment and low energy consumption, further enhancing the technology's economic viability and practicality.

[0088] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the essence and scope of the technical solutions of the present invention.

Claims

1. A method for preparing a silica carrier, characterized in that, Includes the following steps: Fumed silica, silica gel aqueous solution and ethanol are mixed and stirred to obtain a mixed slurry; The mixed slurry was spray-dried to obtain precursor powder; The precursor powder was calcined to obtain a silica carrier.

2. The method for preparing a silica carrier according to claim 1, characterized in that, The mass ratio of the fumed silica, silica gel aqueous solution, and ethanol is 10:0.5:89.

5.

3. The method for preparing a silica carrier according to claim 1, characterized in that, The fumed silica has a particle size of 10-50 nm and a specific surface area of ​​200-400 m². 2 / g; the SiO2 content in the silica gel aqueous solution is 28%~32%.

4. The method for preparing a silica carrier according to claim 1, characterized in that, The inlet air temperature of the spray dryer is 200~300℃, and the outlet air temperature is 80~120℃.

5. The method for preparing a silica carrier according to claim 1, characterized in that, In step 3, calcination is carried out in an air atmosphere at a temperature of 600°C for 5-6 hours.

6. A silica carrier, characterized in that, It is prepared by the method described in any one of claims 1 to 5.

7. A method for preparing a potassium-based low-temperature solid adsorbent material, characterized in that, Prepared using a silica support as described in claim 6, and comprising the following steps: The silica carrier was added to a potassium carbonate aqueous solution for impregnation treatment; The impregnated mixture is dried to obtain a solid powder; The solid powder is sieved to obtain the potassium-based low-temperature solid adsorbent material.

8. The method for preparing a potassium-based low-temperature solid adsorbent material according to claim 7, characterized in that, The mass concentration of the potassium carbonate aqueous solution is 10%~20%; the solid-liquid mass ratio of the silica carrier to the potassium carbonate aqueous solution is 1:(1~2).

9. The method for preparing a potassium-based low-temperature solid adsorbent material according to claim 7, characterized in that, The impregnated mixture is dried to obtain a solid powder, wherein the drying temperature is 80~100℃ and the drying time is 12~24 hours; The solid powder is sieved to obtain a potassium-based low-temperature solid adsorbent material, wherein the sieve used for sieving is 80-100 mesh.

10. A potassium-based low-temperature solid adsorbent material, characterized in that, It is prepared by the method described in any one of claims 7 to 9.