A method for preparing potassium nitrate from waste magnesium oxide from grain-oriented silicon steel

By employing a process sequence of first removing impurities and then undergoing metathesis, and targeting the specific impurity composition of magnesium oxide waste from oriented silicon steel, high-purity potassium nitrate was prepared through pressure filtration and oxidant treatment. This solved the problems of high raw material costs and low product purity in potassium nitrate production, and realized the high-value utilization of magnesium resources.

CN123105679APending Publication Date: 2026-11-17BAOTOU WEIFENG ELECTROMAGNETIC MATERIAL +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611611705.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The current potassium nitrate production process suffers from high raw material costs and difficulty in achieving industrial-grade product purity. Furthermore, the magnesium oxide waste from oriented silicon steel is not effectively utilized, and its direct application in potassium nitrate production presents challenges in removing iron impurities.

Method used

By adopting a process sequence of first removing impurities and then performing metathesis, acid-insoluble substances such as silica are removed by pressure filtration, iron impurities are oxidized with an oxidant and the pH value is adjusted to precipitate, and combined with precision filtration, high-purity potassium nitrate is prepared, with magnesium chloride as a byproduct.

Benefits of technology

This method enables the preparation of industrial-grade potassium nitrate from waste magnesium oxide, reducing production costs, solving the problem of iron impurity removal, and achieving a product purity of over 98.5%, which meets industrial-grade standards, thus realizing the high-value utilization of magnesium resources.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a method for preparing potassium nitrate from waste magnesium oxide from oriented silicon steel, belonging to the field of chemical production technology. The method includes: neutralizing waste magnesium oxide from oriented silicon steel with nitric acid to obtain a magnesium nitrate reaction solution; subjecting the magnesium nitrate reaction solution to impurity removal treatment, which includes at least solid-liquid separation and removal of iron impurities, to obtain a refined magnesium nitrate solution; subjecting the refined magnesium nitrate solution to a metathesis reaction with potassium chloride to obtain a metathesis reaction solution containing potassium nitrate; and cooling and crystallizing the metathesis reaction solution to obtain potassium nitrate crystals. This invention uses waste magnesium oxide from oriented silicon steel instead of purchased high-purity magnesium oxide as the magnesium source, reducing the production cost of potassium nitrate. Simultaneously, it designs a systematic impurity removal scheme to address the high silica and iron oxide content in the waste magnesium oxide from oriented silicon steel, resulting in potassium nitrate products with purity reaching industrial-grade standards, achieving high-value resource utilization of waste magnesium oxide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of chemical production technology, and in particular to a method for preparing potassium nitrate from waste magnesium oxide from oriented silicon steel. Background Technology

[0002] Potassium nitrate is an important inorganic chemical product, widely used in agricultural fertilizers, industrial explosives, glass clarifying agents, and food preservatives. Existing production methods for potassium nitrate mainly include the sodium nitrate-potassium chloride metathesis process, the potassium chloride-nitric acid direct process, and the nitric acid-potassium chloride-magnesium oxide process. Among these, the nitric acid-potassium chloride-magnesium oxide process is widely used due to the readily available raw materials and relatively simple process. This method uses nitric acid, potassium chloride, and magnesium oxide (or magnesia) as raw materials. A neutralization reaction produces magnesium nitrate, which then undergoes metathesis with potassium chloride to produce potassium nitrate, with magnesium chloride as a byproduct.

[0003] However, the existing nitric acid-potassium chloride-magnesium oxide process has two prominent problems: First, this method generally uses purchased high-purity light magnesium oxide or magnesia as the magnesium source. It takes about 0.26 tons of magnesia to produce 1 ton of potassium nitrate, and the raw material cost accounts for a large proportion, resulting in high potassium nitrate prices and making it difficult to promote its widespread application in the agricultural field. Second, the existing process has a relatively simple impurity removal treatment for raw materials. Usually, conventional filtration is only performed after the metathesis reaction to remove acid-insoluble substances. This can meet the requirements when using high-purity magnesium oxide as raw material, but the resulting product is mostly agricultural-grade potassium nitrate, which is difficult to meet industrial-grade standards.

[0004] On the other hand, during the production of grain-oriented silicon steel, the annealing and coating processes generate a large amount of waste magnesium oxide powder (referred to in this invention as: grain-oriented silicon steel waste magnesium oxide). Approximately 6-7 kg of this powder is generated for every ton of grain-oriented silicon steel produced. This waste magnesium oxide powder is predominantly composed of magnesium oxide, with silicon dioxide and iron-containing components as the main impurities. Silicon dioxide mainly exists as acid-insoluble matter, while iron is dispersed within the magnesium oxide particles as iron oxide or iron silicate. Currently, the utilization of this waste magnesium oxide powder mainly focuses on the preparation of magnesium-carbon spheres, flame-retardant magnesium hydroxide, or recycled silicon steel-grade magnesium oxide. However, these utilization methods either result in low added value or complex processes (e.g., recycled magnesium oxide requires more than 10 steps), and the recycled products have low purity and uneven particle size, failing to achieve high-value utilization of this waste.

[0005] More importantly, directly using the aforementioned waste magnesium oxide from oriented silicon steel for the production of potassium nitrate using the existing nitric acid-potassium chloride-magnesium oxide method would face insurmountable technical obstacles. During the acid dissolution stage, the magnesium oxide in the waste magnesium oxide from oriented silicon steel reacts with nitric acid to form magnesium nitrate, while acid-insoluble substances such as silica remain suspended in the reaction solution as solid residues. Iron, on the other hand, is dissolved as Fe. 2+ / Fe 3+Ionic states enter the solution. If the conventional process of "simple filtration after metathesis reaction" is used, the following problems exist: First, after the metathesis reaction, the system simultaneously contains multiple salts such as potassium nitrate, magnesium chloride, and unreacted potassium chloride, significantly increasing the solution viscosity and creating high resistance to filtration of solid impurities; Second, in a chlorine-containing environment (high concentration of Cl),... - Under these conditions, Fe 3+ It readily forms soluble complexes with chloride ions (such as [FeCl4]). - At this point, even adjusting the pH value makes it difficult to completely precipitate iron ions, causing iron impurities to enter the crystallization system with the mother liquor. As a result, the final product has excessive iron content and a yellowish color, barely meeting the agricultural grade standard and failing to meet the purity requirements of industrial grade potassium nitrate.

[0006] Therefore, under the current technological background, magnesium oxide waste from oriented silicon steel is regarded as a low-quality magnesium-containing waste that "cannot be directly used for potassium nitrate production". The existing technology has never provided technical guidance on how to remove the high silicon and high iron impurities of this specific waste in the potassium nitrate production system, and has never publicly or implied the use of "magnesium oxide waste from oriented silicon steel can be used to prepare potassium nitrate".

[0007] In summary, there are few reports in the existing technology on the direct use of magnesium oxide from oriented silicon steel waste in potassium nitrate production, and there are also very few process methods that can overcome the specific technical obstacles mentioned above and use this industrial waste as raw material to prepare industrial-grade potassium nitrate. Summary of the Invention

[0008] To address the problems in existing technologies, such as high raw material costs for potassium nitrate production, difficulty in achieving industrial-grade purity, low added value of the resource utilization pathways for magnesium oxide from oriented silicon steel, and a lack of effective coupling with potassium nitrate production processes, this invention provides a method for preparing potassium nitrate from magnesium oxide from oriented silicon steel. This invention addresses the specific impurity composition of magnesium oxide from oriented silicon steel, characterized by high silicon and high iron content. Breaking away from the conventional approach of first performing secondary decomposition followed by impurity removal, this invention adopts a specific process sequence of "impurity removal first, then secondary decomposition," and designs a matching system for impurity removal. This allows for the production of industrial-grade potassium nitrate using industrial waste as raw material, while simultaneously producing magnesium chloride as a byproduct. This achieves high-value, targeted utilization of waste magnesium oxide and a significant reduction in potassium nitrate production costs.

[0009] The technical solution of the present invention is as follows: This invention provides a method for preparing potassium nitrate from waste magnesium oxide from oriented silicon steel, comprising the following steps: Magnesium oxide waste from oriented silicon steel is neutralized with nitric acid to obtain a magnesium nitrate reaction solution; the magnesium nitrate reaction solution is then subjected to impurity removal treatment, which includes at least a solid-liquid separation step and an iron impurity removal step, to obtain a refined magnesium nitrate solution; the refined magnesium nitrate solution is then subjected to a metathesis reaction with potassium chloride to obtain a metathesis reaction solution containing potassium nitrate; the metathesis reaction solution is then cooled and crystallized to obtain potassium nitrate crystals.

[0010] Preferably, the method for preparing potassium nitrate from waste magnesium oxide of oriented silicon steel specifically includes the following steps: S1. Pre-treat the magnesium oxide waste from oriented silicon steel; S2. Neutralize the pretreated waste magnesium oxide with nitric acid to obtain magnesium nitrate reaction solution; S3. The magnesium nitrate reaction solution is subjected to a purification treatment, which includes a solid-liquid separation step and a step of removing iron impurities to obtain a refined magnesium nitrate solution. S4. The refined magnesium nitrate solution is subjected to a double decomposition reaction with potassium chloride to obtain a double decomposition reaction solution containing potassium nitrate and magnesium chloride. S5. The obtained double decomposition reaction solution is first evaporated and concentrated, then subjected to two-stage cooling crystallization, and solid-liquid separation is performed to obtain crude potassium nitrate crystals and mother liquor. S6. The crude potassium nitrate crystals are washed and dried to obtain the potassium nitrate product; S7. Post-process the mother liquor obtained in step S5.

[0011] Preferably, the composition of the oriented silicon steel waste magnesium oxide includes: 75~88wt% MgO, 4~13wt% SiO2, 2~6wt% iron oxides calculated as Fe2O3, 1~10wt% loss on burn, and the balance being unavoidable trace impurities.

[0012] In this invention, the burn-off mainly originates from the carbonaceous components remaining in the annealing process of the grain-oriented silicon steel. These carbonaceous components are chemically inert in the acid reaction process and are insoluble in the acidic reaction solution. Therefore, they can be effectively retained and removed along with acid-insoluble substances such as silica in step S3 via pressure filtration. They will not enter the subsequent magnesium nitrate solution, nor will they be introduced into the final potassium nitrate product, thus having no adverse impact on key indicators such as product purity and chloride ion content. Based on this, the waste magnesium oxide powder from the grain-oriented silicon steel of this invention does not require pretreatment such as calcination to remove carbonaceous components and can be directly used as a magnesium source, further simplifying the process and reducing energy consumption and production costs.

[0013] Preferably, in step S1, the pretreatment includes at least one of crushing, screening, washing, ultrasonic assistance, and slurry preparation.

[0014] More preferably, the pretreatment is crushing and sieving, in which the waste magnesium oxide powder is crushed and sieved to 80-200 mesh.

[0015] Preferably, in step S2, the amount of pretreated waste magnesium oxide and nitric acid is mixed according to the molar ratio of MgO to HNO3 of 1:(2.0~2.3).

[0016] Preferably, in step S2, the concentration of nitric acid is 30wt%~65wt%, the temperature of the neutralization reaction is 60~90℃, and the reaction time is 1~3h.

[0017] In further explanation of the present invention, in step S2 above, during the reaction of waste magnesium oxide with nitric acid, the magnesium oxide in the waste magnesium oxide undergoes a neutralization reaction with nitric acid to generate magnesium nitrate and water. Acid-insoluble substances such as silicon dioxide are suspended in the reaction solution as solid residues, while iron elements enter the solution in ionic form.

[0018] Preferably, in step S3, the solid-liquid separation is pressure filtration. Since the magnesium oxide waste from oriented silicon steel contains a large amount of acid-insoluble matter, mainly silicon dioxide, if these solid impurities are not removed first, they will be mixed into the product during subsequent metathesis reactions and crystallization processes, affecting the purity of potassium nitrate. Pressure filtration can achieve efficient separation of magnesium nitrate solution from solid impurities such as silicon dioxide; it is simple to operate and has a large processing capacity, making it suitable for industrial production.

[0019] Preferably, in step S3, the removal of iron impurities includes adding an oxidant to oxidize and adjusting the pH of the magnesium nitrate reaction solution to 4.5-5, causing iron ions to form hydroxide precipitates, which are then removed by filtration. Iron impurities in waste magnesium oxide from silicon steel exist in ionic form in the solution after acid dissolution, with some iron existing as ferrous ions. By adding an oxidant to the solution, the ferrous ions are first fully oxidized to ferric ions, and then the pH is adjusted to hydrolyze the ferric ions to form ferric hydroxide colloidal precipitates, which are then effectively removed by solid-liquid separation. Compared to directly adjusting the pH for precipitation, the method of oxidation followed by precipitation allows for more complete precipitation of iron ions and a more thorough iron removal effect. If this step is omitted, the iron ions will enter the metathesis reaction along with the magnesium nitrate solution and either co-precipitate with potassium nitrate during subsequent crystallization or become trapped between crystal particles, leading to yellowing of the product and a decrease in purity.

[0020] More preferably, in step S3, the impurity removal process further includes a precision filtration step. The magnesium nitrate solution after pressure filtration to remove silicon and iron may still contain trace amounts of suspended particles or colloidal impurities. Precision filtration, such as microfiltration or membrane filtration, can further purify the solution, ensuring that the magnesium nitrate solution entering the metathesis reaction has sufficient purity, laying the foundation for the preparation of industrial-grade potassium nitrate.

[0021] More preferably, step S3 specifically involves: conveying the magnesium nitrate reaction solution obtained in step S2 to a plate and frame filter press for filtration, collecting the filtrate; adding an oxidant to the filtrate and stirring at 30-60°C for 30-50 minutes to oxidize the solution, thereby reducing the Fe content. 2+ Fully oxidized to Fe 3+ The amount of oxidant added is 0.3-1.0% of the total mass of the magnesium nitrate reaction solution; then, a pH adjuster is added to the solution to adjust the pH value to 4.5-5, so that Fe... 3+ Hydrolysis produces Fe(OH)3 colloidal precipitate, which is then filtered again after standing for 20-30 minutes to remove the iron precipitate. The filtrate after iron removal is then subjected to final precision filtration through a 0.5-1.0 μm microporous precision filter to obtain a refined magnesium nitrate solution.

[0022] More preferably, the oxidant is a hydrogen peroxide solution; the concentration of the hydrogen peroxide solution is 28wt%~32wt%.

[0023] More preferably, the pH adjuster is selected from at least one of magnesium hydroxide, magnesium oxide, and magnesium carbonate.

[0024] Preferably, in step S4, the molar ratio of potassium chloride to magnesium nitrate in the refined magnesium nitrate solution is (2.0~2.2):1, the temperature of the metathesis reaction is 60~100℃, and the reaction time is 1~3h.

[0025] Preferably, S5 specifically includes: The metathesis reaction solution obtained in step S4 is first evaporated and concentrated at 60-90℃ and a vacuum of 0.08-0.09 MPa to obtain a solution density of 1.30-1.35 g / cm³. 3 Then, the concentrated metathesis reaction solution was cooled to 35-45℃ at a cooling rate of 0.5-1.5℃ / min, and stirred for 0.5-1.5h. Solid-liquid separation was performed to obtain the first stage of crude potassium nitrate crystals and the first stage of mother liquor. The first stage of mother liquor was then cooled to 5-15℃ at a cooling rate of 0.3-1.0℃ / min, and stirred for 1-3h. Solid-liquid separation was performed to obtain the second stage of crude potassium nitrate crystals and the second stage of mother liquor.

[0026] Preferably, the first stage of crude potassium nitrate crystals directly enters step S6 for processing; the second stage of crude potassium nitrate crystals returns to the metathesis reaction in step S4 for redissolution, or enters step S6 after recrystallization.

[0027] Preferably, S6 specifically includes: The crude potassium nitrate crystals obtained in step S5 are washed using a countercurrent slurry washing method. The washing solution is a saturated potassium nitrate solution pre-cooled to 0~5℃. The number of washing stages is 2~3, and the total amount of washing solution is 15~30% of the mass of the crude crystals. After each washing stage, the crystals are centrifuged to remove water until the water content of the crystals is ≤5%. The washed and dehydrated crystals are dried at 100~110℃ to constant weight to obtain the potassium nitrate product.

[0028] Preferably, after washing and dehydration, the Cl of the crystals... - When the content is higher than 0.02%, a recrystallization step is also included before drying: the washed and dehydrated crystals are dissolved in hot water at 80-95°C at a solid-liquid ratio of 1:(1.5~2.5), filtered while hot, and the filtrate is cooled to 10-20°C at a cooling rate of 0.5~1.0°C / min for recrystallization. The solid and liquid are separated to obtain recrystallized potassium nitrate crystals and recrystallization mother liquor; the recrystallization mother liquor is returned to step S4 or step S5 for recycling.

[0029] Preferably, in step S7, the post-processing is as follows: the mother liquor obtained in step S5 is recycled back to the metathesis reaction in step S4, and / or the mother liquor obtained in step S5 is concentrated by evaporation and cooled to crystallize, to obtain magnesium chloride by-product.

[0030] More preferably, S7 specifically includes: The first mother liquor obtained in step S5 is recycled back to the metathesis reaction in step S4; the second mother liquor obtained in step S5 is divided into two parallel processes: the first process directly recycles 70-90% of the total volume of the second mother liquor back to the metathesis reaction in step S4; the second process leads the remaining mother liquor to an evaporation and concentration device, where it is evaporated, concentrated, cooled, and crystallized to obtain magnesium chloride hexahydrate as a byproduct.

[0031] Further explanation of the present invention: In industrial continuous production, the recycled mother liquor can return the residual potassium nitrate and magnesium nitrate to the metathesis reaction system, which is beneficial to improving the total yield of potassium; while recovering magnesium chloride hexahydrate by-products from the evaporated mother liquor, the impurities that gradually accumulate during the mother liquor circulation process can be discharged from the system, avoiding the accumulation of impurities in the system and affecting product quality.

[0032] The present invention also provides a potassium nitrate product prepared by the above method.

[0033] Preferably, the purity of the potassium nitrate product is ≥98.5%, which meets the technical requirements of Class III products in GB / T 1918-2021 Industrial Potassium Nitrate.

[0034] The present invention has the following beneficial effects: 1. Compared with existing technologies, this invention uses waste magnesium oxide from oriented silicon steel to replace purchased high-purity magnesium oxide or magnesia as the magnesium source, fundamentally reducing the raw material cost of potassium nitrate production and solving the environmental pollution problem caused by the accumulation of waste magnesium oxide in the silicon steel industry. More importantly, targeting the specific impurities in waste magnesium oxide from oriented silicon steel, such as high silica content and high ferric oxide content, this invention incorporates a systematic impurity removal process after the acid dissolution step and before the metathesis reaction. Pressure filtration effectively retains acid-insoluble substances such as silica; an oxidant fully oxidizes ferrous ions to ferric ions, and the pH value is adjusted to precipitate and remove them; and precision filtration intercepts trace suspended solids. These three impurity removal steps work together progressively, effectively removing key impurities such as iron and silicon before magnesium enters the metathesis reaction. This allows the potassium nitrate product prepared from waste magnesium oxide to achieve a purity of over 98.5%, meeting industrial-grade standards. In existing technologies, whether using commercial magnesia to produce potassium nitrate or using waste magnesium oxide from other sources, no specific system for removing such impurities has been designed. Therefore, it is impossible to stably obtain industrial-grade potassium nitrate products using waste magnesium oxide as raw material.

[0035] 2. Compared to existing technologies, this invention directly couples the utilization of waste magnesium oxide from oriented silicon steel with the production of potassium nitrate, eliminating the intermediate conversion step of regenerating waste magnesium oxide from oriented silicon steel into high-purity magnesium oxide, thus significantly shortening the process flow. Magnesium in the waste magnesium oxide from oriented silicon steel is converted into magnesium nitrate during the neutralization reaction stage, participating in the production of the main product, potassium nitrate. The magnesium chloride contained in the mother liquor after the metathesis reaction can be recovered as a byproduct of magnesium chloride hexahydrate through evaporation and concentration. Throughout the process, magnesium resources are fully extracted and recovered at a high value. Simultaneously, the disposal method of partially recycling the mother liquor for the metathesis reaction and partially extracting it for the production of magnesium chloride byproducts avoids the discharge of saline wastewater, achieving clean production. Compared to existing technologies that use waste magnesium oxide from oriented silicon steel to produce low-value-added products such as magnesium-carbon spheres and magnesium pellets, this invention allows the magnesium resources in the waste magnesium oxide from oriented silicon steel to enter two high-value product chains: potassium nitrate and magnesium chloride. The utilization efficiency and added value of magnesium resources are significantly improved. Detailed Implementation

[0036] The technical solutions described below in conjunction with the embodiments will be clearly and completely described. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0037] This invention provides a method for preparing potassium nitrate from waste magnesium oxide from oriented silicon steel, comprising the following steps: Magnesium oxide waste from oriented silicon steel is neutralized with nitric acid to obtain a magnesium nitrate reaction solution; the magnesium nitrate reaction solution is then subjected to impurity removal treatment, which includes at least a solid-liquid separation step and an iron impurity removal step, to obtain a refined magnesium nitrate solution; the refined magnesium nitrate solution is then subjected to a metathesis reaction with potassium chloride to obtain a metathesis reaction solution containing potassium nitrate; the metathesis reaction solution is then cooled and crystallized to obtain potassium nitrate crystals.

[0038] Preferably, the method for preparing potassium nitrate from waste magnesium oxide of oriented silicon steel specifically includes the following steps: S1. Pre-treat the magnesium oxide waste from oriented silicon steel; S2. Neutralize the pretreated waste magnesium oxide with nitric acid to obtain magnesium nitrate reaction solution; S3. The magnesium nitrate reaction solution is subjected to a purification treatment, which includes a solid-liquid separation step and a step of removing iron impurities to obtain a refined magnesium nitrate solution. S4. The refined magnesium nitrate solution is subjected to a double decomposition reaction with potassium chloride to obtain a double decomposition reaction solution containing potassium nitrate and magnesium chloride. S5. The obtained double decomposition reaction solution is first evaporated and concentrated, then subjected to two-stage cooling crystallization, and solid-liquid separation is performed to obtain crude potassium nitrate crystals and mother liquor. S6. The crude potassium nitrate crystals are washed and dried to obtain the potassium nitrate product; S7. Post-process the mother liquor obtained in step S5.

[0039] Preferably, the composition of the oriented silicon steel waste magnesium oxide includes: 75~88wt% MgO, 4~13wt% SiO2, 2~6wt% iron oxides calculated as Fe2O3, 1~10wt% loss on burn, and the balance being unavoidable trace impurities.

[0040] Preferably, in step S1, the pretreatment includes at least one of crushing, screening, washing, ultrasonic assistance, and slurry preparation.

[0041] More preferably, the pretreatment is crushing and sieving, in which the waste magnesium oxide powder is crushed and sieved to 80-200 mesh.

[0042] Preferably, in step S2, the amount of pretreated waste magnesium oxide and nitric acid is mixed in a molar ratio of MgO to HNO3 of 1:(2.0~2.3).

[0043] Preferably, in step S2, the concentration of nitric acid is 30wt%~65wt%, the temperature of the neutralization reaction is 60~90℃, and the reaction time is 1~3h.

[0044] Preferably, in step S3, the solid-liquid separation is pressure filtration separation.

[0045] Preferably, in step S3, the removal of iron impurities includes adding an oxidant to oxidize and adjusting the pH of the magnesium nitrate reaction solution to 4.5-5, so that the iron ions form hydroxide precipitates and are then removed by filtration.

[0046] More preferably, in step S3, the impurity removal process further includes a precision filtration step.

[0047] More preferably, step S3 specifically involves: conveying the magnesium nitrate reaction solution obtained in step S2 to a plate and frame filter press for filtration, collecting the filtrate; adding an oxidant to the filtrate and stirring at 30-60°C for 30-50 minutes to oxidize the solution, thereby reducing the Fe content. 2+ Fully oxidized to Fe 3+ The amount of oxidant added is 0.3~1.0 wt% of the total mass of the magnesium nitrate reaction solution; then, a pH adjuster is added to the solution to adjust the pH value to 4.5~5, so that Fe... 3+ Hydrolysis produces Fe(OH)3 colloidal precipitate, which is then filtered again after standing for 20-30 minutes to remove the iron precipitate. The filtrate after iron removal is then subjected to final precision filtration through a 0.5-1.0 μm microporous precision filter to obtain a refined magnesium nitrate solution.

[0048] More preferably, the oxidant is a hydrogen peroxide solution; the concentration of the hydrogen peroxide solution is 28wt%~32wt%.

[0049] More preferably, the pH adjuster is selected from at least one of magnesium hydroxide, magnesium oxide, and magnesium carbonate.

[0050] Preferably, in step S4, the molar ratio of potassium chloride to magnesium nitrate in the refined magnesium nitrate solution is (2.0~2.2):1, the temperature of the metathesis reaction is 60~100℃, and the reaction time is 1~3h.

[0051] Preferably, S5 specifically includes: The metathesis reaction solution obtained in step S4 is first evaporated and concentrated at 60-90℃ and a vacuum of 0.08-0.09 MPa to obtain a solution density of 1.30-1.35 g / cm³. 3 Then, the concentrated metathesis reaction solution was cooled to 35-45℃ at a cooling rate of 0.5-1.5℃ / min, and stirred for 0.5-1.5h. Solid-liquid separation was performed to obtain the first stage of crude potassium nitrate crystals and the first stage of mother liquor. The first stage of mother liquor was then cooled to 5-15℃ at a cooling rate of 0.3-1.0℃ / min, and stirred for 1-3h. Solid-liquid separation was performed to obtain the second stage of crude potassium nitrate crystals and the second stage of mother liquor.

[0052] Preferably, the first stage of crude potassium nitrate crystals directly enters step S6 for processing; the second stage of crude potassium nitrate crystals returns to the metathesis reaction in step S4 for redissolution, or enters step S6 after recrystallization.

[0053] Preferably, S6 specifically includes: The crude potassium nitrate crystals obtained in step S5 are washed using a countercurrent slurry washing method. The washing solution is a saturated potassium nitrate solution pre-cooled to 0~5℃. The number of washing stages is 2~3, and the total amount of washing solution is 15~30% of the mass of the crude crystals. After each washing stage, the crystals are centrifuged to remove water until the water content of the crystals is ≤5%. The washed and dehydrated crystals are dried at 100~110℃ to constant weight to obtain the potassium nitrate product.

[0054] Preferably, after washing and dehydration, the Cl of the crystals... - When the content is higher than 0.02%, a recrystallization step is also included before drying: the washed and dehydrated crystals are dissolved in hot water at 80-95°C at a solid-liquid ratio of 1:(1.5~2.5), filtered while hot, and the filtrate is cooled to 10-20°C at a cooling rate of 0.5~1.0°C / min for recrystallization. The solid and liquid are separated to obtain recrystallized potassium nitrate crystals and recrystallization mother liquor; the recrystallization mother liquor is returned to step S4 or step S5 for recycling.

[0055] Preferably, in step S7, the post-processing is as follows: the mother liquor obtained in step S5 is recycled back to the metathesis reaction in step S4, and / or the mother liquor obtained in step S5 is concentrated by evaporation and cooled to crystallize, to obtain magnesium chloride by-product.

[0056] More preferably, S7 specifically includes: The first mother liquor obtained in step S5 is recycled back to the metathesis reaction in step S4; the second mother liquor obtained in step S5 is divided into two parallel processes: the first process directly recycles 70-90% of the total volume of the second mother liquor back to the metathesis reaction in step S4; the second process leads the remaining mother liquor to an evaporation and concentration device, where it is evaporated, concentrated, cooled, and crystallized to obtain magnesium chloride hexahydrate as a byproduct.

[0057] The present invention also provides a potassium nitrate product prepared by the above method.

[0058] Preferably, the purity of the potassium nitrate product is ≥98.5%, which meets the technical requirements of Class III products in GB / T 1918-2021 Industrial Potassium Nitrate.

[0059] The technical solution of the present invention will be further described below with reference to specific embodiments.

[0060] Example 1

[0061] A method for preparing potassium nitrate from waste magnesium oxide from oriented silicon steel includes the following steps: S1. Waste magnesium oxide powder collected directly from the annealing process of oriented silicon steel was tested and found to contain 78.5 wt% MgO, 7.2 wt% SiO2, 3.1 wt% iron oxide (calculated as Fe2O3), and 9.8 wt% loss on ignition. The remainder consisted of unavoidable trace impurities. The waste magnesium oxide powder was crushed, ground, and passed through a 100-mesh sieve to obtain pretreated waste magnesium oxide. S2. Add the pretreated waste magnesium oxide obtained in S1 to a reaction vessel containing 45wt% nitric acid, so that the amount of pretreated waste magnesium oxide and nitric acid fed is 1:2.1 in molar ratio of MgO to HNO3. Then, keep the temperature at 80℃ and stir continuously for 3 hours. After the reaction is completed, magnesium nitrate reaction solution is obtained. S3. The magnesium nitrate reaction solution obtained in step S2 is transferred to a plate and frame filter press for filtration, and the filtrate is collected. A 30wt% hydrogen peroxide solution is added to the filtrate and stirred at 40°C for 40 minutes to oxidize the solution, thereby reducing the Fe content. 2+ Fully oxidized to Fe 3 + The amount of hydrogen peroxide solution added was 0.6 wt% of the total mass of the magnesium nitrate reaction solution; then magnesium hydroxide was added to the solution to adjust the pH to 4.5, so that Fe... 3+ Hydrolysis produces Fe(OH)3 colloidal precipitate, which is then filtered again after standing for 30 minutes to remove the iron precipitate. The filtrate after iron removal is then subjected to final precision filtration through a 0.5 μm microporous precision filter to obtain a refined magnesium nitrate solution. S4. Transfer the refined magnesium nitrate solution obtained in step S3 to a double decomposition reaction vessel, add potassium chloride, control the molar ratio of potassium chloride to magnesium nitrate to be 2.1:1, and carry out the double decomposition reaction at 85°C for 2 hours to generate a double decomposition reaction solution containing potassium nitrate and magnesium chloride. S5. The metathesis reaction solution obtained in step S4 is fed into a vacuum evaporation and concentration apparatus, and evaporated and concentrated at 70°C and a vacuum of 0.08 MPa until the solution density is 1.32 g / cm³. 3 Then, the concentrated metathesis reaction solution was cooled to 40°C at a cooling rate of 1.0°C / min, kept at this temperature and stirred for 1 hour, and then separated into solid and liquid phases using a centrifuge while still hot to obtain the first stage of crude potassium nitrate crystals and the first stage of mother liquor. The first stage of mother liquor was then cooled to 10°C at a cooling rate of 0.5°C / min, kept at this temperature and stirred for 2 hours, and then separated into solid and liquid phases using a centrifuge to obtain the second stage of crude potassium nitrate crystals and the second stage of mother liquor. The second stage of crude potassium nitrate crystals was returned to the metathesis reaction vessel in step S4 for redissolution. S6. The first stage of potassium nitrate crude crystals obtained in step S5 is sent into the washing system. A saturated potassium nitrate solution pre-cooled to 3°C is used as the washing liquid. Three-stage countercurrent pulping washing is performed. The total amount of washing liquid is 20% of the mass of the first stage of potassium nitrate crude crystals. After each stage of washing, the crystals are dehydrated by centrifuge until the crystal moisture content is ≤5%. The washed and dehydrated crystals are dried at 105°C to constant weight to obtain potassium nitrate product. S7. The first stage mother liquor obtained in step S5 is directly returned to the double decomposition reactor in step S4 for recycling. The second stage mother liquor obtained in step S5 is divided into two parallel processes: the first process returns 85% of the total volume of the second stage mother liquor to the double decomposition reactor in step S4 for recycling; the second process sends the remaining 15% of the volume of mother liquor to an evaporation and concentration device, heats and evaporates to remove some water. When the MgCl2 concentration in the mother liquor reaches 45wt%, the concentrate is transferred to a crystallization tank and cooled to room temperature for crystallization. Magnesium chloride hexahydrate crystals are obtained by centrifugation.

[0062] The potassium nitrate product obtained in this embodiment has a purity of 98.8 wt%, a chloride ion content of 0.01 wt%, no detected iron, and no water-insoluble matter, meeting the Class III standard requirements of GB / T 1918-2021 Industrial Potassium Nitrate.

[0063] Example 2

[0064] A method for preparing potassium nitrate from waste magnesium oxide from oriented silicon steel includes the following steps: S1. Waste magnesium oxide powder collected directly from the annealing process of oriented silicon steel was tested and found to contain 76.5 wt% MgO, 8.5 wt% SiO2, 4.2 wt% iron oxide (calculated as Fe2O3), and 9.2 wt% loss on ignition. The remainder consisted of unavoidable trace impurities. The waste magnesium oxide powder was crushed, ground, and passed through a 100-mesh sieve to obtain pretreated waste magnesium oxide. S2. Add the pretreated waste magnesium oxide obtained in S1 to a reactor containing 40wt% nitric acid, so that the amount of pretreated waste magnesium oxide and nitric acid fed is 1:2.25 in molar ratio of MgO to HNO3. Then, keep the temperature at 85℃ and stir continuously for 2.5h. After the reaction is completed, magnesium nitrate reaction solution is obtained. S3. The magnesium nitrate reaction solution obtained in step S2 is transferred to a plate and frame filter press for filtration, and the filtrate is collected. A 30 wt% hydrogen peroxide solution is added to the filtrate and stirred at 45°C for 30 min to oxidize the solution, thereby reducing the Fe content. 2+ Fully oxidized to Fe 3 + The amount of hydrogen peroxide solution added was 0.8 wt% of the total mass of the magnesium nitrate reaction solution; then magnesium hydroxide was added to the solution to adjust the pH to 4.8, so that Fe... 3+Hydrolysis produces Fe(OH)3 colloidal precipitate, which is then filtered again after standing for 25 minutes to remove the iron precipitate. The filtrate after iron removal is then subjected to final precision filtration through a 0.8 μm microporous precision filter to obtain a refined magnesium nitrate solution. S4. Transfer the refined magnesium nitrate solution obtained in step S3 to a double decomposition reaction vessel, add potassium chloride, control the molar ratio of potassium chloride to magnesium nitrate to be 2.15:1, and carry out the double decomposition reaction at 90°C for 1.5 hours to generate a double decomposition reaction solution containing potassium nitrate and magnesium chloride. S5. The metathesis reaction solution obtained in step S4 is fed into a vacuum evaporation and concentration apparatus, and evaporated and concentrated at 70°C and a vacuum of 0.09 MPa until the solution density is 1.35 g / cm³. 3 The concentrated metathesis reaction solution was then cooled to 38°C at a cooling rate of 1.2°C / min, kept at this temperature and stirred for 1.3 hours, and then separated into solid and liquid phases using a centrifuge while still hot to obtain the first stage of crude potassium nitrate crystals and the first stage of mother liquor. The first stage of mother liquor was then cooled to 8°C at a cooling rate of 0.6°C / min, kept at this temperature and stirred for 3 hours, and then separated into solid and liquid phases using a centrifuge to obtain the second stage of crude potassium nitrate crystals and the second stage of mother liquor. The second stage of crude potassium nitrate crystals was returned to the metathesis reaction vessel in step S4 for redissolution. S6. The first stage of potassium nitrate crude crystals obtained in step S5 is sent into the washing system. A saturated potassium nitrate solution pre-cooled to 1°C is used as the washing liquid for three-stage countercurrent pulping washing. The total amount of washing liquid used is 18% of the mass of the first stage of potassium nitrate crude crystals. After each stage of washing, the crystals are dehydrated by centrifuge until the crystal moisture content is ≤5%. The washed and dehydrated crystals are dried at 105°C to constant weight to obtain potassium nitrate product. S7. The first stage mother liquor obtained in step S5 is directly returned to the double decomposition reactor in step S4 for recycling. The second stage mother liquor obtained in step S5 is divided into two parallel processes: the first process returns 75% of the total volume of the second stage mother liquor to the double decomposition reactor in step S4 for recycling; the second process sends the remaining 25% of the volume of mother liquor to an evaporation and concentration device, heats and evaporates to remove some water. When the MgCl2 concentration in the mother liquor reaches 45wt%, the concentrate is transferred to a crystallization tank and cooled to room temperature for crystallization. Magnesium chloride hexahydrate crystals are obtained by centrifugation.

[0065] The potassium nitrate product obtained in this embodiment has a purity of 98.6 wt%, a chloride ion content of 0.01 wt%, no detected iron, and no water-insoluble matter, meeting the Class III standard requirements of GB / T 1918-2021 Industrial Potassium Nitrate.

[0066] Example 3

[0067] A method for preparing potassium nitrate from waste magnesium oxide from oriented silicon steel includes the following steps: S1. Waste magnesium oxide powder collected directly from the annealing process of oriented silicon steel was tested and found to contain 85.2 wt% MgO, 4.6 wt% SiO2, 2.8 wt% iron oxide (calculated as Fe2O3), and 6.5 wt% loss on ignition. The remainder consisted of unavoidable trace impurities. The waste magnesium oxide powder was crushed, ground, and passed through a 100-mesh sieve to obtain pretreated waste magnesium oxide. S2. Add the pretreated waste magnesium oxide obtained in S1 to a reactor containing 50wt% nitric acid, so that the amount of pretreated waste magnesium oxide and nitric acid fed is 1:2.05 in molar ratio of MgO to HNO3. Then, keep the temperature at 90℃ and stir continuously for 1.5h. After the reaction is completed, magnesium nitrate reaction solution is obtained. S3. The magnesium nitrate reaction solution obtained in step S2 is transferred to a plate and frame filter press for filtration, and the filtrate is collected. A 30 wt% hydrogen peroxide solution is added to the filtrate and stirred at 40°C for 45 min to oxidize the solution, thereby reducing the Fe content. 2+ Fully oxidized to Fe 3 + The amount of hydrogen peroxide solution added was 0.7 wt% of the total mass of the magnesium nitrate reaction solution; then magnesium oxide was added to the solution to adjust the pH to 4.5, so that Fe... 3+ Hydrolysis produces Fe(OH)3 colloidal precipitate, which is then filtered again after standing for 30 minutes to remove the iron precipitate. The filtrate after iron removal is then subjected to final precision filtration through a 0.5 μm microporous precision filter to obtain a refined magnesium nitrate solution. S4. Transfer the refined magnesium nitrate solution obtained in step S3 to a double decomposition reaction vessel, add potassium chloride, control the molar ratio of potassium chloride to magnesium nitrate to be 2.05:1, and carry out the double decomposition reaction at 80°C for 2.5 hours to generate a double decomposition reaction solution containing potassium nitrate and magnesium chloride. S5. The metathesis reaction solution obtained in step S4 is fed into a vacuum evaporation and concentration apparatus, and evaporated and concentrated to a solution density of 1.30 g / cm³ under conditions of 80°C and a vacuum of 0.085 MPa. 3 The concentrated metathesis reaction solution was then cooled to 45°C at a cooling rate of 0.8°C / min, kept at this temperature and stirred for 0.8 h, and then separated into solid and liquid phases using a centrifuge while still hot to obtain the first stage of crude potassium nitrate crystals and the first stage of mother liquor. The first stage of mother liquor was then cooled to 12°C at a cooling rate of 0.4°C / min, kept at this temperature and stirred for 2.5 h, and then separated into solid and liquid phases using a centrifuge to obtain the second stage of crude potassium nitrate crystals and the second stage of mother liquor. The second stage of crude potassium nitrate crystals was returned to the metathesis reaction vessel in step S4 for redissolution. S6. The first stage of potassium nitrate crude crystals obtained in step S5 is sent into the washing system. A saturated potassium nitrate solution pre-cooled to 3°C is used as the washing liquid for three-stage countercurrent pulping washing. The total amount of washing liquid is 25% of the mass of the first stage of potassium nitrate crude crystals. After each stage of washing, the crystals are dehydrated by centrifuge until the crystal moisture content is ≤5%. The washed and dehydrated crystals are dried at 105°C to constant weight to obtain potassium nitrate product. S7. The first stage mother liquor obtained in step S5 is directly returned to the double decomposition reactor in step S4 for recycling. The second stage mother liquor obtained in step S5 is divided into two parallel processes: the first process returns 90% of the total volume of the second stage mother liquor to the double decomposition reactor in step S4 for recycling; the second process sends the remaining 10% of the volume of mother liquor to an evaporation and concentration device, heats and evaporates to remove some water. When the MgCl2 concentration in the mother liquor reaches 45wt%, the concentrate is transferred to a crystallization tank and cooled to room temperature for crystallization. Magnesium chloride hexahydrate crystals are obtained by centrifugation.

[0068] The potassium nitrate product obtained in this embodiment has a purity of 98.7 wt%, a chloride ion content of 0.02 wt%, no detected iron, and no water-insoluble matter, meeting the Class III standard requirements of GB / T 1918-2021 Industrial Potassium Nitrate.

[0069] Comparative Example 1 The difference between this comparative example and Example 1 is that the oxidation and iron removal operation in step S3 is omitted, while the remaining operation steps and parameters are the same as in Example 1.

[0070] The potassium nitrate product obtained in this comparative example had a purity of 94.5 wt% and an iron content of 0.042 wt%, and its appearance was dark yellow. It failed to meet the Class III standard requirements of GB / T 1918-2021 Industrial Potassium Nitrate.

[0071] Comparative Example 2 The difference between this comparative example and Example 1 is that all the impurity removal operations in step S3 are omitted, while the remaining operation steps and parameters are the same as in Example 1.

[0072] The potassium nitrate product obtained in this comparative example had a purity of 91.8 wt%, an iron content of 0.068 wt%, a SiO2 content of 0.58 wt%, and a grayish-yellow appearance. It failed to meet the Class III standard requirements of GB / T 1918-2021 Industrial Potassium Nitrate.

[0073] In summary, this invention provides a method for preparing potassium nitrate from magnesium oxide waste from oriented silicon steel. This invention uses magnesium oxide waste from oriented silicon steel as a magnesium source for potassium nitrate production, replacing purchased high-purity magnesium oxide or magnesia. By implementing a systematic impurity removal treatment targeting the characteristics of impurities in the magnesium oxide waste after the acid neutralization reaction and before the metathesis reaction, the resulting potassium nitrate product meets industrial-grade standards. Simultaneously, it achieves high-value recovery and utilization of magnesium resources from the magnesium oxide waste from oriented silicon steel. This invention organically combines potassium nitrate production with the resource utilization of steel industry waste, reducing the cost of potassium nitrate raw materials while providing a high-value-added utilization pathway for magnesium oxide waste from oriented silicon steel. It has good economic and environmental benefits and is suitable for industrial-scale application.

[0074] The above description is merely a preferred embodiment of the present invention and does not limit the patent scope of the present invention. Any equivalent structural transformations made using the contents of the present invention under the inventive concept of the present invention, or direct / indirect applications in other related technical fields, are included within the patent protection scope of the present invention.

Claims

1. A method for preparing potassium nitrate from waste magnesium oxide from oriented silicon steel, characterized in that, Includes the following steps: Magnesium oxide waste from oriented silicon steel is neutralized with nitric acid to obtain a magnesium nitrate reaction solution; the magnesium nitrate reaction solution is then subjected to impurity removal treatment, which includes at least a solid-liquid separation step and an iron impurity removal step, to obtain a refined magnesium nitrate solution; the refined magnesium nitrate solution is then subjected to a metathesis reaction with potassium chloride to obtain a metathesis reaction solution containing potassium nitrate; the metathesis reaction solution is then cooled and crystallized to obtain potassium nitrate crystals; Specifically, the following steps are included: S1. Pre-treat the magnesium oxide waste from oriented silicon steel; S2. Neutralize the pretreated waste magnesium oxide with nitric acid to obtain magnesium nitrate reaction solution; S3. The magnesium nitrate reaction solution is subjected to a purification treatment, which includes a solid-liquid separation step and an iron impurity removal step to obtain a refined magnesium nitrate solution; the purification treatment also includes a precision filtration step. S4. The refined magnesium nitrate solution is subjected to a double decomposition reaction with potassium chloride to obtain a double decomposition reaction solution containing potassium nitrate and magnesium chloride. S5. The obtained double decomposition reaction solution is first evaporated and concentrated, then subjected to two-stage cooling crystallization, and solid-liquid separation is performed to obtain crude potassium nitrate crystals and mother liquor. S6. The crude potassium nitrate crystals are washed and dried to obtain potassium nitrate product; the purity of the potassium nitrate product is ≥98.5%, which meets the technical requirements of Class III products in GB / T 1918-2021 Industrial Potassium Nitrate; S7. Post-process the mother liquor obtained in step S5.

2. The method according to claim 1, characterized in that, In step S1, the pretreatment includes at least one of crushing, screening, washing, ultrasonic assistance, and slurry preparation.

3. The method according to claim 1, characterized in that, In step S2, the concentration of nitric acid is 30wt%~65wt%, the temperature of the neutralization reaction is 60~90℃, and the reaction time is 1~3h.

4. The method according to claim 1, characterized in that, In step S3, the solid-liquid separation is pressure filtration separation; The removal of iron impurities includes: adding an oxidant to oxidize and adjusting the pH of the magnesium nitrate reaction solution to 4.5-5, so that iron ions form hydroxide precipitates and are then removed by filtration. The oxidation conditions are: stirring at 30-60°C for 30-50 minutes, and the amount of oxidant added is 0.3-1.0% of the total mass of the magnesium nitrate reaction solution.

5. The method according to claim 1, characterized in that, In step S4, the molar ratio of potassium chloride to magnesium nitrate in the refined magnesium nitrate solution is (2.0~2.2):1, the temperature of the metathesis reaction is 60~100℃, and the reaction time is 1~3h.

6. The method according to claim 1, characterized in that, Specifically, S5 includes: The metathesis reaction solution obtained in step S4 is first evaporated and concentrated at 60-90℃ and a vacuum of 0.08-0.09 MPa to obtain a solution density of 1.30-1.35 g / cm³. 3 Then, the concentrated metathesis reaction solution was cooled to 35-45℃ at a cooling rate of 0.5-1.5℃ / min, and stirred for 0.5-1.5h. Solid-liquid separation was performed to obtain the first stage of crude potassium nitrate crystals and the first stage of mother liquor. The first stage of mother liquor was then cooled to 5-15℃ at a cooling rate of 0.3-1.0℃ / min, and stirred for 1-3h. Solid-liquid separation was performed to obtain the second stage of crude potassium nitrate crystals and the second stage of mother liquor. The first stage of crude potassium nitrate crystals directly enters step S6 for processing; the second stage of crude potassium nitrate crystals returns to the metathesis reaction in step S4 for redissolution, or enters step S6 after recrystallization.

7. The method according to claim 1, characterized in that, In step S7, the post-processing is as follows: the mother liquor obtained in step S5 is recycled back to the metathesis reaction in step S4, and / or the mother liquor obtained in step S5 is concentrated by evaporation and cooled to crystallize, so as to obtain magnesium chloride by-product.

8. A potassium nitrate product, characterized in that, It is prepared by the method described in any one of claims 1 to 7.