A method and apparatus for preparing nanoscale sheet-like alumina-based materials

By combining two-dimensional carbon nanomaterials with an aluminum source and using plasma-assisted air jet milling, the problem of nanofragmentation of high-toughness materials was solved, achieving low-energy consumption and high-efficiency preparation of nanoscale sheet-like alumina, which is suitable for large-scale production.

CN123105695APending Publication Date: 2026-11-17ZHONGHONG INNOVATION TECHNOLOGY (INNER MONGOLIA) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611482803.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-22
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies are insufficient to effectively break down high-toughness or high-hardness materials to the nanoscale. Furthermore, particles tend to agglomerate instantly during the crushing process, making it difficult to maintain monodispersity. Traditional processes are cumbersome and energy-intensive, making it difficult to meet the needs of large-scale production.

Method used

Two-dimensional carbon nanomaterials were combined with an aluminum source and subjected to plasma-assisted air jet milling. The two-dimensional structure of the two-dimensional carbon nanomaterials induced the aluminum source to grow into a sheet-like precursor. The template was removed during plasma treatment. Combined with plasma activation and multi-field coupling fragmentation of the carrier airflow, the agglomeration of nanoparticles was suppressed.

Benefits of technology

It enables materials to be crushed to the nanoscale at low temperatures, reducing energy consumption and ensuring that the materials have small particle size, narrow distribution, and good dispersibility, making them suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123105695A_ABST
    Figure CN123105695A_ABST
Patent Text Reader

Abstract

This application provides a method and apparatus system for preparing nanoscale sheet-like alumina-based materials. The preparation method includes: compositing an aluminum source with two-dimensional carbon nanomaterials to obtain a micron-sized composite precursor; and subjecting the composite precursor to plasma-assisted air jet milling to obtain sheet-like alumina-based materials. In this application, the two-dimensional carbon nanomaterials simultaneously serve as a nanoscale spatial template, a mechanically fragile interface, and an electric field coupling medium, jointly ensuring that the final nanoparticles possess comprehensive excellent properties such as small particle size, narrow distribution, good dispersibility, and high purity. Simultaneously, the plasma-assisted air jet milling process effectively breaks high-toughness or high-hardness materials down to the nanoscale, and also solves the problem of easy instantaneous particle agglomeration and difficulty in maintaining monodispersity during the crushing process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of alumina-based material preparation technology, and relates to a method and apparatus system for preparing nanoscale sheet-like alumina-based materials. Background Technology

[0002] Flaky alumina nanoparticles, especially γ-phase flaky alumina nanoparticles, have broad application prospects in catalyst supports, ceramic reinforcing phases, and adsorption separation due to their high specific surface area, excellent adsorption performance, and thermal stability. Currently, the main methods for preparing flaky alumina nanoparticles include the molten salt method (particle size distribution between 3 nm and 10 nm, thickness between 0.3 μm and 0.6 μm), the hydrothermal / solvothermal method (particle size distribution between 50 nm and 150 nm, thickness between 10 nm and 20 nm), and the solution-gel method (particle size distribution between 2 μm and 5 μm, thickness between 0.2 μm and 0.5 μm). These methods are relatively mature and simple, and the experimental conditions are easy to control, but the aspect ratio of the resulting nanomaterials is small. The template method, by introducing a template agent, can induce the directional growth of the aluminum source and optimize the aspect ratio of the material. However, existing template methods mostly use surfactants or hard templates (such as mesoporous silica). Template removal usually requires strong acid or strong alkali etching or high-temperature calcination, which is not only cumbersome but also easily introduces impurities and may even damage the morphology of the product.

[0003] In recent years, studies in the field of alumina preparation have used graphene oxide as a template to generate GO / Al(OH) through the hydrolysis of aluminum sources. x The precursor is then calcined at high temperature to remove the template, resulting in ultrathin γ-Al2O3 nanosheets with an extremely large specific surface area, fully leveraging their adsorption and catalytic properties. However, the calcination process is time-consuming, energy-intensive, produces a single product, has a limited template function, and is difficult to scale up for continuous production.

[0004] Furthermore, in the industrial preparation of nanomaterials, the degree of integration of the equipment system directly affects production efficiency and product quality. Carrier airflow milling technology utilizes compressed air or superheated steam, through ultra-fine nozzles or even Laval ring structures, to generate carrier airflow, causing material particles to be pulverized under high-speed collision and shearing. However, for tough materials that are initially at the micrometer scale, the pulverization limit is limited, making it difficult to consistently obtain particles smaller than 100nm. Traditional plasma technology generally uses high-temperature plasmas such as plasma torches and arc evaporation, vaporizing raw materials in plasma through high-temperature gas-phase synthesis, followed by rapid condensation and nucleation to grow nanomaterials or micromaterials. This process is simple and efficient, but the powder morphology and particle size distribution are wide, and it is prone to forming hard agglomerates. The batch process used in the preparation of sheet-like nano-alumina involves multiple independent unit operations, such as precursor synthesis, drying, calcination, and pulverization. This multi-step, multi-equipment process suffers from material transfer losses and contamination between steps, energy waste due to multiple heating and cooling cycles, and the difficulty of meeting the demands of large-scale production due to its batch operation. Summary of the Invention

[0005] To address the shortcomings of existing technologies, the purpose of this application is to provide a method and apparatus system for preparing nanoscale sheet-like alumina-based materials. The entire process is carried out at low temperatures, which solves the problem that traditional crushing processes cannot effectively crush high-toughness or high-hardness materials to the nanoscale, and that particles are prone to instantaneous agglomeration during the crushing process, making it difficult to maintain monodispersity.

[0006] To achieve this objective, the following technical solution is adopted in this application: In a first aspect, this application provides a method for preparing nanoscale sheet-like alumina-based materials, the method comprising: By combining an aluminum source with two-dimensional carbon nanomaterials, a micron-sized composite precursor is obtained. The composite precursor was subjected to plasma-assisted air jet milling to obtain a sheet-like alumina-based material.

[0007] This application introduces two-dimensional carbon nanomaterials and utilizes their two-dimensional structure to induce the directional growth of aluminum sources into sheet-like precursors, ensuring that the final nanoscale sheet-like alumina-based material possesses comprehensive superior properties such as small particle size, narrow distribution, good dispersibility, and high purity. At the same time, the two-dimensional carbon nanomaterials can act as sacrificial agents, being oxidized and burned to generate CO2 gas and removed in subsequent plasma treatment, eliminating the need for additional etching steps. Furthermore, plasma-assisted air jet milling achieves multi-field coupled nanoscale fragmentation, suppressing the instantaneous aggregation of nanoparticles and ensuring the monodispersity of the material.

[0008] As a preferred technical solution of this application, the mass ratio of the aluminum source to the two-dimensional carbon nanomaterial is (20~1000):1.

[0009] As one embodiment of this application, the aluminum source includes any one or a combination of at least two of aluminum nitrate, aluminum carbonate, aluminum sulfate, aluminum chlorate, and aluminum oxide.

[0010] As one embodiment of this application, the two-dimensional carbon nanomaterial includes any one or a combination of at least two of graphene, graphynylene, and nanographite sheets.

[0011] As a preferred technical solution of this application, the composite process includes: heating an aluminum source while simultaneously adding two-dimensional carbon nanomaterials in batches and dispersing them evenly to obtain a composite homogeneous hot slurry; subsequently, atomizing and pyrolyzing the slurry to obtain a solid porous composite precursor.

[0012] The temperature of the heat treatment is lower than the thermal decomposition temperature of the aluminum source.

[0013] The porous composite precursor D 50 ≤4.5μm.

[0014] As one embodiment of this application, the temperature of the heat treatment is 80℃~180℃.

[0015] The entire process of this application is a dry operation, with no solvent addition, no wastewater generation, and is environmentally friendly.

[0016] As a preferred technical solution of this application, the composite includes: uniformly dispersing an aluminum source and two-dimensional carbon nanomaterials in a solvent to form a composite material, followed by atomization pyrolysis to obtain a solid porous composite precursor.

[0017] The solvent includes any one or a combination of at least two of water, sodium dodecyl sulfate, and ammonia.

[0018] The porous composite precursor D 50 ≤6μm.

[0019] This application utilizes solvent dispersion of aluminum source and two-dimensional carbon nanomaterials, which has high uniformity, simple operation, and significantly reduces synthesis temperature, thereby reducing production energy consumption.

[0020] As a preferred technical solution of this application, the pressure of the atomization pyrolysis is 0.2MPa~0.5MPa.

[0021] As one embodiment of this application, the temperature of the atomization pyrolysis is 150℃~350℃.

[0022] This application introduces two-dimensional carbon nanomaterials and uses melt atomization pyrolysis or solution atomization pyrolysis to prepare brittle porous composite precursor materials, which greatly reduces the energy consumption of subsequent crushing.

[0023] As one embodiment of this application, the dispersion includes high-speed stirring and shearing.

[0024] As one embodiment of this application, the dispersion speed is 100rpm~300rpm and the dispersion time is 10min~30min.

[0025] As a preferred technical solution of this application, the plasma-assisted air jet milling process includes: Provide the first reactant gas and the second reactant gas; The first reactant gas is activated by plasma to form an activated gas stream; The second reactant gas forms a carrier gas flow through the nozzle of the air jet mill; In the crushing chamber, the composite precursor is carried by a carrier airflow and crushed by collision. At the same time, the activating airflow chemically activates the composite precursor to obtain nanoscale sheet-like alumina-based material.

[0026] As a preferred technical solution of this application, the preparation method further includes: accelerating the activated gas flow with a Laval ring and then introducing it into the crushing chamber.

[0027] As one embodiment of this application, the power of plasma activation is 2000W~3000W.

[0028] As one embodiment of this application, the first reactant gas and the second reactant gas each independently contain any one of an oxygen atmosphere, an inert atmosphere, or a reducing atmosphere.

[0029] As one embodiment of this application, the length of the sheet-like alumina-based material is 2μm~5μm and the thickness is 0.03μm~0.10μm.

[0030] Based on the multi-field coupling mechanism of plasma activation and high-speed crushing, the composite precursor is subjected to the synergistic effect of chemical activation field, high-speed flow field and mechanical impact field under controlled atmosphere to fully crush particles and obtain nanoscale powder.

[0031] In a second aspect, this application provides a preparation apparatus system for nanoscale sheet-like alumina-based materials. The preparation apparatus system is used for the preparation method described in the first aspect. The preparation apparatus system includes a precursor preparation device and an air jet mill-plasma coupling device connected in sequence. The air jet mill-plasma coupling device includes an air jet mill device and a plasma generator device. The air jet mill device is connected to the precursor preparation device and the plasma generator device respectively.

[0032] As a preferred embodiment of this application, the preparation apparatus system further includes a collection device, which is connected to the outlet end of the airflow mill-plasma coupling device.

[0033] As one embodiment of this application, the precursor preparation apparatus includes a spray decomposition furnace.

[0034] As one embodiment of this application, a Laval nozzle is provided between the air jet mill and the plasma generator.

[0035] This application integrates a plasma generator into an air jet mill, achieving multi-field coupling of the reactive gas activation field, plasma flow field, and mechanical impact field. Its design is reasonable, highly applicable, and can be used in the preparation of various types of ceramic matrix materials.

[0036] The system refers to an equipment system, device system, or production device.

[0037] Compared with the prior art, the beneficial effects of this application are as follows: (1) This application forms a brittle composite precursor by introducing two-dimensional carbon nanomaterials, and combines the activation and weakening effect of plasma to transform the difficult nano-pulverization into the brittle treatment of brittle materials, which greatly reduces the energy consumption of crushing and breaks through the crushing limit of traditional air jet mill. (2) This application utilizes plasma to provide in-situ charging and surface modification during the fragmentation process, and the carrier airflow provides high shear force. The two work together to effectively suppress the instantaneous aggregation of nanoparticles from both physical and chemical aspects, thus ensuring the monodispersity of the material. (3) This application integrates the plasma generator into the air jet mill, realizing the multi-field coupling of the reactive gas activation field, plasma flow field and mechanical impact field; at the same time, the active particles activated by the plasma produce a chemical etching effect on the material surface, reducing its fracture toughness, and co-occurs with the mechanical crushing effect of high-speed collision, significantly improving the crushing efficiency, and can directly crush high toughness or high hardness composite precursors to the nanoscale. Attached Figure Description

[0038] Figure 1 This is a schematic diagram of the structure of a device system for preparing sheet-like alumina-based materials according to a specific embodiment of this application.

[0039] Figure 2 This is a SEM characterization image of the nanoscale sheet-like alumina-based material provided in Example 1 of this application.

[0040] Figure 3 The image shows the SEM+NanoMeasurer1.2 analysis of the nanoscale sheet-like alumina-based material provided in Example 1 of this application.

[0041] Figure 4 The XRD pattern of the nanoscale sheet-like alumina-based material provided in Example 1 of this application (the horizontal axis is 2θ and the vertical axis is intensity).

[0042] Figure 5 EDS layering diagram of the nanoscale sheet-like alumina-based material provided in Example 2 of this application.

[0043] Figure 6 This is a distribution diagram of carbon element in the nanoscale sheet-like alumina-based material provided in Example 2 of this application.

[0044] Figure 7 This is a distribution diagram of the O element in the nanoscale sheet-like alumina-based material provided in Example 2 of this application.

[0045] Figure 8 This is a distribution diagram of Al element in the nanoscale sheet-like alumina-based material provided in Example 2 of this application.

[0046] Wherein, 1-crushing chamber; 2-powder inlet; 3-grading wheel; 4-microwave generator; 5-carrier airflow nozzle; 6-Laval nozzle; 7-extraction assembly; 8-tuner; 9-cyclone separator; 10-backflush port; 11-partition plate; 12-filter assembly; 13-extraction component; 14-first powder collection chamber; 15-second powder collector. Detailed Implementation

[0047] It should be understood that in the description of this application, the terms "first," "second," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Therefore, a feature defined with "first," "second," etc., may explicitly or implicitly include one or more of that feature. In the description of this application, unless otherwise stated, "multiple" or "several" means two or more.

[0048] It should be noted that, in the description of this application, unless otherwise expressly specified and limited, the terms "set up," "connected," and "linked" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection of two components. Those skilled in the art can understand the specific meaning of the above terms in this application based on the specific circumstances.

[0049] The scope of this application can be defined by lower and upper limits. The selected lower and upper limits define the boundaries of a specific range. The range defined in this way can be defined by the inclusion or exclusion of endpoints. Any endpoint can be independently selected for inclusion or exclusion, and all lower and upper limits can be arbitrarily combined to form new ranges. That is, any lower limit can be combined with any upper limit to form a valid range. For example, if the ranges of 60~120 and 80~110 are listed for specific parameters, it should be understood that the ranges of 60~110 and 80~120 also fall within the scope of this application. In addition, if the minimum range values ​​1 and 2 are listed, and the maximum range values ​​3, 4 and 5 are also listed, then all ranges of 1~3, 1~4, 1~5, 2~3, 2~4 and 2~5 fall within the scope of this application.

[0050] In this application, the order in which the steps are written in the methods described in the various embodiments does not imply a strict execution order. The actual execution order of each step should be determined according to its function and possible internal logic. Unless otherwise specified, all steps in this application can be executed in the order they are written, or in any order without technical conflict. For example, if the method includes steps (a) and (b), it means that the method may include steps (a) and (b) executed sequentially, or it may include steps (b) and (a) executed sequentially. If the method also includes step (c), then step (c) can be added to the method in any order without conflict, including but not limited to the execution order of steps (a), (b), and (c), steps (a), (c), and (b), steps (c), (a), and (b), etc.

[0051] The technical solution of this application will be further described below with reference to the accompanying drawings and specific embodiments.

[0052] In one specific embodiment, this application provides a method for preparing nanoscale sheet-like alumina-based materials, the preparation method comprising: Step 1: Combine the aluminum source with two-dimensional carbon nanomaterials to obtain a micron-sized composite precursor; Step 2: The composite precursor is subjected to plasma-assisted air jet milling to obtain a sheet-like alumina-based material.

[0053] In some embodiments, the mass ratio of the aluminum source to the two-dimensional carbon nanomaterial is (20~1000):1, for example, it can be 20:1, 25:1, 30:1, 35:1, 50:1, 100:1, 150:1, 200:1, 400:1, 500:1, 600:1, 800:1, 900:1 or 1000:1, but is not limited to the listed values. Other unlisted values ​​within this range are also applicable, preferably (50~200)1. This application controls the ratio of the two within the above range. On the one hand, it avoids that the content of the two-dimensional carbon nanomaterial is too high, which would lead to agglomeration, excessive viscosity, and difficulty in atomization. On the other hand, it prevents that the content of the two-dimensional carbon nanomaterial is too low, which would be detrimental to the construction of carbon nanocomposite precursor network.

[0054] In some embodiments, the aluminum source includes any one or a combination of at least two of aluminum nitrate, aluminum carbonate, aluminum sulfate, aluminum chlorate, and aluminum oxide. Typical but non-limiting combinations include: combinations of aluminum nitrate and aluminum carbonate, combinations of aluminum sulfate and aluminum oxide, combinations of aluminum sulfate and aluminum chlorate, combinations of aluminum carbonate and aluminum sulfate, and combinations of aluminum sulfate, aluminum chlorate, and aluminum oxide. Preferably, aluminum nitrate is used.

[0055] In some embodiments, the two-dimensional carbon nanomaterial includes any one or a combination of at least two of graphene, graphyne and nanographite sheets, wherein typical but non-limiting combinations include: a combination of graphene and graphyne, a combination of graphene, graphyne and nanographite sheets, a combination of graphene and nanographite sheets, a combination of graphyne and nanographite sheets, etc., preferably graphene.

[0056] In some embodiments, the two-dimensional carbon nanomaterial is a carbon nanomaterial with a two-dimensional sheet-like or standard sheet-like structure. The two-dimensional carbon nanomaterial serves as a nanoscale spatial template, utilizing its two-dimensional layered structure to achieve physical barrier and pore formation within a nanoscale confined space, restricting the migration and fusion of metal oxide grains. Simultaneously, the two-dimensional carbon nanomaterial acts as a mechanically fragile interface; due to the significant property differences (such as modulus and coefficient of thermal expansion) between the carbon nanomaterial and the matrix, numerous interfaces and defects are formed, and these locations become stress concentration points. Introducing these stress concentration points guides efficient fragmentation. Furthermore, the two-dimensional carbon nanomaterial can also serve as an electric field coupling medium, activating the reaction through field enhancement effects and promoting its own selective removal. Based on the synergistic effect of these three effects, the final nanoparticles possess excellent comprehensive characteristics: small particle size, narrow distribution, good dispersibility, and high purity. In this application, the two-dimensional carbon nanomaterial also forms a large effective contact area with the aluminum matrix, thereby constructing a bridging or network structure.

[0057] In some embodiments, in step one, the composite of the aluminum source and the two-dimensional carbon nanomaterial is performed using a melt atomization pyrolysis method, specifically including: S11: The aluminum source is heated and treated, and two-dimensional carbon nanomaterials are added in batches and dispersed evenly to obtain a composite homogeneous hot slurry.

[0058] The heating temperature is lower than the thermal decomposition temperature of the aluminum source. During the heating process, the aluminum source melts first to form a hot fluid material, thus preventing the aluminum salt from thermally decomposing.

[0059] In one embodiment, the heat treatment temperature is 80℃~180℃, for example, it can be 80℃, 90℃, 100℃, 110℃, 120℃, 130℃, 140℃, 150℃, 160℃, 170℃ or 180℃, but is not limited to the listed values, other unlisted values ​​within this range are also applicable. This application controls the heating temperature within the above range to avoid excessively high temperatures causing direct thermal decomposition into oxides. Oxides have a melting temperature of 2000℃ and strong mechanical properties, making them less likely to form nanosheet structures; at the same time, it avoids excessively low temperatures that would prevent melting and the formation of a hot slurry.

[0060] This application involves adding two-dimensional carbon nanomaterials in batches while stirring the hot fluid material, followed by continuous high-speed stirring and shearing until a uniform, stable, and visible agglomerate-free composite homogeneous hot slurry is formed.

[0061] In one implementation, the dispersion speed is 100 rpm to 300 rpm, for example, 100 rpm, 150 rpm, 200 rpm, 250 rpm, or 300 rpm, but is not limited to the listed values; other unlisted values ​​within this range are also applicable. The dispersion time is 10 min to 30 min, for example, 10 min, 15 min, 20 min, 25 min, or 30 min, but is not limited to the listed values; other unlisted values ​​within this range are also applicable.

[0062] S12: The composite homogeneous hot slurry is atomized and pyrolyzed to obtain a solid porous composite precursor.

[0063] The atomization pyrolysis process can be completed in a spray decomposition furnace.

[0064] In one implementation, the atomizing gas used in the atomization pyrolysis includes nitrogen and / or argon, and the pressure of the atomization pyrolysis is 0.2 MPa to 0.5 MPa, to atomize the composite homogeneous thermal slurry into micron-sized droplets. The pressure of the atomization pyrolysis can be 0.2 MPa, 0.25 MPa, 0.3 MPa, 0.35 MPa, 0.4 MPa, 0.45 MPa, or 0.5 MPa, but is not limited to the listed values; other unlisted values ​​within this range are also applicable.

[0065] In one implementation, the atomization pyrolysis temperature is 150℃~350℃, causing the material to decompose into solid powder and a mixed gas. The solid powder is a porous, brittle composite precursor, and the mixed gas contains any one or a combination of at least two of NO2, O2, H2O, and CO2 gases. The atomization pyrolysis temperature can be 150℃, 180℃, 200℃, 220℃, 250℃, 280℃, 300℃, 320℃, or 350℃, but is not limited to the listed values; other unlisted values ​​within this range are also applicable.

[0066] In one implementation method, before starting the atomization pyrolysis, the spray-type decomposition furnace needs to be preheated to the target atomization temperature. Then, a carrier gas with a flow rate of 2 L / min to 5 L / min is introduced, and the air is continuously purged for 10 to 30 minutes. Finally, the composite homogeneous hot slurry is transported into the decomposition furnace through an insulated pipeline. The flow rate of the carrier gas can be 2 L / min, 2.5 L / min, 3 L / min, 3.5 L / min, 4 L / min, 4.5 L / min, or 5 L / min, but is not limited to the listed values; other unlisted values ​​within this range are also applicable. The duration can be 10 minutes, 15 minutes, 20 minutes, 25 minutes, or 30 minutes, but is not limited to the listed values; other unlisted values ​​within this range are also applicable.

[0067] In some embodiments, in step one, the composite of the aluminum source and the two-dimensional carbon nanomaterial is performed using a solution atomization pyrolysis method, specifically including: S21: Aluminum source and two-dimensional carbon nanomaterials are uniformly dispersed in a solvent to form a composite material.

[0068] The solvent includes any one or a combination of at least two of water, sodium dodecyl sulfate, and ammonia.

[0069] As one implementation, the dispersion speed is 100 rpm to 300 rpm, for example, it can be 100 rpm, 150 rpm, 200 rpm, 250 rpm or 300 rpm, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0070] The dispersion time is 10 min to 30 min, for example, it can be 10 min, 15 min, 20 min, 25 min or 30 min, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable. The composite material is in solution or sol state.

[0071] S22: The composite material is atomized and pyrolyzed to obtain a solid porous composite precursor.

[0072] The atomization pyrolysis process can be completed in a spray decomposition furnace.

[0073] In one implementation, the atomizing gas used in the atomization pyrolysis includes nitrogen and / or argon, and the pressure of the atomization pyrolysis is 0.2 MPa to 0.5 MPa, to atomize the composite homogeneous thermal slurry into micron-sized droplets. The pressure of the atomization pyrolysis can be 0.2 MPa, 0.25 MPa, 0.3 MPa, 0.35 MPa, 0.4 MPa, 0.45 MPa, or 0.5 MPa, but is not limited to the listed values; other unlisted values ​​within this range are also applicable.

[0074] In one implementation, the atomization pyrolysis temperature is 150℃~350℃, causing the material to decompose into solid powder and a mixed gas. The solid powder is a porous, brittle composite precursor, and the mixed gas contains any one or a combination of at least two of the following gases: NO2, O2, H2O, and CO2. The atomization pyrolysis temperature can be 150℃, 180℃, 200℃, 220℃, 250℃, 280℃, 300℃, 320℃, or 350℃, but is not limited to the listed values; other unlisted values ​​within this range are also applicable.

[0075] In one implementation method, before starting the atomization pyrolysis, the spray-type decomposition furnace needs to be preheated to the target atomization temperature. Then, a carrier gas with a flow rate of 2 L / min to 5 L / min is introduced, and the air is continuously purged for 10 to 30 minutes. Finally, the composite homogeneous hot slurry is transported into the decomposition furnace through an insulated pipeline. The flow rate of the carrier gas can be 2 L / min, 2.5 L / min, 3 L / min, 3.5 L / min, 4 L / min, 4.5 L / min, or 5 L / min, but is not limited to the listed values; other values ​​within this range are also applicable. The duration can be 10 minutes, 15 minutes, 20 minutes, 25 minutes, or 30 minutes, but is not limited to the listed values; other values ​​within this range are also applicable.

[0076] In some embodiments, the plasma-assisted air jet milling process in step two includes the following specific methods: Provide the first reactant gas and the second reactant gas; The first reactant gas is activated by plasma to form an activated gas stream; The second reactant gas forms a carrier gas flow through the nozzle of the air jet mill; In the crushing chamber, the composite precursor is carried by a carrier airflow and crushed by collision. At the same time, the activating airflow chemically activates the composite precursor to obtain nanoscale sheet-like alumina-based material.

[0077] The first and second reactant gases are selected according to the target product requirements, and each independently contains any one of an oxygen atmosphere, an inert atmosphere, or a reducing atmosphere. When an oxygen-containing gas is used, the oxygen-active particles generated by plasma activation simultaneously oxidize and remove the exposed carbon nanomaterials in situ during particle breakage, directly obtaining alumina sheet-like nanomaterials. When a non-oxygen-active or inert gas is used, the plasma activates or dops the newly formed surface during the breakage process, obtaining a sheet-like alumina-based material composed of an aluminum source and two-dimensional carbon nanomaterials. The first and second reactant gases can be the same or different.

[0078] In some embodiments, the preparation method further includes: accelerating the activated gas flow using a Laval ring before introducing it into the crushing chamber. The first reactant gas is first activated by a plasma generator to form an activated gas flow containing active particles, and then accelerated through a Laval nozzle before entering the crushing chamber; while the carrier gas flow is directly introduced into the crushing chamber, and the composite precursor undergoes high-speed collisions under the carrying force of the carrier gas flow formed by the gas mill nozzle, while simultaneously being chemically etched by the active particles in the activated gas flow. Under the synergistic effect of mechanical collision and chemical activation, the solid porous composite precursor particles are broken into nanoscale powder.

[0079] In some embodiments, the first and second reactant gases are introduced into the crushing chamber via two separate paths. One path of the second reactant gas serves as the pulverizing gas, forming a carrier gas flow through the nozzle of the air jet mill, carrying the composite precursor particles for high-speed collision and crushing. The other path of the first reactant gas serves as the plasma working gas, generating active particles in situ through a plasma generator to act on the composite precursor particles. The pulverization process and the plasma treatment process are synchronized in time and space. The composite precursor particles are exposed to the plasma atmosphere at the moment of crushing, undergoing the synergistic effect of mechanical impact stress and plasma chemical etching or activation to form nanoscale powder.

[0080] In one implementation, the power of plasma activation is 2000W to 3000W, for example, it can be 2000W, 2100W, 2200W, 2300W, 2400W, 2500W, 2600W, 2700W, 2800W, 2850W, 2900W, 2950W or 3000W, but is not limited to the listed values, other unlisted values ​​within this range are also applicable.

[0081] In some embodiments, the length of the sheet-like alumina-based material is 2 μm to 5 μm, for example, it can be 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, or 5 μm, but is not limited to the listed values; other unlisted values ​​within this range are also applicable. The thickness of the sheet-like alumina-based material is 0.03 μm to 0.10 μm, for example, it can be 0.03 μm, 0.04 μm, 0.05 μm, 0.06 μm, 0.07 μm, 0.08 μm, 0.09 μm, or 0.10 μm, but is not limited to the listed values; other unlisted values ​​within this range are also applicable. By controlling the dimensions within the above range, this application effectively enhances the material's mechanical properties, improves toughness, and simultaneously improves the material's thermal conductivity and barrier properties.

[0082] In another specific embodiment, this application provides a preparation apparatus system for nanoscale sheet-like alumina-based materials, used in the preparation method described in one embodiment. The preparation apparatus system includes a precursor preparation device and an air jet mill-plasma coupling device connected sequentially. The precursor preparation device is used to composite an aluminum source with carbon nanomaterials to prepare a micron-sized particulate composite precursor. The air jet mill-plasma coupling device includes an air jet mill and a plasma generator. The air jet mill is connected to both the precursor preparation device and the plasma generator, and is used to drive the composite precursor particles to collide and break down at high speed, forming nanoscale powder materials.

[0083] In some embodiments, a Laval nozzle is provided between the air jet mill and the plasma generator to accelerate the activating gas, thereby creating a high-speed flow field within the crushing chamber.

[0084] In some embodiments, the precursor preparation apparatus includes a spray decomposition furnace, which comprises three stages: atomization, thermal decomposition, and collection. In the atomization stage, the material is dispersed into tiny droplets by an atomizer; the atomized droplets enter a high-temperature reaction chamber, where solvent evaporation, solute pyrolysis, and product sintering occur instantaneously to form a solid particulate product; the solid particulate product leaves the high-temperature zone with the airflow and undergoes gas-solid separation and collection.

[0085] In some implementations, such as Figure 1 As shown, the airflow mill includes a crushing chamber 1, with a powder inlet 2 at the top and a plasma generator connected to its bottom via a Laval nozzle 6. At least two carrier airflow nozzles 5 are circumferentially arranged on the outer peripheral wall of the crushing chamber 1 near the Laval nozzle 6; a discharge port is also provided on the side wall of the crushing chamber 1 near the powder inlet 2.

[0086] In one embodiment, the inner cavity of the air jet mill is also provided with a classifying wheel 3, which is located close to the powder feed inlet 2 to precisely control the particle size of the material.

[0087] In some embodiments, the plasma generating device includes a microwave generator 4, a circulator, a tuner 8, and an extraction assembly 7 connected sequentially, with the extraction assembly 7 connected to the Laval nozzle 6. Those skilled in the art will understand that the plasma generating device may also include necessary pipelines, conventional valves, general-purpose pumps, conventional electrical components, gas sources, gas distribution components, and cooling components for achieving process integrity. However, the above is not the main inventive point of this application, and those skilled in the art can add their own layout based on the process flow and equipment structure selection. This application does not make any special requirements or specific limitations in this regard.

[0088] The aforementioned air jet mill, as an ultrafine pulverizing device, can achieve material refinement and uniform mixing through carrier airflow, but it cannot achieve high-temperature crystallization treatment when used alone. While plasma reactors can provide a high-temperature, high-activity environment suitable for rapid phase transformation and surface modification of materials, their ability to control precursor morphology is limited when used alone. This application couples the two, achieving integrated pulverization and reaction, solving the problems of existing methods such as limited product types, difficulty in flexibly controlling product composition through a single process platform, and difficulty in achieving continuous production.

[0089] In some embodiments, the preparation apparatus system further includes a collection device connected to the outlet end of the air jet mill-plasma coupling device for collecting the crushed nanoparticles.

[0090] To help those skilled in the art better understand the overall technical solution and working process of this application, this application provides the following specific structure of the collection device by way of example: like Figure 1 As shown, the collection device includes a cyclone separator 9, a filter, and an extraction component 13. The cyclone separator 9 has a material inlet and a gas outlet. The material inlet is connected to the discharge port of the air jet mill, and the gas outlet is connected to the filter. A first powder collection chamber 14 is also provided at the bottom of the cyclone separator 9. The filter includes a chamber, which includes a discharge section, a filtration section, and a collection section connected sequentially from top to bottom. A partition plate 11 is provided between the discharge section and the filtration section, and a backflush port 10 is provided on the side wall of the chamber corresponding to the discharge section. A plurality of filter screen assemblies 12 are provided in the filtration section, and the plurality of filter screen assemblies 12 are arranged sequentially at intervals along the material movement direction. The collection section has a hollow structure and serves as a second powder collector 15. The chamber has a material inlet and a gas outlet. The material inlet is located near the collection section, and the gas outlet is connected to the discharge section. The material inlet is connected to the gas outlet of the cyclone separator 9, and the gas outlet is also connected to the extraction component 13. The air extraction component 13 includes, but is not limited to, a spiral air extraction pump.

[0091] Those skilled in the art should understand that this application also includes necessary pipelines, conventional valves and general pump equipment for achieving process integrity, but the above content is not the main inventive point of this application. Those skilled in the art can add layouts based on process flow and equipment structure selection, and this application does not make any special requirements or specific limitations in this regard.

[0092] It should be noted that the above description of the collection device does not constitute a further limitation on the scope of protection of this application. That is, the structure of other collection devices that have been disclosed in the prior art or not disclosed in the new technology can be used in this application. It is not limited to having the above structure. As long as the operating module can achieve the same or similar function, it can be arbitrarily replaced. The technical solution obtained after replacement also falls within the scope of protection and disclosure of this application.

[0093] For example, the method of using the airflow mill-plasma coupling device provided in this application includes: W1: Start the equipment and turn on the circulating cooling water, working gas (oxygen / air, flow rate of 1μL / min~30μL / min) and carrier gas, plasma generator power switch, air mill switch, freeze dryer switch in sequence. Set the fan frequency to 30Hz~50Hz and the classifier wheel frequency to 260Hz~300Hz. W2: Add the dry aluminum source and the composite precursor of two-dimensional carbon nanomaterials into the air jet mill. Start feeding after setting the feed voltage to 150V~200V and turn off the feed after feeding is completed. W3: Turn on the plasma generator, set the power to 2000W~3000W, and the working gas and carrier gas enter the crushing chamber for crushing after passing through the low-temperature plasma zone. W4: The device will be shut down after running for 15 to 20 minutes.

[0094] Example 1 This embodiment provides a method for preparing nanoscale sheet-like alumina-based materials, specifically including the following steps: (1) Weigh 5 kg of aluminum nitrate nonahydrate and heat it at 85°C. At the same time, slowly add 50 g of few-layer graphene powder in batches. Under high-speed shear dispersion, continue to disperse for 20 min to form a homogeneous hot slurry. (2) Preheat the decomposition furnace to the target temperature of 150°C, introduce high-purity nitrogen into the quartz tube at a flow rate of 4L / min, and replace the air for 20min; then transport the homogeneous hot slurry to the decomposition furnace through an insulated pipeline (below 80°C), turn on the atomizing nitrogen at a pressure of 0.3MPa, so that aluminum nitrate nonahydrate undergoes violent decomposition, producing a large amount of NO2 and O2 gas, which violently rushes out from the inside of the droplets, generating amorphous Al2O3, which is anchored on the graphene sheets and assembled together to form an Al2O3 / graphene composite precursor, whose D 50 ≤4.5μm; (3) 5 kg of Al2O3 / graphene composite precursor was fed into the air jet mill, and the plasma generator was turned on at the same time with the power set to 2400W. Oxygen was generated by forming a plasma-activated gas flow in the low-temperature plasma region and entered the crushing chamber. The high-speed nitrogen carrier gas flow of the air jet mill carried the Al2O3 / graphene composite precursor to collide and crush it. The plasma-activated gas flow chemically activated the composite precursor and the reaction continued for 20 min to obtain nanoscale sheet-like alumina-based material.

[0095] This application characterizes the nanoscale sheet-like alumina-based material obtained in Example 1 using SEM, and analyzes its particle morphology and XRD. The results are as follows: Figure 2 , Figure 3 and Figure 4 As shown. Figure 2The SEM image is magnified 2000 times. The material prepared in this embodiment exhibits a uniform lamellar structure with good dispersion between the lamellars. No obvious agglomeration or fusion was observed. The planar size of the lamellars is mainly distributed in the range of 2~5µm. Figure 3 The SEM image is at 10,000x magnification. The thickness of the material prepared in this embodiment was measured to be 0.03~0.10μm and the length was 2μm~5μm, as measured by Nano Measurer 1.2 software. Figure 4 The image shown is the XRD pattern of the material prepared in this embodiment, indicating that the crystal form is γ phase.

[0096] Example 2 This embodiment provides a method for preparing nanoscale sheet-like alumina-based materials, specifically including the following steps: (1) Weigh 5 kg of aluminum nitrate and heat it at 180°C. At the same time, slowly add 50 g of few-layer graphene powder in batches. Under high-speed shear dispersion, continue to disperse for 20 min to form a homogeneous hot slurry. (2) Preheat the decomposition furnace to the target temperature of 320°C, introduce high-purity nitrogen into the quartz tube at a flow rate of 5 L / min, and replace the air for 20 min; then transport the homogeneous hot slurry to the decomposition furnace through an insulated pipeline (below 110°C), turn on the atomizing nitrogen at a pressure of 0.5 MPa, causing aluminum nitrate to decompose violently, producing a large amount of NO2 and O2 gas, which violently rush out from the inside of the droplets, generating amorphous Al2O3, which is anchored on the graphene sheets and assembled together to form an Al2O3 / graphene composite precursor, whose D 50 ≤4.4μm; (3) 5 kg of Al2O3 / graphene composite precursor was fed into the air jet mill. At the same time, the plasma generator was turned on and the power was set to 2800W. Nitrogen gas was sent into the crushing chamber through the low-temperature plasma region to form a plasma activation gas flow. The high-speed nitrogen carrier gas flow of the air jet mill carried the Al2O3 / graphene composite precursor to collision crushing. The plasma activation gas flow chemically activated the composite precursor. The reaction continued for 15 min to obtain nanoscale sheet-like alumina-based material.

[0097] This application performs EDS analysis on the nanoscale sheet-like alumina-based material prepared in Example 2, and the results are as follows: Figure 5 , Figure 6 , Figure 7 and Figure 8 As shown. The material elements in this embodiment include C, Al, and O, and each element is uniformly distributed within the sheet region. Since the only carbon source in the precursor solution of this sample is graphene, it can be determined that the C element measured by EDS originates from the introduced graphene raw material.

[0098] Example 3 This embodiment provides a method for preparing nanoscale sheet-like alumina-based materials, specifically including the following steps: (1) Weigh 10 kg of aluminum nitrate nonahydrate and heat it at 200°C. At the same time, slowly add 50 g of few-layer graphene powder in batches and disperse it under high-speed shear dispersion for 30 min to form a homogeneous hot slurry. (2) Preheat the decomposition furnace to the target temperature of 150°C, introduce high-purity nitrogen into the quartz tube at a flow rate of 3L / min, and replace the air for 30min; then transport the homogeneous hot slurry to the decomposition furnace through an insulated pipeline (below 110°C), turn on the atomizing nitrogen at a pressure of 0.2MPa, causing aluminum nitrate to decompose violently, producing a large amount of NO2 and O2 gas, which violently rush out from the inside of the droplets, generating amorphous Al2O3, which is anchored on the graphene sheets and assembled together to form an Al2O3 / graphene composite precursor, whose D 50 ≤4.4μm; (3) 10 kg of Al2O3 / graphene composite precursor was fed into the air jet mill. At the same time, the plasma generator was turned on and the power was set to 2800W. Nitrogen gas was sent into the crushing chamber through the low-temperature plasma region to form a plasma activation gas flow. The high-speed nitrogen gas flow carried the Al2O3 / graphene composite precursor to collision crushing. The plasma activation gas flow chemically activated the composite precursor. The reaction continued for 18 min to obtain nanoscale sheet-like alumina-based material.

[0099] Example 4 This embodiment provides a method for preparing nanoscale sheet-like alumina-based materials, specifically including the following steps: (1) Weigh 5 kg of aluminum sulfate octadechydrate and heat it at 230°C. At the same time, slowly add 50 g of graphene powder in batches and disperse it under high-speed shear dispersion for 30 min to form a homogeneous hot slurry. (2) Preheat the decomposition furnace to the target temperature of 860°C, introduce high-purity nitrogen into the quartz tube at a flow rate of 4L / min, and replace the air for 15min; then transport the homogeneous hot slurry to the decomposition furnace through an insulated pipeline (below 300°C), turn on the atomizing nitrogen at a pressure of 0.3MPa, so that aluminum sulfate octadechydrate undergoes a thermal decomposition reaction, producing a large amount of H2O, SO3 and SO2 gases, which violently rush out from the inside of the droplets, generating amorphous Al2O3, which is anchored on the graphene sheets and assembled together to form an Al2O3 / graphene composite precursor, whose D 50 ≤4.2μm; (3) 5 kg of Al2O3 / graphene composite precursor was fed into the air jet mill. At the same time, the plasma generator was turned on and the power was set to 3000W. Oxygen was generated by forming a plasma activation gas flow in the low-temperature plasma region and entered the crushing chamber. The Al2O3 / graphene composite precursor was carried by the high-speed argon gas flow for collision crushing. The plasma activation gas flow chemically activated the composite precursor. The reaction continued for 18 min to obtain nanoscale sheet-like alumina-based material.

[0100] Example 5 This embodiment provides a method for preparing nanoscale sheet-like alumina-based materials, specifically including the following steps: (1) Weigh 5 kg of aluminum ammonium carbonate and heat it at 200°C. At the same time, slowly add 85 g of few-layer nano-graphite sheet powder in batches. Under high-speed shear dispersion, continue to disperse for 25 min to form a homogeneous hot slurry. (2) Preheat the decomposition furnace to the target temperature of 200°C, introduce high-purity nitrogen into the quartz tube at a flow rate of 4L / min, and replace the air for 15min; then transport the homogeneous hot slurry to the decomposition furnace through an insulated pipeline (below 200°C), turn on the atomizing nitrogen at a pressure of 0.25MPa, causing the aluminum ammonium carbonate to decompose violently, producing gases such as ammonia and carbon dioxide, which violently rush out from the inside of the droplets, generating amorphous Al2O3, which is anchored on the nano-graphite sheets and assembled together to form an Al2O3 / nano-graphite composite precursor, whose D 50 ≤4.5μm; (3) 5 kg of Al2O3 / nanographite sheet composite precursor was fed into the air jet mill device, and the plasma generator was turned on at the same time with the power set to 3000W. Oxygen was generated by forming plasma activation gas flow in the low temperature plasma region and entered the crushing chamber. The Al2O3 / nanographite sheet composite precursor was carried by high-speed argon gas flow for collision crushing. The plasma activation gas flow chemically activated the composite precursor and the reaction continued for 12 min to obtain nanoscale sheet alumina-based material.

[0101] Example 6 This embodiment provides a method for preparing nanoscale sheet-like alumina-based materials, specifically including the following steps: (1) Weigh 1.3g of sodium dodecyl sulfate (SDS), add it to 13L of deionized water, stir to dissolve, and obtain a 0.10g / L SDS aqueous solution. Then add 18g of graphene powder to the above SDS solution and sonicate (power 500~900W, time 30~120min) until a uniform black dispersion is formed. Slowly add 5kg of aluminum nitrate nonahydrate to the graphene dispersion, add deionized water, and bring the total volume of the solution to 22L. Then slowly add dilute ammonia water until the pH of the solution reaches 9.5~10.5; (2) Preheat the spray decomposition furnace to the target temperature of 450°C, introduce high-purity nitrogen into the quartz tube at a flow rate of 4L / min, and replace the air for 15min; then transport the prepared composite sol to the spray decomposition furnace through an insulated pipeline (below 100°C), turn on the atomizing nitrogen, and pressurize it to 0.25MPa, so that the composite sol droplets can quickly complete the solvent evaporation and nitrate decomposition at high temperature, producing NOx, H2O and other gases, which are violently ejected from the inside of the droplets, generating amorphous Al2O3, which is anchored on the graphene sheets and assembled together to form a graphene / alumina composite precursor, whose D 50 ≤6μm; (3) The graphene / alumina composite precursor is fed into the air jet mill, and the plasma generator is turned on at the same time. The power is set to 3000W. Oxygen enters the crushing chamber through the low-temperature plasma region to form a plasma-activated gas flow. The Al2O3 / nanographite sheet composite precursor is carried by the high-speed nitrogen gas flow for collision crushing. The plasma-activated gas flow chemically activates the composite precursor. The reaction continues for 12 minutes to obtain nanoscale sheet alumina-based material.

[0102] Example 7 This embodiment provides a method for preparing nanoscale sheet-like alumina-based materials. The difference from Example 1 is that the amount of graphene powder added is 2g, while the other materials and preparation process are the same as in Example 1.

[0103] In this embodiment, due to insufficient graphene addition, the alumina sheets were not adequately isolated and instead directly bonded by Al-O-Al chemical bonds. After plasma-assisted air jet milling, this chemical bonding significantly weakened the mechanical fragmentation effect. This resulted in incomplete sheet fragmentation, with most products remaining as irregular, interconnected aggregates, failing to fully dissociate into independent sheets.

[0104] Example 8 This embodiment provides a method for preparing nanoscale sheet-like alumina-based materials. The difference from Example 1 is that the amount of graphene powder added is 100g, while the other materials and preparation process are the same as in Example 1.

[0105] In this embodiment, the excessive amount of graphene added to the sheet-like alumina-based material significantly reduces the dispersibility of the graphene itself, making it prone to aggregation. At the same time, the excessive amount of graphene will also increase the purification load in the subsequent removal process, increasing the risk of residual carbon impurities.

[0106] Comparative Example 1 This comparative example provides a method for preparing nanoscale sheet-like alumina-based materials. The difference from Example 1 is that aluminum nitrate nonahydrate is not combined with graphene powder, while the other materials and preparation process are the same as in Example 1.

[0107] The comparative example, lacking the introduction of two-dimensional carbon nanomaterials, exhibited a wider particle size distribution and poorer dispersibility. In contrast, the two-dimensional carbon nanomaterials introduced in Example 1, with their two-dimensional layered structure, effectively induced the aluminum source to form a sheet-like morphology, and the abundant oxygen-containing functional groups on their surface facilitated uniform loading of the aluminum source. Simultaneously, the two-dimensional carbon nanomaterials achieved physical barrier and pore formation within a nanoscale confinement space, limiting the migration and fusion of metal oxide grains, reducing particle agglomeration, and guiding efficient fragmentation by introducing stress concentration points, thereby reducing powder particle size. Furthermore, the field-enhanced effect activated the reaction and promoted selective removal, ensuring high material purity.

[0108] Comparative Example 2 This comparative example provides a method for preparing nanoscale sheet-like alumina-based materials. The difference from Example 1 is that in step (3), 5 kg of Al2O3 / graphene composite precursor is fed into an air jet mill for conventional air jet milling and is not activated by plasma. The other materials and preparation process are the same as in Example 1.

[0109] Compared to Example 1, the crushing capacity of this comparative example is limited, mainly because the single air jet mill crushing relies solely on kinetic energy impact, resulting in a high lower limit for material crushing and difficulty in reaching the nanoscale. Furthermore, the newly generated nanoparticles during the crushing process have extremely high surface energy and lack an effective in-situ dispersion mechanism, leading to rapid particle re-agglomeration and a wide particle size distribution in the product.

[0110] Comparative Example 3 This comparative example provides a method for preparing nanoscale sheet-like alumina-based materials. The difference from Example 1 is that the composite precursor is broken down using traditional plasma technology, but air jet milling is not combined with the process. The other materials and preparation process are the same as in Example 1.

[0111] This comparative example uses a single plasma technology, which requires the temperature to reach the gasification temperature of the raw material to rapidly condense and nucleate. The products are mostly spherical or shell-shaped, with a wide morphology and particle size distribution, and are prone to forming hard agglomerates. Example 1, however, designs a brittle composite precursor and uses pulverization instead of synthesis. The structure of the precursor determines the porous, sheet-like complex structure of the final product, thus obtaining nanoscale sheet materials that meet the requirements.

[0112] Comparative Example 4 This comparative example provides a method for preparing nanoscale sheet-like alumina-based materials, using graphene oxide templates to prepare γ-Al2O3 nanosheet materials.

[0113] In this comparative example, the removal efficiency of the graphene oxide template was low, mainly relying on long-term calcination in a muffle furnace, resulting in high energy consumption and long processing time. The entire process involves separate steps such as precursor preparation, drying, and calcination, making continuous production difficult and failing to fully utilize atmosphere control to achieve product diversification.

[0114] The applicant declares that the above description is only a specific implementation of this application, but the protection scope of this application is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in this application fall within the protection and disclosure scope of this application.

Claims

1. A method for preparing a nanoscale sheet-like alumina-based material, characterized in that, The preparation method includes: By combining an aluminum source with two-dimensional carbon nanomaterials, a micron-sized composite precursor is obtained. The composite precursor was subjected to plasma-assisted air jet milling to obtain a sheet-like alumina-based material.

2. The preparation method according to claim 1, characterized in that, The mass ratio of the aluminum source to the two-dimensional carbon nanomaterial is (20~1000):1; And / or, the aluminum source includes any one or a combination of at least two of aluminum nitrate, aluminum carbonate, aluminum sulfate, aluminum chlorate and aluminum oxide.

3. The preparation method according to claim 1, characterized in that, The two-dimensional carbon nanomaterials include any one or a combination of at least two of graphene, graphynylene, and nanographite sheets.

4. The preparation method according to any one of claims 1-3, characterized in that, The composite includes: Aluminum source is heated and treated, and two-dimensional carbon nanomaterials are added in batches and dispersed evenly to obtain a composite homogeneous hot slurry; then atomized pyrolysis is performed to obtain a solid porous composite precursor. The temperature of the heat treatment is lower than the thermal decomposition temperature of the aluminum source; The porous composite precursor D 50 ≤4.5μm.

5. The preparation method according to any one of claims 1-3, characterized in that, The composite includes: An aluminum source and two-dimensional carbon nanomaterials are uniformly dispersed in a solvent to form a composite material, which is then atomized and pyrolyzed to obtain a solid porous composite precursor. The solvent includes any one or a combination of at least two of water, sodium dodecyl sulfate, and ammonia. The porous composite precursor D 50 ≤6μm.

6. The preparation method according to claim 4 or 5, characterized in that, The pressure of the atomization pyrolysis is 0.2 MPa to 0.5 MPa; And / or, the temperature of the atomization pyrolysis is 150℃~350℃; And / or, the dispersion includes high-speed stirring and shearing; And / or, the dispersion speed is 100 rpm to 300 rpm, and the dispersion time is 10 min to 30 min.

7. The preparation method according to any one of claims 1-3, characterized in that, The plasma-assisted air jet milling process includes: Provide the first reactant gas and the second reactant gas; The first reactant gas is activated by plasma to form an activated gas stream; The second reactant gas forms a carrier gas flow through the nozzle of the air jet mill; In the crushing chamber, the composite precursor is carried by a carrier airflow and crushed by collision. At the same time, the activating airflow chemically activates the composite precursor to obtain nanoscale sheet-like alumina-based material.

8. The preparation method according to claim 7, characterized in that, The preparation method further includes: accelerating the activated gas flow with a Laval ring before introducing it into the crushing chamber; And / or, the power of plasma activation is 2000W~3000W; And / or, the first reactant gas and the second reactant gas each independently contain any one of an oxygen atmosphere, an inert atmosphere, or a reducing atmosphere; And / or, the length of the sheet-like alumina-based material is 2μm~5μm and the thickness is 0.03μm~0.10μm.

9. A device system for preparing nanoscale sheet-like alumina-based materials, characterized in that, The preparation apparatus system is used in the preparation method according to any one of claims 1-8, and the preparation apparatus system includes a precursor preparation device and an air jet mill-plasma coupling device connected in sequence. The aforementioned air jet mill-plasma coupling device includes an air jet mill device and a plasma generator; The air jet mill is connected to the precursor preparation device and the plasma generator, respectively.

10. The preparation apparatus system according to claim 9, characterized in that, The preparation apparatus system further includes a collection device, which is connected to the outlet end of the air jet mill-plasma coupling device; And / or, the precursor preparation apparatus includes a spray decomposition furnace; And / or, a Laval nozzle is provided between the air jet mill and the plasma generator.