A method for the co-digestion of titanium-containing blast furnace slag to produce hydrochloric acid and chlorine as byproducts

By treating titanium-containing blast furnace slag with impregnation, boiling hydrolysis, and molten salt chlorination, the problem of hydrochloric acid and chlorine disposal in the production of metallic magnesium from salt lakes has been solved, achieving efficient utilization of resources and production of high-end titanium products, while reducing production costs.

CN123105707APending Publication Date: 2026-11-17QINGHAI SALT LAKE IND +2
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611255480.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing technologies, the disposal of hydrochloric acid and chlorine, byproducts of magnesium production from salt lakes, is a challenge. Traditional alkaline absorption methods consume large amounts of resources, and the resource utilization efficiency of titanium-containing blast furnace slag is low, resulting in high production costs and serious resource waste.

Method used

Titanium-containing blast furnace slag is mixed with hydrochloric acid solution and impregnated, followed by boiling hydrolysis and drying to obtain titanium-enriched slag. Then, it undergoes molten salt chlorination reaction with molten salt and calcined petroleum coke to generate titanium tetrachloride, thus achieving the synergistic digestion of hydrochloric acid and chlorine.

Benefits of technology

It has achieved efficient treatment of hydrochloric acid and chlorine, improved the grade of titanium resources, produced key raw materials for high-end sponge titanium and chloride process titanium dioxide, reduced production costs, and made resource-efficient use of titanium-containing blast furnace slag.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This invention relates to the field of titanium-containing blast furnace slag treatment, specifically disclosing a method for the synergistic digestion of titanium-containing blast furnace slag to produce hydrochloric acid and chlorine as byproducts. The method includes: 1) mixing titanium-containing blast furnace slag with a hydrochloric acid solution and then impregnating the mixture to obtain a leaching slurry; the solid-liquid ratio of the titanium-containing blast furnace slag to the hydrochloric acid solution is 1g:5~15mL; 2) subjecting the leaching slurry to boiling hydrolysis, filtering the resulting reaction products, washing the resulting filter residue with water, and then drying it at 450~650℃ to obtain titanium-enriched slag with a TiO2 content greater than or equal to 55wt%; 3) subjecting the titanium-enriched slag to a molten salt chlorination reaction with molten salt, calcined petroleum coke, and chlorine; 4) sequentially collecting dust and condensing the gaseous products generated during the molten salt chlorination reaction to obtain titanium tetrachloride. This invention utilizes waste to treat waste, achieving the resource utilization of titanium-containing blast furnace slag from ironmaking.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of titanium-containing blast furnace slag treatment, and specifically to a method for the synergistic digestion of titanium-containing blast furnace slag to produce hydrochloric acid and chlorine as byproducts. Background Technology

[0002] Chlorine disposal has always been a core bottleneck restricting the large-scale and sustainable development of magnesium resources in salt lakes. Chlorine treatment costs (including safety, environmental protection, conversion, storage, and transportation) account for a high proportion of magnesium production costs, even becoming a decisive factor. Inefficient or high-cost disposal methods such as producing PVC, liquid chlorine, hydrochloric acid, or hypochlorite severely weaken the market competitiveness of magnesium. Simultaneously, during the production of magnesium in salt lakes, different processes generate a certain amount of low-concentration hydrochloric acid, requiring neutralization with expensive alkali solutions, further increasing the production cost. Titanium-containing blast furnace slag is a byproduct of vanadium-titanium magnetite ironmaking. During blast furnace smelting, almost all the titanium in the concentrate enters the slag, with TiO2 content ranging from 5% to 30%. Blast furnace slag with a grade below 15% is mainly used as building materials, while blast furnace slag with a grade above 20% cannot directly meet the production needs of building materials, and its TiO2 content is too low as a raw material for titanium extraction. The titanium content in my country's titanium-containing blast furnace slag is generally high, and it is currently accumulating in slag yards at an increase of nearly 4 million tons per year. This not only wastes titanium resources but also increases environmental pressure.

[0003] Chinese patent application CN105217664A discloses a method for treating and utilizing waste acid from titanium-containing blast furnace slag. This method mainly involves ball milling and leaching titanium-containing blast furnace slag with waste dilute sulfuric acid, separating the filter residue and the leachate. After controlling the equivalent concentration of TiO2 in the leachate through reduced pressure evaporation, an oxidative hydrolysis reaction is carried out. The hydrolysis product is filtered, washed, and dried to obtain a metatitanic acid-silicic acid composite. Tungsten is further loaded onto this composite, and after calcination, titanium-tungsten silicon powder is obtained. The ball-milled filter residue undergoes simple suspension separation, drying, and calcination to obtain calcium sulfate-SiO2 composite whisker material. The hydrolyzed liquid can be crystallized and separated to obtain aluminum sulfate chemicals. Chinese patent application CN103966455A discloses an aluminothermic process for extracting titanium from titanium-containing blast furnace slag, employing carbothermic reduction, acid leaching, and alkali calcination steps to obtain relatively pure TiC. This process can effectively separate and enrich titanium elements in titanium-containing blast furnace slag. Chinese patent application CN103952567A discloses a method for recovering titanium, silicon, aluminum, calcium, and magnesium through multi-stage acid leaching. This method utilizes acid leaching, particularly multi-stage acid leaching, to extract and separate useful metals such as titanium, aluminum, calcium, and magnesium. However, the aforementioned methods involve complex processes and require stringent separation and purification procedures, resulting in high energy consumption and costs during the extraction process. Summary of the Invention

[0004] To address the problems of high costs and difficulties in disposing of chlorine / acid byproducts from existing salt lakes, inefficient storage and limited resource utilization of titanium-containing blast furnace slag, and high energy consumption and costs of existing treatment processes, this invention provides a method for the co-digestion of titanium-containing blast furnace slag as a byproduct of hydrochloric acid and chlorine. This method can safely and efficiently dispose of hydrochloric acid and chlorine byproducts of magnesium metal from salt lakes, fundamentally avoiding the drawbacks of traditional alkaline absorption methods, which consume large amounts of resources and can only produce low-value-added chemical products. At the same time, it produces titanium tetrachloride through molten salt chlorination reaction, providing a key raw material for the production of high-end sponge titanium and chloride-process titanium dioxide.

[0005] To achieve the above objectives, this invention provides a method for the co-digestion of titanium-containing blast furnace slag to produce hydrochloric acid and chlorine as byproducts, comprising the following steps: 1) mixing titanium-containing blast furnace slag with hydrochloric acid solution and then impregnating the mixture to obtain a leachate slurry; the solid-liquid ratio of titanium-containing blast furnace slag to hydrochloric acid solution is 1g:5~15mL; 2) subjecting the leachate slurry to boiling hydrolysis, filtering the resulting reaction product, washing the resulting filter residue with water, and then drying it at 450~650℃ to obtain enriched titanium slag with a TiO2 content greater than or equal to 55wt%; 3) subjecting the enriched titanium slag to molten salt, calcined petroleum coke, and chlorine for molten salt chlorination reaction, wherein the mass ratio of molten salt, enriched titanium slag, and calcined petroleum coke is 100:5~7:2~5, and the amount of chlorine used is 200~500mL / min relative to 20g of titanium-containing blast furnace slag; 4) sequentially collecting dust and condensing the gaseous products generated during the molten salt chlorination reaction to obtain titanium tetrachloride product.

[0006] Preferably, the TiO2 content in the titanium-containing blast furnace slag is greater than 18 wt%, and more preferably 19 to 25 wt%.

[0007] Preferably, the water content in the titanium-containing blast furnace slag is less than or equal to 5 wt%.

[0008] Preferably, in step 1), the concentration of the hydrochloric acid solution is 5~30wt%.

[0009] Preferably, in step 1), the impregnation treatment is carried out under stirring, with a stirring speed of 300~500 r / min, a time of 1~3 h, and a temperature of 15~90℃.

[0010] Preferably, in step 2), the boiling hydrolysis temperature is 90~130℃.

[0011] Preferably, in step 2), the method further includes: mixing the filtrate collected during the filtration process with the washing liquid generated during the water washing process to obtain a mixture, then adding calcium oxide to the mixture to adjust the pH value of the mixture to 6.5~7, and then sequentially evaporating, concentrating and crystallizing to obtain calcium magnesium complex chloride.

[0012] Preferably, in step 2), the washing process includes a first wash, a second wash, and a third wash performed sequentially. The washing liquid obtained from the first wash is mixed with the filtrate obtained from filtration. The washing liquid obtained from the second wash is returned to the first wash. The third wash uses fresh water for washing, and the washing liquid obtained from the third wash is returned to the second wash.

[0013] Preferably, in step 2), the drying temperature is 500~600℃ and the time is 1~5h.

[0014] Preferably, in step 2), the TiO2 content in the enriched titanium slag is 55~65wt%.

[0015] Preferably, the molten salt is sodium chloride and / or potassium chloride.

[0016] Preferably, in step 3), the temperature of the molten salt chlorination reaction is 900~1100℃ and the time is 1.5~2h.

[0017] Compared with the prior art, the present invention has the following advantages:

[0018] 1. This invention addresses the challenge of disposing of hydrochloric acid and chlorine, byproducts of magnesium production in salt lakes, by proposing a resource recovery method that utilizes titanium-containing blast furnace slag for synergistic digestion. This method not only safely and efficiently disposes of hydrochloric acid and chlorine byproducts of magnesium production in salt lakes, but also fundamentally avoids the drawbacks of traditional alkaline absorption methods, which consume large amounts of resources and can only produce low-value-added chemical products.

[0019] 2. This invention utilizes titanium-containing blast furnace slag to synergistically absorb hydrochloric acid and chlorine. Hydrochloric acid is used to leach soluble impurities from the slag, increasing the TiO2 content and producing enriched titanium slag. This enriched titanium slag is then chlorinated using a molten salt chlorination process to produce titanium tetrachloride, a key raw material for the subsequent production of high-end sponge titanium and chloride-process titanium dioxide. The entire process treats waste with waste, achieving resource-based upgrading of slag and hazardous waste. Detailed Implementation

[0020] The following provides a detailed description of specific embodiments of the present invention. It should be understood that the specific embodiments described herein are for illustrative and explanatory purposes only and are not intended to limit the scope of the invention.

[0021] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0022] In the description of this application, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating relative importance or implying the number of technical features indicated. Therefore, unless otherwise stated, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature; "multiple" means two or more. The term "comprising" and any variations thereof mean non-exclusive inclusion, where one or more other features, integers, steps, operations, units, components, and / or combinations thereof may be present or added.

[0023] The method for co-digesting titanium-containing blast furnace slag to produce hydrochloric acid and chlorine byproducts according to the present invention includes the following steps: 1) Mixing titanium-containing blast furnace slag with hydrochloric acid solution and then impregnating it to obtain a leaching slurry; the solid-liquid ratio of titanium-containing blast furnace slag to hydrochloric acid solution is 1g:5~15mL; 2) Boiling hydrolysis of the leaching slurry, filtering the obtained reaction product, washing the obtained filter residue with water, and then drying it at 450~650℃ to obtain enriched titanium slag with TiO2 content greater than or equal to 55wt%; 3) Performing a molten salt chlorination reaction with molten salt, calcined petroleum coke and chlorine, wherein the mass ratio of molten salt, enriched titanium slag and calcined petroleum coke is 100:5~7:2~5, and the amount of chlorine used is 200~500mL / min relative to 20g of titanium-containing blast furnace slag; 4) Collecting dust and condensing the gaseous products generated during the molten salt chlorination reaction to obtain titanium tetrachloride product.

[0024] The treatment of titanium-containing blast furnace slag involved in this invention is mainly for titanium-containing blast furnace slag with a TiO2 content greater than 18 wt%, preferably 19-25 wt%.

[0025] In the method of the present invention, titanium-containing blast furnace slag can be obtained by rapidly cooling the titanium-rich industrial waste slag produced during the ironmaking process of vanadium-titanium magnetite, followed by drying.

[0026] In some embodiments, the titanium-containing blast furnace slag contains 19-25 wt% TiO2, 20-25 wt% CaO, and 15-23 wt% SiO2.

[0027] In some embodiments, the moisture content of the dried titanium-containing blast furnace slag is preferably controlled to below 5 wt%.

[0028] In the method of this invention, the hydrochloric acid solution can be a prepared hydrochloric acid solution or a hydrochloric acid solution generated during industrial production, such as a hydrochloric acid solution produced as a byproduct of the HCl synthesis tail gas treatment process in a salt lake PVC plant. The concentration of the hydrochloric acid solution can be 5~30wt%, preferably 15~28wt%.

[0029] In this invention, titanium-containing blast furnace slag is impregnated with hydrochloric acid solution at room temperature. The resulting leaching slurry exhibits CaO and MgO leaching rates exceeding 95%, and Fe₂O₃ leaching rate exceeding 87%. To achieve the aforementioned impurity removal effect, the solid-liquid ratio of the titanium-containing blast furnace slag to the hydrochloric acid solution is 1g:5~15mL, preferably 1g:5~10mL.

[0030] The impregnation treatment of the present invention can be carried out under stirring, with a stirring speed of 300~500 r / min, a time of 1~3 h, and a temperature of 15~40℃.

[0031] In this invention, boiling hydrolysis can be carried out at 90-130°C, and is completed when the pH value rises to 5-6. Directly subjecting the leachate obtained after impregnation treatment to boiling hydrolysis enables efficient separation of titanium components.

[0032] After boiling hydrolysis, the solution is filtered to obtain filter residue and filtrate. The filter residue is washed with water and then dried at 450~650℃, preferably 500~600℃, for 1~5 hours to obtain enriched titanium slag with a TiO2 content of greater than or equal to 55wt%, preferably 55~65wt%. The obtained filtrate can be mixed with calcium oxide to neutralize the residual hydrochloric acid, resulting in neutralized filtrate, which can be directly returned to the salt pond for evaporation, concentration, and crystallization to obtain calcium-magnesium composite chloride.

[0033] In this invention, the filter residue can be washed using a countercurrent washing method, and can be performed three times, i.e., the filter residue is washed sequentially with a first water wash, a second water wash, and a third water wash. To save on washing costs, the third water wash uses fresh deionized water, and the resulting washing liquid is returned to the second water wash as washing water. The washing liquid obtained from the second water wash is returned to the first water wash as washing water. The washing liquid obtained from the first water wash can be mixed with the filtrate and then neutralized with calcium oxide before finally being sent to the salt drying pond.

[0034] In the method of the present invention, the calcined petroleum coke is the product of petroleum coke calcined at a high temperature of 1000~1350℃. The main component of the calcined petroleum coke is carbon, the volatile matter content is less than 0.5wt%, and the moisture content is less than 0.5wt%.

[0035] In some embodiments, the calcined petroleum coke has a carbon content of 98.9 wt%, a moisture content of 0.4 wt%, a sulfur content of 0.3 wt%, and other contents of 0.4 wt%.

[0036] In the method of this invention, the chlorine gas can be a byproduct of the HCl synthesis tail gas treatment process in a salt lake PVC plant. The concentration of the chlorine gas can be 93~98.5 vol%.

[0037] In this invention, the enriched titanium slag is further mixed with molten salt, calcined petroleum coke, and chlorine gas to undergo a molten salt chlorination reaction. The reaction temperature of the molten salt chlorination reaction can be 900~1100℃, preferably 950~1000℃, and the reaction time is 1.5~2h, preferably 1.6~1.8h.

[0038] In the molten salt chlorination reaction of this invention, the mass ratio of molten salt, enriched titanium slag and calcined petroleum coke is 100:5~7:2~5, preferably 100:6~6.5:2~2.5.

[0039] In the above-mentioned molten salt chlorination reaction, the molten salt is generally sodium chloride and / or potassium chloride. To further reduce production costs, a mixture of sodium chloride and potassium chloride can be selected as the molten salt, wherein the mass ratio of sodium chloride to potassium chloride is 1:0.1~0.15.

[0040] In the molten salt chlorination reaction of the present invention, the amount of chlorine gas used is 200~500mL / min relative to 20g of titanium-containing blast furnace slag, preferably 300~450mL / min.

[0041] In this invention, the crude titanium tetrachloride product obtained has a TiCl4 content of over 98.7%, and after further refining, it can be used as a key raw material for high-end sponge titanium and chloride-process titanium dioxide.

[0042] The following examples further illustrate the method for the co-digestion of titanium-containing blast furnace slag to produce hydrochloric acid and chlorine as byproducts of the present invention. These examples are implemented based on the technical solution of the present invention, providing detailed implementation methods and specific operating procedures; however, the scope of protection of the present invention is not limited to the following examples.

[0043] Unless otherwise specified, the experimental methods used in the following embodiments are conventional methods in the art. Unless otherwise specified, the experimental materials used in the following embodiments are commercially available.

[0044] In some embodiments and comparative examples, the calcined petroleum coke used was purchased from Shandong Yixing Carbon New Materials Co., Ltd., and its physicochemical parameters are shown in Table 1.

[0045] Table 1

[0046]

[0047] Example 1

[0048] The specific steps for preparing titanium tetrachloride are as follows:

[0049] 1) 20g of titanium-containing blast furnace slag with a water content of less than 5wt% (from water-quenched slag produced by blast furnace ironmaking, in which the content of TiO2 is 22wt%, the content of CaO is 25wt%, and the content of SiO2 is 22wt%) was impregnated with a 20wt% hydrochloric acid solution (from the HCl synthesis tail gas treatment process of the salt lake PVC plant) at room temperature. The impregnation treatment was carried out under stirring conditions, the stirring speed was 400r / min, and the treatment time was 2h to obtain the leachate slurry. The solid-liquid ratio of titanium-containing blast furnace slag to hydrochloric acid solution was 1g:10mL.

[0050] 2) The leachate obtained in step 1) is heated to 110°C for boiling hydrolysis. Heating is stopped when the pH reaches 6. The reaction product obtained from boiling hydrolysis is cooled to room temperature and filtered to obtain filter residue and filtrate. The filter residue is repeatedly washed with water in the first, second and third water washes. The third water wash is performed with 200 mL of fresh deionized water. The washing liquid is returned to the second water wash and used as the washing water for the second water wash. The washing liquid obtained from the second water wash is returned to the first water wash and used as the washing water for the first water wash. The washing liquid obtained from the first water wash is mixed with the above filtrate, and calcium oxide is added to adjust the pH of the solution to 6.5. After stabilizing for 5 min, the resulting solution is sent to the salt drying pond. After further evaporation, concentration and crystallization, calcium magnesium complex chloride is obtained.

[0051] The washed filter residue was dried in a drying oven at 500°C for 3 hours to obtain titanium-enriched slag, wherein the TiO2 content in the titanium-enriched slag was 65 wt%.

[0052] 3) Place 200g of sodium chloride into a quartz reaction tube, and then place the quartz reaction tube into a tubular furnace reactor. Set the temperature of the tubular furnace reactor to 1000℃ and heat until the sodium chloride is completely melted. Then add 12.5g of the enriched titanium slag obtained in step 2) and 4.16g of calcined petroleum coke into the quartz reaction tube and mix with the melted sodium chloride. At the same time, chlorine gas (from the chlorine purification process of the salt lake PVC plant, with a chlorine concentration of 98 vol%) is introduced at a rate of 300 mL / min. The molten salt chlorination reaction is carried out at 1000℃ for 1.5 hours. The generated gas phase is then subjected to dust collection and condensation to obtain crude titanium tetrachloride product.

[0053] Example 2

[0054] The specific steps for preparing titanium tetrachloride are as follows:

[0055] 1) 20g of titanium-containing blast furnace slag with a water content of less than 5wt% (from water-quenched slag produced by blast furnace ironmaking, in which the content of TiO2 is 19wt%, CaO is 20wt%, and SiO2 is 15wt%) was impregnated with a 15wt% hydrochloric acid solution (from the HCl synthesis tail gas treatment process of the salt lake PVC plant) at room temperature. The impregnation treatment was carried out under stirring conditions, with a stirring speed of 400r / min and a treatment time of 2h to obtain the leachate slurry. The solid-liquid ratio of the titanium-containing blast furnace slag to the hydrochloric acid solution was 1g:7.5mL.

[0056] 2) Heat the leachate obtained in step 1) to 90°C for boiling hydrolysis. Stop heating when the pH reaches 6. Cool the reaction product obtained from boiling hydrolysis to room temperature and filter it. The filter residue and filtrate are repeatedly washed with water in three stages: first, second and third. The third wash is performed with 200 mL of fresh deionized water. The washing liquid is returned to the second wash and used as the washing water for the second wash. The washing liquid obtained from the second wash is returned to the first wash and used as the washing water for the first wash. The washing liquid obtained from the first wash is mixed with the above filtrate. Calcium oxide is added to adjust the pH of the solution to 7 and stabilize it for 5 minutes. The resulting solution is sent to a salt drying pond. After further evaporation, concentration and crystallization, calcium magnesium chloride is obtained.

[0057] The washed filter residue was dried in a drying oven at 600℃ for 2 hours to obtain titanium-enriched slag, wherein the TiO2 content in the titanium-enriched slag was 58 wt%.

[0058] 3) Place 200g of sodium chloride into a quartz reaction tube, and then place the quartz reaction tube into a tubular furnace reactor. Set the temperature of the tubular furnace reactor to 1000℃ and heat until the sodium chloride is completely melted. Then add 12g of the enriched titanium slag obtained in step 2) and 4g of calcined petroleum coke into the quartz reaction tube and mix with the melted sodium chloride. At the same time, chlorine gas (from the chlorine purification process of the salt lake PVC plant, with a chlorine concentration of 98 vol%) is introduced at a rate of 350 mL / min. The molten salt chlorination reaction is carried out at 1000℃ for 1.5 hours. The generated gas phase is then subjected to dust collection and condensation to obtain crude titanium tetrachloride product.

[0059] Example 3

[0060] The specific steps for preparing titanium tetrachloride are as follows:

[0061] 1) 20g of titanium-containing blast furnace slag with a water content of less than 5wt% (from water-quenched slag produced by blast furnace ironmaking, wherein the content of TiO2 is 25wt%, the content of CaO is 25wt%, and the content of SiO2 is 15wt%) was impregnated with a 25wt% hydrochloric acid solution (from the HCl synthesis tail gas treatment process of the salt lake PVC plant) at room temperature. The impregnation treatment was carried out under stirring conditions, the stirring speed was 400r / min, and the treatment time was 2h to obtain the leachate slurry. The solid-liquid ratio of titanium-containing blast furnace slag to hydrochloric acid solution was 1g:5mL.

[0062] 2) Heat the leachate obtained in step 1) to 130°C for boiling hydrolysis. Stop heating when the pH reaches 6. Cool the reaction product obtained from boiling hydrolysis to room temperature and filter it. The filter residue and filtrate are repeatedly washed with water in three stages: first, second and third. The third wash is performed with 200 mL of fresh deionized water. The washing liquid is returned to the second wash and used as the washing water for the second wash. The washing liquid obtained from the second wash is returned to the first wash and used as the washing water for the first wash. The washing liquid obtained from the first wash is mixed with the above filtrate. Calcium oxide is added to adjust the pH of the solution to 7 and stabilize it for 5 minutes. The resulting solution is sent to a salt drying pond. After further evaporation, concentration and crystallization, calcium magnesium chloride is obtained.

[0063] The washed filter residue was dried in a drying oven at 650°C for 2 hours to obtain titanium-enriched slag, wherein the TiO2 content in the titanium-enriched slag was 55 wt%.

[0064] 3) Place 200g of sodium chloride into a quartz reaction tube, and then place the quartz reaction tube into a tubular furnace reactor. Set the temperature of the tubular furnace reactor to 1000℃ and heat until the sodium chloride is completely melted. Then add 13g of the enriched titanium slag obtained in step 2) and 5g of calcined petroleum coke into the quartz reaction tube and mix with the melted sodium chloride. At the same time, chlorine gas (from the chlorine purification process of the salt lake PVC plant, with a chlorine concentration of 98 vol%) is introduced at a rate of 450 mL / min. React at 1000℃ for 1.5 hours. The generated gas phase is then subjected to dust collection and condensation to obtain crude titanium tetrachloride product.

[0065] Example 4

[0066] The titanium-containing blast furnace slag was prepared according to the method of Example 1, except that in step 1), the TiO2 content in the titanium-containing blast furnace slag was 15 wt%.

[0067] Example 5

[0068] The preparation was carried out according to the method of Example 1, except that in step 1), the solid-liquid ratio of titanium-containing blast furnace slag to hydrochloric acid solution was 1g:4mL.

[0069] Example 6

[0070] The preparation was carried out according to the method of Example 1, except that in step 3), the amount of enriched titanium slag material used was 10g.

[0071] Example 7

[0072] The preparation was carried out according to the method of Example 1, except that in step 3), the amount of calcined petroleum coke used was 3g.

[0073] Example 8

[0074] The preparation was carried out according to the method of Example 1, except that in step 3), the flow rate of chlorine gas was 250 mL / min.

[0075] Comparative Example 1

[0076] The preparation was carried out according to the method of Example 1, except that in step 1), the solid-liquid ratio of titanium-containing blast furnace slag to hydrochloric acid was 1g:2mL.

[0077] Comparative Example 2

[0078] The preparation was carried out according to the method of Example 1, except that in step 2), the drying temperature was 350°C.

[0079] Comparative Example 3

[0080] The preparation was carried out according to the method of Example 1, except that in step 3), the amount of sodium chloride used was 150g.

[0081] Comparative Example 4

[0082] The preparation was carried out according to the method of Example 1, except that in step 3), the amount of calcined petroleum coke used was 2g.

[0083] Comparative Example 5

[0084] The preparation was carried out according to the method of Example 1, except that in step 3), the flow rate of chlorine gas introduced was 180 mL / min.

[0085] The parameters of the crude titanium tetrachloride products obtained from the examples and comparative examples were tested, and the performance parameters are shown in Table 2.

[0086] Table 2

[0087]

[0088] As can be seen from the results in Table 1, the crude titanium tetrachloride product prepared by the method of the present invention has a TiCl4 content of up to 98.7%, and after further refining, it can be used as a key raw material for high-end sponge titanium and chloride-process titanium dioxide.

[0089] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combining the various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A method for the co-digestion of titanium-containing blast furnace slag to produce hydrochloric acid and chlorine as byproducts, characterized in that, Includes the following steps: 1) Titanium-containing blast furnace slag is mixed with hydrochloric acid solution and then impregnated to obtain a leachate slurry; the solid-liquid ratio of the titanium-containing blast furnace slag to the hydrochloric acid solution is 1g:5~15mL; 2) The leaching slurry is subjected to boiling hydrolysis, and the resulting reaction product is filtered. The resulting filter residue is then washed with water and dried at 450~650℃ to obtain titanium-enriched slag with a TiO2 content of greater than or equal to 55wt%. 3) The enriched titanium slag is subjected to molten salt chlorination reaction with molten salt, calcined petroleum coke and chlorine gas, wherein the mass ratio of the molten salt, the enriched titanium slag and the calcined petroleum coke is 100:5~7:2~5, and the amount of chlorine gas used is 200~500mL / min relative to 20g of the titanium-containing blast furnace slag. 4) The gaseous products generated during the molten salt chlorination reaction are sequentially collected and condensed to obtain titanium tetrachloride product.

2. The method for co-digesting titanium-containing blast furnace slag to produce hydrochloric acid and chlorine as byproducts according to claim 1, characterized in that, The TiO2 content in the titanium-containing blast furnace slag is greater than 18 wt%, preferably 19-25 wt%.

3. The method for co-digesting titanium-containing blast furnace slag to produce hydrochloric acid and chlorine as byproducts according to claim 1 or 2, characterized in that, In step 1), the concentration of the hydrochloric acid solution is 5~30wt%.

4. The method for co-digesting titanium-containing blast furnace slag to produce hydrochloric acid and chlorine as byproducts according to any one of claims 1 to 3, characterized in that, In step 1), the impregnation treatment is carried out under stirring, with a stirring speed of 300~500 r / min, a time of 1~3 h, and a temperature of 15~90℃.

5. The method for co-digesting titanium-containing blast furnace slag to produce hydrochloric acid and chlorine as byproducts according to any one of claims 1 to 4, characterized in that, In step 2), the boiling hydrolysis temperature is 90~130℃.

6. The method for co-digesting titanium-containing blast furnace slag to produce hydrochloric acid and chlorine as byproducts according to any one of claims 1 to 5, characterized in that, In step 2), the method further includes: mixing the filtrate collected during the filtration process with the washing liquid generated during the water washing process to obtain a mixture, then adding calcium oxide to the mixture to adjust the pH value of the mixture to 6.5~7, and then sequentially evaporating, concentrating and crystallizing to obtain calcium magnesium complex chloride.

7. The method for co-digesting titanium-containing blast furnace slag to produce hydrochloric acid and chlorine as byproducts according to claim 1 or 6, characterized in that, In step 2), the water washing process includes a first water wash, a second water wash, and a third water wash performed sequentially. The washing liquid obtained from the first water wash is mixed with the filtrate obtained from the filtration. The washing liquid obtained from the second water wash is returned to the first water wash. The third water wash uses fresh water for washing, and the washing liquid obtained from the third water wash is returned to the second water wash.

8. The method for co-digesting titanium-containing blast furnace slag to produce hydrochloric acid and chlorine as byproducts according to any one of claims 1 to 7, characterized in that, In step 2), the drying temperature is 500~600℃ and the time is 1~5h.

9. The method for co-digesting titanium-containing blast furnace slag to produce hydrochloric acid and chlorine as byproducts according to any one of claims 1 to 8, characterized in that, In step 2), the TiO2 content in the enriched titanium slag is 55-65 wt%. The molten salt is sodium chloride and / or potassium chloride.

10. The method for co-digesting titanium-containing blast furnace slag to produce hydrochloric acid and chlorine as byproducts according to any one of claims 1 to 9, characterized in that, In step 3), the temperature of the molten salt chlorination reaction is 900~1100℃ and the time is 1.5~2h.

Citation Information

Patent Citations

  • Method for recycling titanium, silicon, aluminum, calcium and magnesium from titaniferous blast furnace slag by multistage acid leaching

    CN103952567A

  • Method for extracting titanium from titanium-containing blast furnace slag by aluminothermy

    CN103966455A

  • Treating and using method for titanium-containing blast furnace slag

    CN105217664A