Composite ore raw materials for mineralized filter elements, mineralized filter elements and their preparation methods

By modifying and calcining composite ore raw materials, mineralized filter cartridges are prepared, solving the problems of low magnesium ion release and unsuitable calcium-magnesium ratio. This achieves stable magnesium ion release and a suitable calcium-magnesium ratio, improving water quality and user experience.

CN123105828APending Publication Date: 2026-11-17青岛海尔施特劳斯科技有限公司 +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510623388.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing mineralized filter cartridges have low magnesium ion release rates, making it impossible to achieve a suitable calcium-magnesium ratio, resulting in a poor user experience.

Method used

The mineralized filter element is prepared by using composite mineral raw materials, including modified calcite, modified magnesite, modified dolomite and modified brucite, through the compounding of various magnesium-containing mineral raw materials, combined with modification treatment and calcination process.

Benefits of technology

It achieves stable release of magnesium ions and a suitable calcium-magnesium ratio, improving the health of the effluent and the user experience. The magnesium ion content is between 5 and 20 mg/L, which meets the requirements for healthy drinking water.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005403281240000151
    Figure BDA0005403281240000151
  • Figure BDA0005403281240000152
    Figure BDA0005403281240000152
  • Figure BDA0005403281240000161
    Figure BDA0005403281240000161
Patent Text Reader

Abstract

This application belongs to the field of water treatment technology, specifically providing a composite mineral raw material for mineralized filter cartridges, a mineralized filter cartridge, and a method for preparing the same. The aim is to solve the problems of low magnesium ion release and inability to obtain water with a suitable calcium-magnesium ratio in existing mineralized filter cartridges, thus failing to meet user water quality needs. To this end, the composite mineral raw material for mineralized filter cartridges in this application includes modified calcite, modified magnesite, modified dolomite, and modified brucite. By compounding multiple magnesium-containing mineral raw materials, the source of magnesium ions is improved, not limited to a single ore. This allows for the stable release of magnesium and calcium ions at different stages of the filter cartridge process, thereby maintaining a relatively stable calcium-magnesium ion content in the effluent, meeting the recommended ratio for healthy drinking water, and improving water quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of water treatment technology, specifically providing a composite mineral raw material for mineralized filter cartridges, a mineralized filter cartridge, and a method for preparing the same. Background Technology

[0002] As people's quality of life continues to improve, their understanding of drinking water has deepened. The focus has shifted from simply having convenient drinking water to ensuring its safety. Correspondingly, water purification technologies are constantly being updated, transitioning from traditional municipal tap water to pure water machines based on reverse osmosis technology. However, while reverse osmosis solves drinking water safety issues, its characteristic of removing beneficial minerals from the water reduces the health benefits of the water produced by pure water machines. To compensate for this shortcoming, mineralization filters have emerged. These filters increase the mineral content of the water by releasing minerals into it.

[0003] Existing mineralized filter cartridges release low levels of magnesium ions, generally below 5 mg / L, and the water flowing through them cannot achieve a suitable calcium-magnesium ratio, resulting in a poor user experience.

[0004] Accordingly, a new technical solution is needed in this field to solve the above-mentioned technical problems. Summary of the Invention

[0005] This application aims to solve the aforementioned technical problems, namely, to address the issues that existing mineralized filter cartridges have low magnesium ion release and cannot obtain water with a suitable calcium-magnesium ratio, thus failing to meet users' water needs.

[0006] In a first aspect, this application provides a composite ore raw material for mineralizing filter cartridges, the composite ore raw material comprising modified calcite, modified magnesite, modified dolomite, and modified brucite.

[0007] In the preferred technical scheme of the composite ore raw material for mineralized filter element described above, the composite ore raw material includes, by weight, 10-20 parts modified calcite, 5-10 parts modified magnesite, 5-10 parts modified dolomite and 1-5 parts modified brucite.

[0008] In the preferred technical solution of the composite ore raw material for mineralized filter cartridges described above, the composite ore raw material further includes 1 to 5 parts of modified carnallite; and / or, the composite ore raw material further includes 5 to 10 parts of modified forsterite; and / or, the composite ore raw material further includes 5 to 10 parts of modified serpentine.

[0009] In the preferred technical solution of the composite ore raw material for the above-mentioned mineralized filter element, the modified calcite is prepared by the following steps: crushing water-washed natural calcite to a first particle size range, rinsing with pure water and drying, calcining at a first temperature for a first set time, cooling and soaking in pure water for a second set time, introducing CO2 into the pure water during the soaking process, then filtering to obtain a solid and drying to obtain the modified calcite; and / or, the modified magnesite is prepared by the following steps: crushing water-washed natural magnesite to a first particle size range, rinsing with pure water and drying, calcining at a second temperature for a first set time, cooling and soaking in pure water for a second set time, introducing CO2 into the pure water during the soaking process, then filtering to obtain a solid and drying. The modified magnesite is obtained by means of the following steps: pulverizing water-washed natural dolomite to a first particle size range, rinsing with pure water and drying, calcining at a third temperature for a first set time, cooling and soaking in pure water for a second set time, introducing CO2 into the pure water during the soaking process, then filtering to obtain a solid and drying to obtain the modified dolomite; and / or, the modified brucite is obtained by means of the following steps: pulverizing water-washed natural brucite to a first particle size range, rinsing with pure water and drying, calcining at a fourth temperature for a third set time, cooling and soaking in pure water for a second set time, introducing CO2 into the pure water during the soaking process, then filtering to obtain a solid and drying to obtain the modified brucite.

[0010] In the preferred technical solution of the above-mentioned composite ore raw material for mineralized filter cartridges, the modified carnallite is prepared by the following steps: pulverizing water-washed natural carnallite to a first particle size range, rinsing with pure water and drying, calcining at a third temperature for a first set time, cooling and soaking in pure water for a second set time, during which a mixed gas of HCl and CO2 is introduced into the pure water, and after drying and filtration, the modified carnallite is obtained; and / or, the modified forsterite is prepared by the following steps: pulverizing water-washed natural forsterite to a first particle size range, rinsing with pure water and drying, calcining at a fourth temperature for a third set time, cooling and sieving, the modified forsterite is obtained; and / or, the modified serpentine is prepared by the following steps: pulverizing water-washed natural serpentine to a first particle size range, rinsing with pure water and drying, calcining at a third temperature for a third set time, cooling and sieving, the modified serpentine is obtained.

[0011] In the preferred technical solution of the composite ore raw material used for mineralized filter elements described above, the first setting time is 50-90 min; preferably, the first setting time is 60 min; and / or, the second setting time is 20-40 min; preferably, the second setting time is 30 min; and / or, the third setting time is 20-40 min; preferably, the third setting time is 30 min; and / or, the first particle size range is 50-200 mesh; and / or, the first temperature is 800℃-900℃, preferably, the first temperature is 850℃; and / or, the second temperature is 550℃-650℃, preferably, the second temperature is 600℃; and / or, the third temperature is 600℃-850℃, preferably, the third temperature is 700℃-850℃; and / or, the fourth temperature is 400℃-850℃.

[0012] In a second aspect, this application provides a mineralized filter element, the mineralized filter element comprising a composite mineral raw material, an adsorbent, and a binder, wherein the adsorbent comprises carbon powder, and the composite mineral raw material is the aforementioned composite mineral raw material used in the mineralized filter element.

[0013] In the preferred technical solution of the above-mentioned mineralized filter element, the mineralized filter element comprises, by weight, 21 to 70 parts of composite mineral raw material, 50 to 140 parts of adsorbent material, and 20 to 40 parts of binder.

[0014] In the preferred embodiment of the above-mentioned mineralized filter element, the adsorbent further includes cellulose carbon, and the weight ratio of the carbon powder to the cellulose carbon is (50-70):(60-70); and / or, the binder includes one or more of food-grade polyethylene, food-grade polyvinyl chloride, food-grade polyvinyl alcohol, cellulose, and polylactic acid.

[0015] In a third aspect, this application provides a method for preparing a mineralized filter element, the method comprising the following steps: mixing composite ore raw materials, adsorbents and binders uniformly to obtain a mixture; and preparing the mineralized filter element by means of a sintering process, an extrusion process or a wet carbon fiber process.

[0016] When the above technical solution is adopted, the composite mineral raw materials for mineralized filter elements in this application include modified calcite, modified magnesite, modified dolomite, and modified brucite. By compounding multiple magnesium-containing mineral raw materials, the source of magnesium ions is improved. It is not limited to a single ore and can stably release magnesium and calcium ions at different stages of the filter element, thereby keeping the magnesium ion content in the effluent relatively stable, maintaining a suitable calcium-magnesium ratio, meeting the requirements of healthy drinking water, and improving water quality.

[0017] Furthermore, the composite mineral raw materials include 10-20 parts modified calcite, 5-10 parts modified magnesite, 5-10 parts modified dolomite, and 1-5 parts modified brucite. This formula ratio can effectively control the calcium-magnesium ratio of the effluent, keeping it between 1 and 5, making the effluent more in line with health requirements. At the same time, it solves the problems of difficult slow release and low precipitation of magnesium ions, ensuring that the magnesium ion content in the effluent is between 5 and 20 mg / L, meeting the user's healthy water needs.

[0018] Furthermore, the composite ore raw materials also include modified carnallite, which further increases the source of magnesium ions and further increases the release of magnesium ions from water, thus helping to improve the lifespan of magnesium release.

[0019] Furthermore, the composite mineral raw material also includes 5 to 10 parts of modified magnesium olivine. Magnesium olivine can provide magnesium ions and release metasilicic acid, thereby improving the taste of water and enhancing the user experience.

[0020] Furthermore, the composite mineral raw material also includes 5 to 10 parts of modified serpentine. Serpentine can provide magnesium ions and release metasilicic acid, thereby improving the taste of water and enhancing the user experience.

[0021] Furthermore, the crushed and rinsed natural calcite is first calcined to remove organic impurities, improve the quality of the effluent, and enhance its taste. Then, it is soaked in cold water and carbon dioxide is introduced to react with the carbon dioxide generated during the calcination stage and restore it to calcium carbonate, thereby preventing the release of calcium ions from the calcite too quickly after it is made into a filter element.

[0022] Furthermore, the crushed and rinsed natural magnesite is first calcined to remove organic impurities, improve the quality of the effluent, and enhance its taste. Then, it is soaked in cold water and carbon dioxide is introduced to react with the carbon dioxide to restore some of the magnesium hydroxide generated during the calcination stage to magnesium carbonate, thereby preventing the release of magnesium ions from the magnesite too quickly after it is made into a filter element.

[0023] Furthermore, the crushed and rinsed natural dolomite is first calcined to remove organic impurities, improve water quality, and enhance the taste of the water. Then, it is soaked in cold water and carbon dioxide is introduced to react with the carbon dioxide to restore some of the magnesium hydroxide generated during the calcination stage to magnesium carbonate. At the same time, some of the calcium hydroxide generated during the calcination stage reacts with the carbon dioxide to restore calcium carbonate, thereby preventing the release of calcium and magnesium ions from the dolomite too quickly after it is made into a filter element.

[0024] Furthermore, the crushed and rinsed natural brucite is first calcined to remove organic impurities, improve the quality of the output water, and enhance its taste. Then, it is soaked in cold water and carbon dioxide is introduced to allow some of the magnesium hydroxide to react with the carbon dioxide to form magnesium carbonate, thereby preventing the release of magnesium ions from the brucite too quickly after it is made into a filter element.

[0025] Furthermore, the crushed and rinsed natural carnallite is first calcined to remove organic impurities, improve water quality, and enhance the taste of the water. Then, it is soaked in cold water and carbon dioxide is introduced to react some of the magnesium hydroxide generated during the calcination stage with carbon dioxide to form magnesium carbonate and with HCl to form magnesium chloride, thereby preventing the release of magnesium ions from the carnallite too quickly after it is made into a filter element.

[0026] Furthermore, the crushed and rinsed natural magnesium olivine is calcined to remove organic impurities from the natural magnesium olivine, improve the quality of the effluent, enhance the taste of the effluent, and improve the safety of the composite mineral raw materials.

[0027] Furthermore, the crushed and rinsed natural serpentine is calcined to remove organic impurities from the natural serpentine, improve the quality of the effluent, enhance the taste of the effluent, and increase the safety of the composite mineral raw materials.

[0028] Furthermore, the mineralized filter element of this application includes the aforementioned composite mineral raw materials, adsorbents, and binders. This mineralized filter element can stably release calcium and magnesium ions, thereby increasing the magnesium ion content in the water, and can reasonably control the calcium-magnesium ratio to improve the quality of the effluent. Moreover, the modified minerals used in this application are not treated with acids or alkalis, so they will not affect the pH value of the effluent, and there is no impact on water quality deterioration, ensuring the safety of the effluent.

[0029] Furthermore, the mineralized filter element includes 21-70 parts of composite mineral raw materials, 50-140 parts of adsorbent material, and 20-40 parts of binder. This formula ratio can effectively control the calcium-magnesium ratio of the effluent, keeping it between 1 and 5, making the effluent more in line with health requirements. At the same time, it addresses the issues of slow release of magnesium ions and low precipitation, ensuring that the magnesium ion content in the effluent is between 5 and 20 mg / L, thus meeting the user's healthy water needs.

[0030] Furthermore, the adsorbent material includes carbon powder and carbon fiber, and the weight ratio of carbon powder to carbon fiber is (50-70):(60-70). Adding carbon fiber to the adsorbent material and making the weight ratio of carbon powder to carbon fiber (50-70):(60-70) can improve the adsorption effect of the mineralization filter element, making the water cleaner and healthier, and does not affect the precipitation of calcium and magnesium substances. Detailed Implementation

[0031] The preferred embodiments of this application are described below. Those skilled in the art should understand that these embodiments are merely illustrative of the technical principles of this application and are not intended to limit the scope of protection of this application.

[0032] As pointed out in the background art, existing mineralized filter cartridges have low magnesium ion release and cannot obtain water with a suitable calcium-magnesium ratio, thus failing to meet users' water needs.

[0033] The composite mineral raw materials used in this application for mineralized filter cartridges include modified calcite, modified magnesite, modified dolomite, and modified brucite. By compounding multiple magnesium-containing mineral raw materials, the source of magnesium ions is improved. It is not limited to a single ore and can stably release magnesium and calcium ions at different stages of the filter cartridge. This keeps the magnesium ion content in the effluent relatively stable, maintains a suitable calcium-magnesium ratio, meets the requirements for healthy drinking water, and improves water quality.

[0034] Specifically, in a first aspect, this application provides a composite ore raw material for mineralized filter cartridges, the composite ore raw material including modified calcite, modified magnesite, modified dolomite and modified brucite.

[0035] The composite mineral raw materials used in this application for mineralized filter cartridges include modified calcite, modified magnesite, modified dolomite, and modified brucite. By compounding multiple magnesium-containing mineral raw materials, the source of magnesium ions is improved. It is not limited to a single ore and can stably release magnesium and calcium ions at different stages of the filter cartridge. This keeps the magnesium ion content in the effluent relatively stable, maintains a suitable calcium-magnesium ratio, meets the requirements for healthy drinking water, and improves water quality.

[0036] In some embodiments, the composite mineral raw materials of this application, by weight, include: 10-20 parts modified calcite, 5-10 parts modified magnesite, 5-10 parts modified dolomite, and 1-5 parts modified brucite. This formulation ratio can effectively control the calcium-magnesium ratio of the effluent, keeping it between 1 and 5, making the effluent more in line with health requirements. It also solves the problems of difficult slow release and low precipitation of magnesium ions, ensuring that the magnesium ion content in the effluent is between 5 and 20 mg / L, meeting the user's healthy water needs.

[0037] In some embodiments, the composite ore raw material further includes 1 to 5 parts of modified carnallite. The addition of modified carnallite further increases the source of magnesium ions, further enhances the release of magnesium ions from water, and helps to improve the magnesium release lifetime.

[0038] In some embodiments, the composite ore raw material further includes 5 to 10 parts of modified magnesium olivine. The modified magnesium olivine provides magnesium ions and releases metasilicic acid, thereby improving the taste of the water and enhancing the user experience.

[0039] In some embodiments, the composite ore raw material further includes 5 to 10 parts of modified serpentine. The modified serpentine provides magnesium ions and releases metasilicic acid, thereby improving the taste of the water and enhancing the user experience.

[0040] In some embodiments, modified calcite is prepared by the following steps: pulverizing water-washed natural calcite to a first particle size range, rinsing with pure water and drying, calcining at a first temperature for a first set time, cooling and soaking in pure water for a second set time, introducing CO2 into the pure water during the soaking process, filtering to obtain a solid and drying to obtain modified calcite.

[0041] In the above embodiments, the preferred first particle size range is 50 to 200 mesh.

[0042] In the above embodiments, the preferred first temperature is 800-900°C, and the most preferred first temperature is 850°C.

[0043] In the above embodiments, the first set time is preferably 50 to 90 minutes; the most preferred first set time is 60 minutes.

[0044] In the above embodiments, the second set time is preferably 20 to 40 minutes; the most preferred second set time is 30 minutes.

[0045] In this embodiment, the natural calcite is first crushed to facilitate subsequent calcination and direct use after processing. After washing, it is calcined at 800-900℃ for 50-90 minutes, which can effectively remove organic and combustible impurities contained in the natural calcite, improve the quality of the effluent, and enhance the taste of the effluent. Afterward, it is soaked in cold water while carbon dioxide is introduced during the soaking process. This allows some of the calcium hydroxide generated during the calcination stage to react with the carbon dioxide to form calcium carbonate, thereby preventing the release of calcium ions from the calcite too quickly after it is made into a filter element, and thus effectively improving the service life of the filter element.

[0046] In some embodiments, modified magnesite is prepared by the following steps: pulverizing water-washed natural magnesite to a first particle size range, rinsing with pure water and drying, calcining at a second temperature for a first set time, cooling and soaking in pure water for a second set time, introducing CO2 into the pure water during the soaking process, filtering to obtain a solid and drying to obtain modified magnesite.

[0047] In the above embodiments, the preferred first particle size range is 50 to 200 mesh.

[0048] In the above embodiments, the second temperature is preferably 550-650°C, and most preferably 600°C.

[0049] In the above embodiments, the first set time is preferably 50 to 90 minutes; the most preferred first set time is 60 minutes.

[0050] In the above embodiments, the second set time is preferably 20 to 40 minutes; the most preferred second set time is 30 minutes.

[0051] In this embodiment, the natural magnesite is first crushed to facilitate subsequent calcination and direct use after processing. After washing, it is calcined at 550-650℃ for 50-90 minutes, which can effectively remove organic and combustible impurities contained in the natural magnesite, improve the quality of the effluent, and enhance the taste of the effluent. Afterward, it is soaked in cold water while carbon dioxide is introduced during the soaking process. This allows some of the magnesium hydroxide generated during the calcination stage to react with the carbon dioxide and be restored to magnesium carbonate, thereby preventing the release of magnesium ions from the magnesite too quickly after it is made into a filter element, and thus effectively improving the service life of the filter element.

[0052] In some embodiments, modified dolomite is prepared by the following steps: pulverizing water-washed natural dolomite to a first particle size range, rinsing with pure water and drying, calcining at a third temperature for a first set time, cooling and soaking in pure water for a second set time, introducing CO2 into the pure water during the soaking process, filtering to obtain a solid and drying to obtain modified dolomite.

[0053] In the above embodiments, the preferred first particle size range is 50 to 200 mesh.

[0054] In the above embodiments, the third temperature is preferably 700-850°C, and most preferably 800°C.

[0055] In the above embodiments, the first set time is preferably 50 to 90 minutes; the most preferred first set time is 60 minutes.

[0056] In the above embodiments, the second set time is preferably 20 to 40 minutes; the most preferred second set time is 30 minutes.

[0057] In this embodiment, the natural dolomite is first crushed to facilitate subsequent calcination and direct use after processing. After washing, it is calcined at 700-850℃ for 50-90 minutes, which effectively removes organic and combustible impurities contained in the natural dolomite, improves the quality of the effluent, and enhances the taste of the effluent. Afterward, it is soaked in cold water while carbon dioxide is introduced during the soaking process. This allows some of the magnesium hydroxide generated during the calcination stage to react with carbon dioxide and be restored to magnesium carbonate. At the same time, some of the calcium hydroxide generated during the calcination stage will also react with carbon dioxide and be restored to calcium carbonate. This avoids the excessively rapid release of calcium and magnesium ions after the dolomite is made into a filter element, thereby effectively improving the service life of the filter element.

[0058] In some embodiments, modified brucite is prepared by the following steps: pulverizing natural brucite washed with water to a first particle size range, rinsing with pure water and drying, calcining at a fourth temperature for a third set time, cooling and soaking in pure water for a second set time, introducing CO2 into the pure water during the soaking process, filtering to obtain a solid and drying to obtain modified brucite.

[0059] In the above embodiments, the preferred first particle size range is 50 to 200 mesh.

[0060] In the above embodiments, the fourth temperature is preferably 400-850°C, and the most preferred fourth temperature is 400°C.

[0061] In the above embodiments, the third set time is preferably 20 to 40 minutes; the most preferred third set time is 30 minutes.

[0062] In the above embodiments, the second set time is preferably 20 to 40 minutes; the most preferred second set time is 30 minutes.

[0063] In this embodiment, the natural brucite is first crushed to facilitate subsequent calcination and direct use after processing. After washing, it is calcined at 350-450℃ for 20-40 minutes, which can effectively remove organic and combustible impurities contained in the natural brucite, improve the quality of the effluent, and enhance the taste of the effluent. Afterward, it is soaked in cold water while carbon dioxide is introduced during the soaking process, which allows some of the magnesium hydroxide to react with the carbon dioxide to form magnesium carbonate. This prevents the release rate of magnesium ions from the brucite from being too fast after it is made into a filter element, thereby effectively improving the service life of the filter element.

[0064] Preferably, modified carnallite is prepared by the following steps: water-washed natural carnallite is crushed to a first particle size range, rinsed with pure water and dried, calcined at a third temperature for a first set time, cooled and soaked in pure water for a second set time, during which a mixed gas of HCl and CO2 is introduced into the pure water, and after drying and filtration, modified carnallite is obtained.

[0065] In the above embodiments, the preferred first particle size range is 50 to 200 mesh.

[0066] In the above embodiments, the third temperature is preferably 600-850°C, and most preferably 700°C.

[0067] In the above embodiments, the first set time is preferably 50 to 90 minutes; the most preferred first set time is 60 minutes.

[0068] In the above embodiments, the second set time is preferably 20 to 40 minutes; the most preferred second set time is 30 minutes.

[0069] In this embodiment, the natural carnallite is first crushed to facilitate subsequent calcination and direct use after processing. After washing, it is calcined at 600-850℃ for 50-90 minutes, which can effectively remove organic and combustible impurities contained in the natural carnallite, improve the quality of the effluent, and enhance the taste of the effluent. Afterward, it is soaked in cold water while carbon dioxide and HCl are introduced during the soaking process. This allows some of the magnesium hydroxide generated during the calcination stage to react with carbon dioxide to form magnesium carbonate and with HCl to form magnesium chloride. This avoids the excessive release of magnesium ions after the carnallite is made into a filter element, thereby effectively improving the service life of the filter element.

[0070] In some embodiments, modified forsterite is prepared by the following steps: washing natural forsterite with water and crushing it to a first particle size range, rinsing it with pure water and drying it, calcining it at a fourth temperature for a third set time, cooling it and sieving it to obtain modified forsterite.

[0071] In the above embodiments, the preferred first particle size range is 50 to 200 mesh.

[0072] In the above embodiments, the fourth temperature is preferably 400-850°C, and most preferably 600°C.

[0073] In the above embodiments, the third set time is preferably 20 to 40 minutes; the most preferred third set time is 30 minutes.

[0074] In this embodiment, the natural magnesium olivine is first crushed to facilitate subsequent calcination and direct use after processing. After washing, it is calcined at 400-800℃ for 20-40 minutes, which can effectively remove organic impurities and combustible impurities contained in the natural magnesium olivine, improve the quality of the effluent, improve the taste of the effluent, and enhance the safety of the composite mineral raw materials.

[0075] In some embodiments, modified serpentine is prepared by the following steps: washing natural serpentine with water and crushing it to a first particle size range, rinsing it with pure water and drying it, calcining it at a third temperature for a third set time, cooling it and sieving it to obtain modified serpentine.

[0076] In the above embodiments, the preferred first particle size range is 50 to 200 mesh.

[0077] In the above embodiments, the third temperature is preferably 600-850°C, and most preferably 700°C.

[0078] In the above embodiments, the third set time is preferably 20 to 40 minutes; the most preferred third set time is 30 minutes.

[0079] In this embodiment, the natural serpentine is first crushed to facilitate subsequent calcination and direct use after processing. After washing, it is calcined at 600-850℃ for 20-40 minutes, which can effectively remove organic and combustible impurities contained in the natural serpentine, improve the quality of the effluent, improve the taste of the effluent, and enhance the safety of the composite mineral raw materials.

[0080] In a second aspect, this application provides a mineralized filter element, which includes a composite ore raw material, an adsorbent, and a binder, wherein the composite ore raw material is the aforementioned composite ore raw material for the mineralized filter element, and the adsorbent includes carbon powder.

[0081] The mineralized filter element of this application includes the aforementioned composite mineral raw materials, adsorbents, and binders. This mineralized filter element can stably release magnesium ions, thereby increasing the magnesium ion content in the water and controlling the calcium-magnesium ratio to improve the quality of the effluent. Furthermore, the modified minerals used in this application are not treated with acids or alkalis, so they will not affect the pH value of the effluent, and there is no risk of water quality deterioration, ensuring the safety of the effluent.

[0082] Preferably, the mineralized filter element of this application comprises, by weight, 21 to 70 parts of composite mineral raw material, 50 to 140 parts of adsorbent, and 20 to 40 parts of binder. This formulation ratio can effectively control the calcium-magnesium ratio of the effluent, keeping it between 1 and 5, making the effluent more in line with health requirements. It also addresses the issues of slow release and low precipitation of magnesium ions, ensuring that the magnesium ion content in the effluent is between 5 and 20 mg / L, meeting the user's healthy water needs.

[0083] Preferably, the adsorbent also includes cellulose carbon, and the weight ratio of carbon powder to cellulose carbon is (50-70):(60-70).

[0084] The adsorbents include carbon powder and carbon fiber, with a weight ratio of (50-70):(60-70). Adding carbon fiber to the adsorbents and maintaining a weight ratio of (50-70):(60-70) can improve the adsorption effect of the mineralization filter cartridge, making the water cleaner and healthier, without affecting the precipitation of calcium and magnesium substances, resulting in cleaner and safer effluent.

[0085] Preferably, the binder includes one or more of food-grade polyethylene, food-grade polyvinyl chloride, food-grade polyvinyl alcohol, cellulose, and polylactic acid.

[0086] This application provides a method for preparing a mineralized filter element in a third aspect, the method comprising the following steps:

[0087] (1) Mix the composite ore raw materials, adsorbents and binders evenly to obtain a mixture.

[0088] (2) The mixture is processed into a mineralized filter element by sintering, extrusion or wet carbon fiber process.

[0089] The following detailed embodiments illustrate the composite ore raw materials and mineralized filter elements of this application.

[0090] It should be noted that the modified calcite, modified magnesite, modified dolomite, modified brucite, modified carnallite, modified forsterite, and modified serpentine involved in the embodiments of this application are obtained through the following steps.

[0091] Modified calcite: Washed natural calcite is crushed to 50-200 mesh, rinsed with pure water and dried, calcined at 850℃ for 60 min, cooled and soaked in pure water for 30 min, during which CO2 is introduced into the pure water, then filtered to obtain a solid and dried to obtain modified calcite.

[0092] Modified magnesite: Washed natural magnesite is crushed to 50-200 mesh, rinsed with pure water and dried, calcined at 600℃ for 60 min, cooled and soaked in pure water for 30 min. During the soaking process, CO2 is introduced into the pure water. After filtration, the solid is obtained and dried to obtain modified magnesite.

[0093] Modified dolomite: Washed natural dolomite is crushed to 50-200 mesh, rinsed with pure water and dried, calcined at 800℃ for 60 minutes, cooled and soaked in pure water for 30 minutes. During the soaking process, CO2 is introduced into the pure water. After filtration, the solid is obtained and dried to obtain modified dolomite.

[0094] Modified brucite: Washed natural brucite is crushed to 50-200 mesh, rinsed with pure water and dried, calcined at 400℃ for 30 minutes, cooled and soaked in pure water for 30 minutes. During the soaking process, CO2 is introduced into the pure water. After filtration, the solid is obtained and dried to obtain modified brucite.

[0095] Modified carnallite: Washed natural carnallite is crushed to 50-200 mesh, rinsed with pure water and dried, calcined at 700℃ for 60 min, cooled and soaked in pure water for 30 min. During the soaking process, a mixture of HCl and CO2 gas is introduced into the pure water. After drying and filtration, modified carnallite is obtained.

[0096] Modified forsterite: Washed natural forsterite is crushed to 50-200 mesh, rinsed with pure water and dried, calcined at 600℃ for 60 min, cooled and sieved to obtain modified forsterite.

[0097] Modified serpentine: Washed natural serpentine is crushed to 50-200 mesh, rinsed with pure water and dried, calcined at 700℃ for 30 minutes, cooled and sieved to obtain modified serpentine.

[0098] Example 1

[0099] The composite ore raw material in this embodiment includes the following components by weight: 15 parts modified calcite, 8 parts modified magnesite, 8 parts modified dolomite, and 3 parts modified brucite.

[0100] The mineralized filter element of this embodiment comprises the following components by weight: 50 parts composite mineral raw material, 100 parts adsorbent, and 30 parts binder (food-grade polyethylene). The adsorbent consists of carbon powder and carbon fiber, with a weight ratio of carbon powder to carbon fiber of 60:60.

[0101] The mineralized filter element in this embodiment is prepared by the following method:

[0102] (1) Mix the composite ore raw materials, adsorbents and binders evenly to obtain a mixture.

[0103] (2) The mixture is sintered to obtain a mineralized filter element. The sintering parameters are 200℃ and 18MPa for 120min.

[0104] The only difference between Examples 2 to 10 and Example 1 is the composition ratio of the composite ore raw materials. The composition and ratio of the mineralized filter element and its preparation method are the same as those in Example 1. The composition and ratio of the composite ore raw materials in Examples 2 to 6 are shown in Table 1.

[0105] Table 1. Composition of composite ore raw materials in Examples 2 to 10

[0106] The only difference between Examples 11 to 15 and Example 6 is the composition ratio of the mineralized filter element. The composition and ratio of the composite ore raw material are the same as those of Example 6. The composition and ratio of the mineralized filter elements of Examples 11 to 15 are shown in Table 2.

[0107] Table 2. Composition of mineralized filter cartridges in Examples 11 to 15

[0108] Comparative Example 1

[0109] The only difference between this comparative example and Example 6 is the composition ratio of the composite ore raw materials. The composition and ratio of the mineralized filter element and its preparation method are the same as those in Example 6.

[0110] Specifically, the composite ore raw material in this comparative example comprises the following components by weight: 15 parts natural calcite, 8 parts natural magnesite, 8 parts natural dolomite, 3 parts natural brucite, 3 parts natural carnallite, 8 parts natural forsterite, and 8 parts natural serpentine. The particle size of the natural calcite, natural magnesite, natural dolomite, natural brucite, natural carnallite, natural forsterite, and natural serpentine is 50–200 mesh.

[0111] Comparative Example 2

[0112] The mineralized filter element in this comparative example comprises 50 parts of composite mineral raw material, 100 parts of adsorbent material, and 30 parts of binder (food-grade polyethylene). The adsorbent material consists of carbon powder and fiber carbon, with a weight ratio of carbon powder to fiber carbon of 60:60. The preparation method of the mineralized filter element is the same as in Example 6, and the composite mineral raw material is calcium-magnesium mineralized filter media.

[0113] Specifically, the calcium-magnesium mineralized filter media of this comparative example includes a matrix and a coating layer covering the outer surface of the matrix. The matrix is ​​modified limestone with a granular structure, and the coating layer includes recrystallized calcite and recrystallized dolomite. The thickness of the coating layer is 45 μm. The mass ratio of the modified limestone, recrystallized calcite and recrystallized dolomite is 10:1:2.

[0114] The preparation method of the calcium-magnesium mineralized filter media in this comparative example includes the following steps:

[0115] S10. Preparation of calcite and dolomite solutions: Weigh 10g of natural calcite and 10g of natural dolomite, then crush the natural calcite and natural dolomite into granules (0.1cm to 0.5cm in diameter). Wash the granules and place them separately into sealed glass containers. Next, add deionized water to the glass containers containing the granules until they are completely submerged. Finally, in a carbon dioxide atmosphere (carbon dioxide partial pressure 0.15 bar, ambient temperature 10℃), stir the reaction to dissolve the granules in the corresponding deionized water, obtaining calcite and dolomite solutions. The TDS of the calcite solution is 462mg / L, and the TDS of the dolomite solution is 680mg / L.

[0116] S20. Preparation of modified limestone: Weigh out natural limestone according to the specified amount, wash it with deionized water, and crush it into 70-mesh powder. Then, place the crushed limestone into 50 mL of 0.05 mol / L sodium citrate solution, so that the volume ratio between the powdered limestone and sodium citrate is 3:1. Soak the limestone at 85℃ for 9 hours to make the micro-morphology of the limestone surface uneven. Filter and dry to obtain granular modified limestone.

[0117] S30. Coating treatment of modified limestone: The granular modified limestone obtained in step S20 is placed in a tubular furnace, and then the tubular furnace is heated to 350°C. Carbon dioxide gas is then introduced into the tubular furnace, and the calcite solution and dolomite solution obtained in step S10 are mixed in a preset ratio to obtain a reaction solution. Under the atmosphere of carbon dioxide gas, the reaction solution is atomized and introduced into the tubular furnace. The molar ratio between the carbon dioxide gas participating in the reaction, the calcium ions in the reaction solution, and the magnesium ions in the reaction solution is 5:1:2. The tubular furnace is stopped from heating every 0.5 hours and stirred continuously to prevent the granular modified limestone from agglomerating. The reaction is continued for 4 hours to coat the surface of the granular modified limestone with recrystallized calcite and recrystallized dolomite to obtain calcium-magnesium mineralized filter material.

[0118] Test case

[0119] The mineralized filter elements prepared in Examples 1 to 15 and Comparative Examples 1 and 2 were cut into filter rods with a length of 68 mm and assembled with end caps and O-rings to form filter elements. These were then installed at the outlet of a water purifier for testing. The content of calcium and magnesium ions and metasilicic acid in the water purifier's output was measured. The specific testing method was as follows: the test water was pure water / RO water. Based on the total mineralized water volume, the mineralization process was divided into four stages. Samples were taken after the water flowed through the mineralized filter element, with a total of five batches of water samples collected. The sampling points were: the beginning of the formal water flow (first sampling, i.e., water flow rate of 0 L), the end of the 1 / 4 stage (second sampling, i.e., water flow rate of 1000 L), the end of the 2 / 4 stage (third sampling, i.e., water flow rate of 2000 L), the end of the 3 / 4 stage (fourth sampling, i.e., water flow rate of 3000 L), and the end of the 4 / 4 stage (fifth sampling, i.e., water flow rate of 4000 L). Before each sampling, the mineralization device was allowed to stand for 1.5 hours, and 700 ml was taken for testing. The water sample was tested according to the corresponding method in GB / T 5838. The test data are shown in Tables 3 to 7. Specifically, Table 3 shows the test data at 0 L, Table 4 shows the test data at 1000 L, Table 5 shows the test data at 2000 L, Table 6 shows the test data at 3000 L, and Table 7 shows the test data at 4000 L.

[0120] Table 3 Data table of mineralized filter cartridges 0L in Examples 1-15 and Comparative Examples 1-2

[0121] Table 4. Data for 1000L mineralized filter cartridges of Examples 1-15 and Comparative Examples 1-2

[0122] Table 5. Data for 2000L mineralized filter cartridges of Examples 1-15 and Comparative Examples 1-2.

[0123] Table 6. Data for mineralized filter cartridges (3000L) of Examples 1-15 and Comparative Examples 1-2.

[0124] Table 7 Data for mineralized filter cartridges (4000L) of Examples 1-15 and Comparative Examples 1-2

[0125] The data from Tables 3 to 7 show that:

[0126] 1. The mineralization filter cartridges in Examples 1 to 15 maintained a calcium-to-magnesium ratio between 1 and 5 at 0L, 1000L, 2000L, 3000L, and 4000L, with a magnesium ion content between 5 and 20 mg. This ensured relatively stable magnesium ion content in the effluent and maintained a suitable calcium-to-magnesium ratio, meeting the requirements for healthy drinking water. While the mineralization filter cartridge in Comparative Example 1 maintained a calcium-to-magnesium ratio between 1 and 5 at 0L, 1000L, 2000L, and 3000L, with a magnesium ion content between 5 and 20 mg, its magnesium ion content decreased to 5 mg / L at 4000L, and its calcium-to-magnesium ratio exceeded 5, resulting in a shorter service life. The mineralization filter cartridge in Comparative Example 2 showed a calcium-to-magnesium ratio in the flowing water that was significantly greater than 5, indicating an excessively slow release rate of calcium and magnesium ions. Therefore, the composite mineral raw material and mineralized filter element of this application can stably release magnesium ions and calcium ions at different stages of the filter element, thereby keeping the magnesium ion content in the effluent relatively stable, maintaining a suitable calcium-magnesium ratio, meeting the requirements of healthy drinking water, and improving water quality.

[0127] 2. Comparing Example 1 with Examples 3, 4, 5 and 6, it can be seen that adding modified magnesium olivine and modified serpentine to the composite ore raw materials can increase the metasilicic acid value of the effluent, thereby improving the taste of the water and enhancing the user experience.

[0128] 3. Comparing Examples 6 to 10, it can be seen that at 0L, 1000L, 2000L, 3000L, and 4000L, the effluent can effectively maintain a calcium-magnesium ratio of 1 to 5, and the magnesium ion content is between 5 and 20 mg / L. Therefore, the preferred composite mineral raw materials include 10 to 20 parts modified calcite, 5 to 10 parts modified magnesite, 5 to 10 parts modified dolomite, and 1 to 5 parts modified brucite. This formula can make the effluent more in line with the health ratio, while solving the problems of difficult slow release and low precipitation of magnesium ions, ensuring the magnesium ion content in the effluent and meeting the user's healthy water needs.

[0129] 4. Comparing Example 6 with Examples 11-15, it can be seen that at 0L, 1000L, 2000L, 3000L, and 4000L, the effluent can be effectively maintained at a calcium-magnesium ratio of 1-5, and the magnesium ion content is between 5-20 mg / L. Therefore, the preferred mineralized filter element includes 21-70 parts of composite mineral raw material, 50-140 parts of adsorbent, and 20-40 parts of binder. This formula ratio can effectively control the calcium-magnesium ratio of the effluent, keeping it between 1-5, making the effluent more in line with health requirements. At the same time, it avoids the problems of slow release of magnesium ions and low precipitation, ensuring that the magnesium ion content in the effluent meets the user's healthy water needs.

[0130] The technical solutions of this application have been described in conjunction with preferred embodiments. However, it will be readily understood by those skilled in the art that the scope of protection of this application is obviously not limited to these specific embodiments. Without departing from the principles of this application, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will all fall within the scope of protection of this application.

Claims

1. A composite ore raw material for mineralized filter cartridges, characterized in that, The composite ore raw materials include modified calcite, modified magnesite, modified dolomite, and modified brucite.

2. The composite ore raw material for mineralized filter elements according to claim 1, characterized in that, The composite ore raw materials, by weight, include: 10-20 parts modified calcite, 5-10 parts modified magnesite, 5-10 parts modified dolomite, and 1-5 parts modified brucite.

3. The composite ore raw material for mineralized filter elements according to claim 2, characterized in that, The composite ore raw material also includes 1 to 5 parts of modified carnallite; And / or, the composite ore raw material further includes 5 to 10 parts of modified magnesium olivine; And / or, the composite ore raw material further includes 5 to 10 parts of modified serpentine.

4. The composite ore raw material for mineralized filter elements according to any one of claims 1 to 3, characterized in that, The modified calcite is prepared by the following steps: The natural calcite washed with water is crushed to a first particle size range, rinsed with pure water and dried, calcined at a first temperature for a first set time, cooled and soaked in pure water for a second set time. During the soaking process, CO2 is introduced into the pure water, and then filtered to obtain a solid and dried to obtain the modified calcite. And / or, the modified magnesite is prepared by the following steps: The washed natural magnesite is crushed to a first particle size range, rinsed with pure water and dried, calcined at a second temperature for a first set time, cooled and soaked in pure water for a second set time, during which CO2 is introduced into the pure water, then filtered to obtain a solid and dried to obtain the modified magnesite. And / or, the modified dolomite is prepared by the following steps: The natural dolomite washed with water was crushed to the first particle size range, rinsed with pure water and dried, calcined at the third temperature for the first set time, cooled and soaked in pure water for the second set time. During the soaking process, CO2 was introduced into the pure water, and then filtered to obtain a solid and dried to obtain the modified dolomite. And / or, the modified brucite is prepared by the following steps: The natural brucite that has been washed with water is crushed to the first particle size range, rinsed with pure water and dried, calcined at a fourth temperature for a third set time, cooled and then soaked in pure water for a second set time. During the soaking process, CO2 is introduced into the pure water, and then the solid is filtered and dried to obtain the modified brucite.

5. The composite ore raw material for mineralized filter elements according to claim 4, characterized in that, The modified carnallite is prepared through the following steps: The natural carnallite that has been washed with water is crushed to the first particle size range, rinsed with pure water and dried, calcined at the third temperature for the first set time, cooled and soaked in pure water for the second set time. During the soaking process, a mixed gas of HCl and CO2 is introduced into the pure water. After drying and filtration, the modified carnallite is obtained. And / or, the modified forsterite is prepared by the following steps: The natural forsterite washed with water was crushed to the first particle size range, rinsed with pure water and dried, calcined at the fourth temperature for the third set time, cooled and sieved to obtain the modified forsterite. And / or, the modified serpentine is prepared by the following steps: The natural serpentine that has been washed with water is crushed to the first particle size range, rinsed with pure water and dried, calcined at the third temperature for the third set time, cooled and sieved to obtain the modified serpentine.

6. The composite ore raw material for mineralized filter elements according to claim 5, characterized in that, The first set time is 50 to 90 minutes; preferably, the first set time is 60 minutes. And / or, the second set time is 20 to 40 minutes; preferably, the second set time is 30 minutes; And / or, the third set time is 20 to 40 minutes; preferably, the third set time is 30 minutes; And / or, the first particle size range is 50 to 200 mesh; And / or, the first temperature is 800℃~900℃, preferably 850℃; And / or, the second temperature is 550°C to 650°C, preferably 600°C; And / or, the third temperature is 600℃~850℃, preferably 700℃~850℃; And / or, the fourth temperature is 400℃~850℃.

7. A mineralized filter element, characterized in that, The mineralized filter element comprises a composite ore raw material, an adsorbent, and a binder, wherein the adsorbent includes carbon powder, and the composite ore raw material is the composite ore raw material for the mineralized filter element as described in any one of claims 1 to 6.

8. The mineralized filter element according to claim 7, characterized in that, The mineralized filter element comprises, by weight, 21 to 70 parts of composite mineral raw material, 50 to 140 parts of adsorbent material, and 20 to 40 parts of binder.

9. The mineralized filter element according to claim 7 or 8, characterized in that, The adsorbent also includes cellulose carbon, and the weight ratio of the carbon powder to the cellulose carbon is (50-70):(60-70); And / or, the adhesive comprises one or more of food-grade polyethylene, food-grade polyvinyl chloride, food-grade polyvinyl alcohol, cellulose, and polylactic acid.

10. A method for preparing a mineralized filter element, used to prepare the mineralized filter element according to any one of claims 7 to 9, characterized in that, The preparation method includes the following steps: The composite ore raw material, adsorbent, and binder are mixed evenly to obtain a mixture; The mixture is processed into a mineralized filter element through sintering, extrusion, or wet carbon fiber processing.