A composite sustained-release material, its preparation method and application
By designing a composite slow-release material with a core and multi-layer coating structure, the problem of unstable release of active components was solved, achieving balanced release of active components and long-term pollutant treatment effect, thus improving the efficiency and effectiveness of environmental remediation.
Patent Information
- Application Number
- CN202510621878.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-15
- Publication Date
- 2026-11-17
AI Technical Summary
The release of active components in existing slow-release materials is unstable and the release rate is uneven, resulting in initial waste and reduced effectiveness in the later stages, which limits their application efficiency and effectiveness in environmental remediation.
A composite sustained-release material is designed, employing a core and multi-layer coating structure, with the active components decreasing layer by layer from the inside out. Combined with a honeycomb structure and layer-by-layer adjustment of pore size, a gradient distribution of active components is formed, with more active components from the inside to the outside.
It achieves balanced release of active components, maintains long-term pollutant treatment efficiency, avoids the reduction in later effects caused by excessive release in the early stage, and ensures the continuity and stability of environmental remediation.
Smart Images

Figure CN123105829A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of sustained-release materials technology, specifically to a composite sustained-release material, its preparation method, and its application. Background Technology
[0002] Slow-release materials are composite materials capable of controlling the continuous release of active components from pharmaceuticals, chemicals, fertilizers, and other substances over a prolonged period under suitable environmental conditions. These materials encapsulate the active components within a substrate, controlling the release rate through physical or chemical mechanisms. With the development of environmental remediation technologies, slow-release materials are increasingly being used in environmental protection, particularly in pollution control and remediation projects. For example, in addressing groundwater pollution, slow-release materials can be used to construct permeable reactive barriers (PRBs), which effectively intercept and remove harmful chemicals from passing groundwater. Through the continuous release of active components from slow-release materials, pollutants can be treated stably and over a long period, reducing secondary pollution to the environment.
[0003] However, in practical applications, traditional slow-release materials often face the problem of excessively rapid release of active components in the early stages and excessively slow release rates in the later stages. This uneven release dynamic may not only lead to the waste of active components in the initial stages but may also exacerbate side reactions due to excessively high concentrations of active components. Furthermore, the reduced release rate in the later stages results in excessively low concentrations of active components, reducing the environmental remediation effect. These problems limit the efficiency and effectiveness of slow-release materials in environmental remediation. Chinese patent document CN114229947B discloses a composite slow-release material for water pollution remediation. Although this material can achieve a slow-release time of 6 months, the mass transfer distance between the active substances and the outer surface of the material varies, resulting in an inability to achieve a balanced release effect. Chinese patent document CN104837790A uses a double-layer polymer film coating design to control the fertilizer release rate, but such organic polymer coating materials have high production costs and still suffer from the problem of uneven fertilizer release. Summary of the Invention
[0004] The technical problem to be solved by the present invention is to overcome the defects of unstable release of active components and uneven release rate in the prior art, thereby providing a composite sustained-release material that can be stably released in the environment, its preparation method and application.
[0005] Therefore, in a first aspect, the present invention provides a composite sustained-release material, wherein the active components decrease layer by layer from the inside to the outside. This feature can optimize the transport efficiency of the active components from the inner layer to the outer layer, reduce the situation where the active components are released too quickly in the outer layer and are not fully utilized in the inner layer, thereby achieving a more balanced release dynamic of the active components.
[0006] The composite sustained-release material is a basically spherical particle containing a core and n coating layers, where n is an integer from 1 to 8, preferably an integer from 1 to 5, and more preferably an integer from 2 to 3. The core and each coating layer contain an active component and a substrate, wherein the mass fraction of the active component in the nth layer is 70% to 90% of that in the (n-1)th layer. When (n-1) = 0, the coating layer is the core.
[0007] Furthermore, the active component in the core of the composite sustained-release material accounts for 40% to 95% of the total mass of the core, preferably 50% to 85%.
[0008] Furthermore, the total mass of the active component and the substrate in the nth coating layer is 70% to 100% of that in the (n-1)th layer, preferably 80% to 95%.
[0009] Furthermore, the mass ratio of the active component to the substrate in each coating layer is (0.1:1) to (10:1), preferably (0.3:1) to (8:1), and more preferably (0.5:1) to (4:1).
[0010] Furthermore, the composite sustained-release material has a honeycomb porous structure inside, with the maximum pore size of the core being approximately 1 to 1000 μm, preferably 100 to 500 μm, and the minimum pore size of the outermost layer being approximately 100 to 5000 nm, preferably 200 to 2000 nm. The average pore size distribution gradually decreases from the inside to the outside.
[0011] Furthermore, the outer diameter of the composite sustained-release material particles is approximately 2–10 mm.
[0012] The active component is selected from solid powdered substances that can decompose pollutants or provide support for pollutant degradation reactions, and usually has certain oxidizing or reducing properties, such as sodium persulfate, potassium persulfate, zero-valent iron powder, potassium permanganate, potassium ferrate, potassium dihydrogen phosphate, etc.; preferably, the active component is sodium persulfate and / or potassium dihydrogen phosphate.
[0013] The substrate is selected from chemically stable and biocompatible polymer materials, such as polystyrene, ethyl cellulose, polylactic acid, polyhydroxyalkanoate (PHA), polycaprolactone (PCL), etc.; preferably, the substrate is ethyl cellulose and / or polystyrene. The substrate ensures environmental safety and the economic efficiency of the treatment process.
[0014] In a second aspect, the present invention provides a method for preparing a multilayer composite sustained-release material, the method comprising:
[0015] S1: Mix the active components, substrate and organic solvent, granulate and dry to obtain core particles;
[0016] S2: Mix the active component, substrate and organic solvent to make a slurry. Mix the core particles with the slurry so that the slurry is uniformly attached to the particle surface. Dry to obtain particles containing a core and a coating layer. When n≥3, repeat the above process to increase the number of coating layers of the particles from 1 layer to n-1 layers.
[0017] S3: Mix the particles containing n-1 coating layers with the slurry, dry them, and obtain a composite slow-release material containing a core and n coating layers.
[0018] Wherein, n is an integer from 1 to 8, preferably an integer from 1 to 5, and more preferably an integer from 2 to 3. The mass fraction of the active component in the nth coating layer is 50% to 95% of that in the (n-1)th layer, preferably 70% to 90%.
[0019] Furthermore, the active component in the core of the composite sustained-release material accounts for 40% to 95% of the total mass of the core, preferably 50% to 85%.
[0020] Furthermore, the total mass of the active component and the substrate in the nth coating layer is 70% to 100% of that in the (n-1)th layer, preferably 80% to 95%.
[0021] Furthermore, the mass ratio of the active component to the substrate in each coating layer is (0.1:1) to (10:1), preferably (0.3:1) to (8:1), and more preferably (0.5:1) to (4:1).
[0022] In steps S2 and S3, the particles obtained in the previous step are mixed with the slurry obtained, and the mass ratio of the particles to the slurry attached to the particles is 6:1 to 1:1, preferably 5:1 to 2:1.
[0023] Furthermore, the drying temperature in steps S1 to S3 is not lower than 20°C below the boiling point of the organic solvent used, not higher than 80°C above the boiling point of the organic solvent used, and lower than the melting point and decomposition temperature of the coated component.
[0024] Preferably, in step S1, the drying temperature is 10 to 80°C above the boiling point of the organic solvent used, and more preferably 40 to 60°C above the boiling point of the organic solvent used.
[0025] Preferably, in step S2, the drying temperature of the outer layer is 5 to 30°C lower than that of the adjacent inner layer, more preferably 10 to 20°C lower. When n = 1, the adjacent inner layer is the core.
[0026] In a preferred embodiment, in step S3, the drying temperature of the outermost layer is 0 to 20°C below the boiling point of the organic solvent used.
[0027] In each coating step, the mass ratio of the amount of organic solvent to the total mass of the active component and the substrate is 1:5 to 1:20, preferably 1:10 to 1:15.
[0028] The active component is selected from solid powdered substances capable of decomposing pollutants or supporting pollutant degradation reactions, and typically possesses certain oxidizing or reducing properties, such as sodium persulfate, potassium persulfate, zero-valent iron powder, potassium permanganate, potassium ferrate, and potassium dihydrogen phosphate. Preferably, the active component is sodium persulfate and / or potassium dihydrogen phosphate.
[0029] The substrate is selected from one or more of chemically stable and biocompatible polymer materials, such as polystyrene, ethyl cellulose, polylactic acid, polyhydroxyalkanoate (PHA), and polycaprolactone (PCL). The substrate ensures environmental safety and the economic efficiency of the treatment process. Preferably, the substrate is ethyl cellulose and / or polystyrene.
[0030] The organic solvent is selected from low-boiling-point, highly volatile organic solvents, such as ethanol, dichloromethane, trichloromethane, tetrachloroethylene, acetone, and ethyl acetate. These solvents, due to their excellent evaporation rate and solubility, can effectively bind to the substrate and active components and rapidly evaporate during subsequent heating, thereby helping to form an ideal porous structure and coating effect. Preferably, the organic solvent is dichloromethane and / or ethyl acetate.
[0031] In a third aspect, the present invention provides the application of the multilayer composite slow-release material in water purification and soil remediation.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] (1) The present invention adopts a gradient configuration of internal active components, with more components distributed from the inside to the outside, combined with a unique design of internal pore structure that is wider from the inside to the outside. This structure optimizes the transport path of active components, and partially offsets the problem of release rate decline caused by increased transport path by increasing component content. This helps to maintain pollutant treatment efficiency for a long time and avoids the problem of reduced effect in the later stage due to excessive release in the early stage, thereby ensuring the continuity of environmental remediation and the stability of effect.
[0034] (2) Through repeated mixing, coating and drying steps, a multi-layered composite slow-release material is formed. By gradually reducing the mass ratio of active component to substrate in each layer from the inside out and adjusting the drying temperature, the pore structure of each layer gradually narrows from the inside out, and the content of active component decreases from high to low.
[0035] (3) Through precise formulation and process control, the present invention can significantly improve the release stability of active components in slow-release materials, and achieve a more efficient and continuous pollutant treatment effect in environmental remediation.
[0036] (4) The materials prepared by this invention are environmentally friendly and economical, making them an effective tool in the field of environmental protection.
[0037] Other features and advantages of the present invention will be described in detail in the following detailed description section. Attached Figure Description
[0038] The accompanying drawings are provided to further illustrate the invention and form part of the specification. They are used together with the following detailed description to explain the invention, but do not constitute a limitation thereof. In the drawings:
[0039] Figure 1 This is a cross-sectional scanning electron microscope image of the composite sustained-release material obtained in Example 1;
[0040] Figure 2 This is a cross-sectional scanning electron microscope (SEM) image of the Na element in the composite sustained-release material obtained in Example 1;
[0041] Figure 3 This is a cross-sectional scanning electron microscope image of the monolayer sustained-release material obtained in Comparative Example 1. Detailed Implementation
[0042] The technical solutions of this invention will be fully described below with reference to the embodiments thereof. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention. In the following embodiments, unless otherwise specified, commercially available chemical reagents are used, and there are no particular limitations in this regard.
[0043] Example 1
[0044] This embodiment describes a method for preparing a composite sustained-release material using sodium persulfate as the active component, ethyl cellulose as the base material, and dichloromethane (boiling point 40°C) as the organic solvent. This method utilizes layer-by-layer coating technology and progressively adjusts the concentration of the active component and the drying temperature to form a multilayered sustained-release material with optimized release performance. The specific preparation method is as follows:
[0045] S1: Mix sodium persulfate and ethyl cellulose powder (mass ratio 6:4), add dichloromethane and stir until a uniform dough-like mixture is formed. Granulate the mixture to form spherical particles with a particle size of approximately 4 mm. Place the obtained particles in an oven preheated to 80°C and dry to obtain core particles;
[0046] S2: Sodium persulfate and ethyl cellulose powder are mixed (mass ratio 5.4:4.6), dichloromethane is added, and the mixture is stirred until a uniform paste-like slurry is formed. The core particles obtained in S1 are mixed with the paste-like slurry at a mass ratio of 4:1, ensuring that the paste-like slurry basically uniformly covers the particle surface. The mixed particles are separated and dried at 60°C to obtain slow-release material particles containing a core and a coating layer.
[0047] S3: Sodium persulfate and ethyl cellulose powder are mixed (mass ratio 4.86:5.14), dichloromethane is added, and the mixture is stirred until a uniform paste-like slurry is formed. The sustained-release material particles obtained in S2 are mixed with the paste-like slurry at a mass ratio of 4:1, ensuring that the paste-like slurry basically uniformly covers the particle surface. The mixed particles are separated and dried at 50°C to obtain sustained-release material particles containing a core and a two-layer coating.
[0048] S4: Sodium persulfate and ethyl cellulose powder are mixed (4.37:5.23), dichloromethane is added, and the mixture is stirred until a uniform paste-like slurry is formed. The three-layered slow-release material particles obtained in S3 are mixed with the paste-like slurry at a mass ratio of 4:1, ensuring that the paste-like slurry basically uniformly covers the particle surface. The mixed particles are separated and dried at 40°C to obtain composite slow-release material particles containing a core and a three-layer coating, with an outer diameter of approximately 5.3–6.2 mm.
[0049] Example 2
[0050] This embodiment describes a method for preparing a composite sustained-release material using potassium dihydrogen phosphate as the active component, polystyrene as the coating substrate, and ethyl acetate (boiling point 77°C) as the organic solvent. This method utilizes layer-by-layer coating technology and progressively adjusts the concentration of the active component and the drying temperature to form a multilayer sustained-release material with optimized release performance. The specific preparation method is as follows:
[0051] S1: Mix potassium dihydrogen phosphate and polystyrene (mass ratio 8:2), add ethyl acetate and stir until a homogeneous dough-like mixture is formed. Granulate the mixture to form spherical particles with a particle size of 4 mm. Place the obtained particles in an oven preheated to 120°C and dry to obtain core particles;
[0052] S2: Potassium dihydrogen phosphate and polystyrene are mixed (mass ratio 6.8:3.2), ethyl acetate is added, and the mixture is stirred until a uniform paste-like slurry is formed. The inner layer slow-release material particles obtained in S1 are mixed with the paste-like slurry at a mass ratio of 3:1, ensuring that the paste-like slurry basically uniformly covers the particle surface. The mixed particles are separated and dried at 90°C to obtain particles containing a core and a coating layer.
[0053] S3: Potassium dihydrogen phosphate and polystyrene are mixed (mass ratio 5.78:4.22), ethyl acetate is added, and the mixture is stirred until a uniform paste-like slurry is formed. The two-layer slow-release material particles obtained in S2 are mixed with the paste-like slurry at a mass ratio of 3:1, ensuring that the paste-like slurry basically uniformly covers the particle surface. The mixed particles are separated and dried at 60°C to obtain composite slow-release material particles containing a core and a two-layer coating, with an outer diameter of approximately 4.9–5.6 mm.
[0054] Example 3
[0055] Composite sustained-release material particles were prepared according to the method of Example 1, except that the drying temperature of steps S1 to S4 was 80°C, that is, a composite material with the active component decreasing layer by layer from the inside to the outside but with uniform pore structure was constructed.
[0056] Comparative Example 1
[0057] This comparative example describes a method for preparing a sustained-release material using ethyl cellulose as the encapsulation substrate, sodium persulfate as the active component, and dichloromethane as the solvent. This comparative example employs a one-step granulation process to prepare a conventional sustained-release material; the specific preparation method is as follows:
[0058] Sodium persulfate was mixed with ethyl cellulose powder at a mass ratio of 6:4. A suitable amount of dichloromethane was added and stirred until a uniform dough-like substance was formed, followed by granulation. The resulting granules were placed in an oven preheated to 80°C and dried until the solvent was completely evaporated.
[0059] Comparative Example 2
[0060] Composite sustained-release material particles were prepared according to the method of Example 1, except that the mass ratio of sodium persulfate to ethyl cellulose powder in steps S2 to S4 remained consistent with that in step S1, i.e., the mass ratio was 6:4. A composite material with a progressively decreasing pore structure from the inside out, but with uniform active components, was constructed.
[0061] Test Example 1
[0062] The sustained-release materials obtained in Example 1 and Comparative Example 1 were subjected to scanning electron microscopy (SEM) testing (test conditions: carbon-sprayed coating, voltage 5.00 kV), and the results are as follows: Figure 1 , Figure 2 and Figure 3 As shown. Figure 1 The composite sustained-release material particles prepared in Example 1 exhibit a honeycomb structure with extremely abundant internal pores, and the pores gradually decrease in size from the inner layer to the outer layer. Figure 2 The content distribution of the effective active ingredients shows a gradient distribution trend from more at the inside to less at the outside. Figure 3The conventional sustained-release material prepared in Comparative Example 1 exhibits a rich pore structure, but the pore size does not show a gradient distribution. The effective active component is relatively uniformly distributed, without showing a gradient distribution trend.
[0063] Test Example 2: Performance Testing of Sustained-Release Materials
[0064] 10g of the sustained-release material obtained from each example and comparative example was mixed with 200g of medium sand and filled into an acrylic glass column with a height of 20cm and a diameter of 6cm. Distilled water was pumped into the acrylic glass column from bottom to top using a peristaltic pump at a rate of 0.5mL / min. The concentration of persulfate in the water at the outlet of the acrylic glass column was quantitatively measured using a UV spectrophotometer. The test period was 20 days, and the analytical results are shown in Table 1.
[0065] Table 1
[0066]
[0067] As can be seen from Table 1, compared with single-layer slow-release materials or materials that only construct a single gradient of pore size or active component, the composite slow-release materials obtained by constructing gradients of pore size and active component content exhibit more stable release of active components and longer residence time in water, demonstrating good release stability of active components.
[0068] The preferred embodiments of the present invention have been described in detail above with reference to the accompanying drawings. However, the present invention is not limited to the specific details of the above embodiments. Within the scope of the technical concept of the present invention, various simple modifications can be made to the technical solution of the present invention, and these simple modifications all fall within the protection scope of the present invention.
[0069] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not describe the various possible combinations separately.
[0070] Furthermore, various different embodiments of the present invention can be combined in any way, as long as they do not violate the spirit of the present invention, they should also be regarded as the content disclosed by the present invention.
Claims
1. A composite sustained-release material, wherein the composite sustained-release material is a particle containing a core and n coating layers, where n is an integer from 1 to 8; the core and each coating layer contain an active component and a substrate, wherein the mass fraction of the active component in the nth coating layer is 70% to 90% of that in the (n-1)th coating layer, and when (n-1) = 0, the coating layer is the core.
2. The sustained-release material according to claim 1, wherein, n is preferably an integer from 1 to 5, and more preferably an integer from 2 to 3.
3. The sustained-release material according to claim 1, wherein the active component in the core of the sustained-release material accounts for 40% to 95% of the total mass of the core, preferably 50% to 85%.
4. The sustained-release material according to claim 1, wherein, The total mass of the active component and the substrate in the nth coating layer is 70% to 100% of that in the (n-1)th layer, preferably 80% to 95%.
5. The sustained-release material according to claim 1, wherein, The mass ratio of active component to substrate in each coating layer is (0.1:1) to (10:1), preferably (0.3:1) to (8:1), and more preferably (0.5:1) to (4:1).
6. The sustained-release material according to claim 1, wherein the interior of the sustained-release material has a honeycomb porous structure, the maximum pore size of the core is 1-1000 μm, preferably 100-500 μm, the minimum pore size of the outermost layer is 100-5000 nm, preferably 200-2000 nm, and the average pore size distribution gradually decreases from the inside to the outside.
7. The sustained-release material according to claim 1, wherein the outer diameter of the sustained-release material particles is 2 to 10 mm.
8. The slow-release material according to claim 1, wherein the active component is selected from solid powder substances capable of decomposing pollutants or providing support for pollutant degradation reactions; preferably, the active component is selected from one or more of sodium persulfate, potassium persulfate, zero-valent iron powder, potassium permanganate, potassium ferrate, and potassium dihydrogen phosphate; more preferably, the active component is sodium persulfate and / or potassium dihydrogen phosphate.
9. The sustained-release material according to claim 1, wherein the substrate is selected from a polymer material with chemical stability and biocompatibility; preferably, the substrate is selected from one or more of polystyrene, ethyl cellulose, polylactic acid, polyhydroxyalkanoate, and polycaprolactone; more preferably, the substrate is ethyl cellulose and / or polystyrene.
10. A method for preparing a composite sustained-release material, the method comprising: S1: Mix the active components, substrate and organic solvent, granulate and dry to obtain core particles; S2: Mix the active component, substrate and organic solvent to make a slurry. Mix the core particles with the slurry so that the slurry is uniformly attached to the particle surface. Dry to obtain particles containing a core and a coating layer. When n≥3, repeat the above process to increase the number of coating layers of the particles from 1 layer to n-1 layers. S3: Mix the particles containing n-1 coating layers with the slurry and dry them to obtain a composite slow-release material containing a core and n coating layers; Where n is an integer from 1 to 8, and the mass fraction of the active component in the nth coating layer is 50% to 95% of that in the (n-1)th layer.
11. The method according to claim 10, wherein n is preferably an integer from 1 to 5, more preferably an integer from 2 to 3.
12. The method according to claim 10, preferably, the mass fraction of the active component in the nth layer is 70% to 90% of that in the (n-1)th layer.
13. The method according to claim 10, wherein the active component in the core in step S1 accounts for 40% to 95% of the total mass of the core, preferably 50% to 85%.
14. The method of claim 10, wherein, The total mass of the active component and the substrate in the nth coating layer is 70% to 100% of that in the (n-1)th layer, preferably 80% to 95%.
15. The method according to claim 10, wherein, The mass ratio of active component to substrate in each coating layer is (0.1:1) to (10:1), preferably (0.3:1) to (8:1), and more preferably (0.5:1) to (4:1).
16. The method of claim 10, wherein, In steps S2 and S3, the mass ratio of particles to slurry adhering to the particles is 6:1 to 1:1, preferably 5:1 to 2:
1.
17. The method according to claim 10, wherein the drying temperature in steps S1 to S3 is not lower than 20°C below the boiling point of the organic solvent used, not higher than 80°C above the boiling point of the organic solvent used, and lower than the melting point and decomposition temperature of the coated component.
18. The method according to claim 10, wherein, The drying temperature in step S1 is 10 to 80°C above the boiling point of the organic solvent used, preferably 40 to 60°C above the boiling point of the organic solvent used.
19. The method according to claim 10, wherein, In step S2, the drying temperature of the outer layer is reduced by 5 to 30°C compared to the drying temperature of the adjacent inner layer, preferably by 10 to 20°C. When n = 1, the adjacent inner layer is the core.
20. The method of claim 10, wherein, In step S3, the outermost drying temperature is 0–20°C below the boiling point of the organic solvent used.
21. The method according to claim 10, wherein, In steps S1 to S3, the mass ratio of the amount of organic solvent to the total mass of the active component and the substrate is 1:5 to 1:20, preferably 1:10 to 1:
15.
22. The method according to claim 10, wherein, The active component is selected from solid powder substances that can decompose pollutants or provide support for pollutant degradation reactions; preferably, the active component is selected from one or more of sodium persulfate, potassium persulfate, zero-valent iron powder, potassium permanganate, potassium ferrate, and potassium dihydrogen phosphate; more preferably, the active component is sodium persulfate and / or potassium dihydrogen phosphate.
23. The method according to claim 10, wherein, The substrate is selected from polymeric materials with chemical stability and biocompatibility; preferably, the substrate is selected from one or more of polystyrene, ethyl cellulose, polylactic acid, polyhydroxyalkanoate, and polycaprolactone; more preferably, the substrate is ethyl cellulose and / or polystyrene.
24. The method according to claim 10, wherein, The organic solvent is selected from low-boiling-point and highly volatile organic solvents; preferably, the organic solvent is selected from one or more of ethanol, dichloromethane, trichloromethane, tetrachloroethylene, acetone, and ethyl acetate; more preferably, the organic solvent is dichloromethane and / or ethyl acetate.
25. The composite sustained-release material prepared by the method according to any one of claims 10 to 24.
26. The application of the composite slow-release material according to any one of claims 1 to 9 or claim 25 in water purification or soil remediation.
Citation Information
Patent Citations
Manufacturing polymer coated controlled release fertilizers
CN104837790A
A composite sustained-release material, its preparation method and application
CN114229947B