Functional composite ceramsite for water treatment, its preparation method and application
By combining sludge conditioning, ceramsite sintering, and functional carbon layer loading, a porous ceramsite matrix was prepared and loaded with straw biochar and magnesium oxide microcrystals. This solved the problem of insufficient performance of ceramsite in the existing technology, and realized the resource utilization of sludge and straw and the effect of efficient water treatment.
Patent Information
- Application Number
- CN202611624877.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-20
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to effectively combine sludge conditioning, ceramsite sintering, and functional carbon layer loading in the process of preparing ceramsite for water treatment from sludge. This results in insufficient mechanical properties and water treatment capabilities of the ceramsite, and also fails to effectively utilize sludge and straw resources.
The porous ceramsite matrix is made by sintering dewatered sludge filter cake, lightly calcined magnesium oxide powder, clay and magnesium-modified straw powder. It is loaded with a functional carbon layer of straw biochar and magnesium oxide microcrystals. Through conditioning, granulation, sintering and the combination of functional carbon layer, magnesium aluminum spinel crystal phase is formed, which improves the mechanical properties and water treatment effect of ceramsite.
It realizes the resource utilization of sludge and straw, improves the ammonia nitrogen removal rate and mechanical strength of ceramsite, reduces the biochar loss rate, and has a highly efficient water treatment function.
Smart Images

Figure CN123105846A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of solid waste resource utilization and water treatment technology, especially multifunctional ceramsite and its preparation method. Background Technology
[0002] In modern urban wastewater treatment and large-scale aquaculture, the safe disposal of dewatered sludge and the purification of ammonia nitrogen and nitrite in aquaculture water are two major engineering requirements. Converting dewatered sludge into functional expanded clay pellets for water treatment not only achieves the reduction and resource recovery of large quantities of solid waste, but also provides a highly efficient biofilm carrier and purification matrix for high-load aquaculture water, offering both environmental benefits and engineering application value.
[0003] Currently, conventional sludge deep dewatering processes mainly rely on the addition of chemical flocculants such as polyaluminum chloride and polyacrylamide, supplemented by ordinary crop straw or sawdust as a physical framework to reduce the moisture content of the sludge cake and improve filter press performance. In the sludge resource utilization stage, dewatered sludge is often used as the main silica-alumina source, mixed with auxiliary materials such as fly ash and clay, and granulated and sintered at high temperature to produce ordinary lightweight ceramsite. In aquaculture water purification, the above-mentioned ordinary sintered ceramsite or commercial biological packing is often used as the attachment substrate for nitrification filters, or solid carbon source rods are additionally suspended in the system, and liquid organic carbon sources are added, in order to complete the oxidation of ammonia nitrogen and the reduction and denitrification of nitrate in different treatment units respectively.
[0004] In the process of preparing ceramsite for water treatment from sludge, the inorganic components introduced during the sludge conditioning stage, the matrix structure formed during the sintering stage, and the subsequent loading method of functional components need to be interconnected. For ceramsite using a post-loading method to introduce biochar, in addition to considering the amount of biochar introduced, it is also necessary to take into account the distribution of functional components within the pores, the retention performance after loading, and the water treatment performance of the ceramsite. Therefore, there is a need to provide a preparation method that combines sludge conditioning, ceramsite sintering, and post-loading of functional carbon layers, so as to obtain composite ceramsite with corresponding mechanical properties and water treatment functions while utilizing sludge and straw resources. Summary of the Invention
[0005] The purpose of this invention is to provide a functional composite ceramsite for water treatment, its preparation method, and its application, in order to solve the above-mentioned problems existing in the prior art.
[0006] To address the aforementioned problems in the existing technology, the present invention provides the following technical solution: A functional composite ceramsite for water treatment includes a porous ceramsite matrix and a functional carbon layer supported on the inner wall of its pores. The porous ceramsite matrix is prepared by sintering raw materials including dewatered sludge filter cake, lightly calcined magnesium oxide powder, clay, and coarsely graded magnesium-modified straw powder, and its phase contains a magnesium aluminum spinel crystal phase; the functional carbon layer contains straw biochar and magnesium oxide microcrystals.
[0007] The preparation method of the composite ceramsite includes: conditioning and mechanically dewatering sludge using fine-graded magnesium-modified straw powder, polyaluminum chloride, and cationic polyacrylamide; mixing the obtained dewatered sludge filter cake with lightly calcined magnesium oxide powder, clay, and coarse-graded magnesium-modified straw powder to form granules, drying, and sintering at 1000–1150℃ to obtain a porous ceramsite matrix; immersing the porous ceramsite matrix in a magnesium-modified straw biochar suspension containing magnesium chloride under negative pressure, soaking and draining under normal pressure, heat-treating at 500–550℃ for 2–3 hours under an inert protective atmosphere, and cooling to obtain the composite ceramsite.
[0008] Optionally, the aluminum-containing component includes an aluminum component conditioned from polyaluminum chloride, and the magnesium-containing component includes light-burned magnesium oxide powder; The raw materials for preparing the porous ceramsite matrix include, by mass parts: 50-75 parts of dewatered sludge filter cake, 5-15 parts of coarse-graded magnesium-modified straw powder, 10-25 parts of clay, 3-10 parts of lightly calcined magnesium oxide powder, and 0-10 parts of fly ash; wherein the moisture content of the dewatered sludge filter cake is 55%-62%.
[0009] According to another aspect of this application, a method for preparing the aforementioned functional composite ceramsite for water treatment is also provided, comprising the following steps: (1) Fine-graded magnesium-modified straw powder, polyaluminum chloride and cationic polyacrylamide were added to the sludge to be treated for conditioning, and the sludge was dewatered by mechanical dewatering to obtain dewatered sludge filter cake. (2) The dewatered sludge filter cake, lightly calcined magnesium oxide powder, clay and coarse-graded magnesium-modified straw powder are mixed and granulated to obtain raw material balls. The raw material balls are dried and sintered at 1000~1150℃ to obtain a porous ceramsite matrix. (3) The porous ceramsite matrix is placed under negative pressure and impregnated with magnesium-modified straw biochar suspension containing magnesium chloride. After soaking under normal pressure, it is drained. (4) The impregnated ceramsite is heat-treated at 500~550℃ for 2~3 hours under an inert protective atmosphere to form the functional carbon layer in situ on the pore wall surface of the porous ceramsite matrix. After cooling, the functional composite ceramsite for water treatment is obtained.
[0010] Optionally, the fine-graded magnesium-modified straw powder in step (1) has a particle size of less than 150 μm and is added at 5% to 20% of the dry weight of the sludge. The amount of polyaluminum chloride added, calculated as Al, is 0.5% to 2.0% of the dry weight of the sludge. The cationic polyacrylamide is added at a rate of 0.1% to 0.5% of the dry weight of the sludge. During the preparation process, add finely graded magnesium-modified straw powder in sequence and stir for 10-30 minutes, add polyaluminum chloride and stir for 2-5 minutes, and add cationic polyacrylamide and stir slowly for 5-15 minutes.
[0011] Optionally, the solid content of the magnesium-modified straw biochar suspension in step (3) is 5%~15%, and the biochar particle size D 90 For particles smaller than 10 μm, the magnesium chloride solution concentration should be 0.3–0.5 mol / L. During impregnation, first apply a vacuum to -0.07~-0.09MPa and maintain it for 10 minutes, then soak under normal pressure for 30~60 minutes; The inert protective atmosphere mentioned in step (4) is nitrogen atmosphere, the heat treatment temperature is 500~550℃, and the holding time is 2~3 hours.
[0012] Optionally, the coarse-graded magnesium-modified straw powder and the fine-graded magnesium-modified straw powder are obtained by crushing, grading and modifying crop straw by impregnation with magnesium chloride solution; The coarse-graded magnesium-modified straw powder passes through a 20-mesh sieve and is retained on a 40-mesh sieve, with a particle size of 425-850 μm. It is used for mixing and granulation in step (2) and forms pores through burn-off during the sintering process. The fine-graded magnesium-modified straw powder is passed through a 100-mesh sieve with a particle size of less than 150 μm and is used for sludge conditioning in step (1); the fine-graded magnesium-modified straw powder is then pyrolyzed and carbonized to prepare magnesium-modified straw biochar for step (3).
[0013] Optionally, the raw materials for preparing the porous ceramsite matrix include, by mass parts: The dewatered sludge filter cake comprises 50-75 parts of dewatered sludge filter cake, 5-15 parts of coarse-graded magnesium-modified straw powder, 10-25 parts of clay, 3-10 parts of lightly calcined magnesium oxide powder, and 0-10 parts of fly ash; the moisture content of the dewatered sludge filter cake is 55%-62%. The active MgO content of the lightly calcined magnesium oxide powder is not less than 65%, and the 200-mesh passing rate is not less than 85%.
[0014] Optionally, in step (3), the porous ceramsite matrix obtained in step (2) is placed in a vacuum impregnation tank, vacuumed to -0.07 to -0.09 MPa and maintained for 10 minutes, and the magnesium-modified straw biochar suspension is introduced for impregnation under the condition of maintaining negative pressure. After restoring normal pressure, it is soaked for 30 to 60 minutes and then drained. In step (4), the drained ceramsite is heated to 500-550°C under a nitrogen protective atmosphere and kept at that temperature for 2-3 hours. After cooling, the functional composite ceramsite for water treatment is obtained.
[0015] Optionally, the magnesium-modified straw biochar suspension is prepared by: pyrolyzing and carbonizing finely graded magnesium-modified straw powder at 500°C for 2 hours under nitrogen protection, and then grinding it to a particle size D. 90 <10μm, dispersed in 0.3~0.5mol / L MgCl2 aqueous solution at a solid content of 8%~12%, and a uniform suspension is prepared by ultrasonic dispersion and high-speed stirring.
[0016] Optionally, the sintering adopts a segmented heating process: heating from room temperature to 300-600℃ at 3-5℃ / min and holding for 20-30 minutes to complete the pre-decomposition of organic matter and the carbonization of straw to create pores; then heating to 1000-1100℃ at 5-10℃ / min and holding for 30-60 minutes to complete high-temperature sintering and the formation of magnesium aluminum spinel.
[0017] According to another aspect of this application, a functional composite ceramsite for water treatment prepared by any of the methods described above is also provided.
[0018] The above-mentioned functional composite ceramsite for water treatment is used in the purification of water quality in fish and shrimp farming. The composite ceramsite is used as a biological filter filler, a pond bottom conditioner, or an artificial wetland substrate.
[0019] The beneficial effects of this invention are as follows: This scheme combines sludge conditioning, ceramsite sintering, and post-loading with functional carbon layers. In the conditioning stage, polyaluminum chloride and magnesium-modified straw are used. The aluminum and magnesium components in the dewatered sludge filter cake participate in subsequent sintering along with the filter cake, resulting in a porous ceramsite matrix containing a magnesium-aluminum spinel crystal phase.
[0020] Under the listed experimental conditions, this scheme achieved the following results: (1) The fine-graded magnesium-modified straw powder was introduced during the conditioning stage, and the moisture content of the dehydrated filter cake was 55% to 62%, which was lower than 68% of Comparative Example 3 without the addition of this component; (2) The porous ceramsite matrix contained magnesium aluminum spinel crystal phase, and the compressive strength of the cylinder in the example was 3.6 to 6.5 MPa, taking into account both lightweight and mechanical strength; (3) After the introduction of the functional carbon layer, the ammonia nitrogen removal rate of Example 1 was 86.0%, which was higher than 52.0% of Comparative Example 4 without post-loading treatment, and the ammonia nitrogen and total phosphorus removal rates of each example were 74.0% to 86.5% and 65.0% to 74.0%, respectively; (4) The 24-hour biochar loss rate of the examples was 5.2% to 8.5%, of which Example 1 was 6.5% ± 1.2%, which was lower than 38.0% of Comparative Example 1 without magnesium modification of the front-end straw. At the same time, this scheme realized the resource utilization of sludge and straw. Attached Figure Description
[0021] Figure 1 These are the XRD diffraction patterns of Example 1 and Comparative Example 1 of the present invention, and the characteristic peak positions of MgAl2O4.
[0022] Figure 2 These are SEM images of the cross-sections of the composite materials in Embodiment 1 and Comparative Example 1 of the present invention.
[0023] Figure 3 This is a TEM image of magnesium oxide microcrystals in the functional carbon layer of Embodiment 1 of the present invention.
[0024] Figure 4 This is the Raman spectrum of the present invention. Detailed Implementation
[0025] Raw material pre-preparation: Preparation of magnesium-modified straw powder Corn stalks were washed to remove attached impurities, dried at 85℃, pulverized, and graded to obtain fine-graded straw powder with a particle size of less than 150 μm and coarse-graded straw powder with a particle size of 425–850 μm. The fine-graded and coarse-graded straw powders were then separately impregnated with magnesium chloride, without mixing them during impregnation.
[0026] Take 100.0 g of dried straw powder and add 2000 mL of 0.50 mol / L magnesium chloride aqueous solution. Stir and soak at 200 r / min for 24 hours at 25 ± 2℃. After soaking, filter to separate the solid and liquid. The obtained solid is not washed with water and is dried at 85℃ for 24 hours. If constant weight is not reached, continue drying. The drying endpoint is defined as the difference between two weighings taken 2 hours apart not exceeding 0.5% of the previous weight. After drying and cooling, perform slight depolymerization and verify the particle size to obtain fine-graded magnesium-modified straw powder and coarse-graded magnesium-modified straw powder, respectively, which are then sealed and stored.
[0027] Fine-graded magnesium-modified straw powder is used for sludge conditioning, and another fine-graded magnesium-modified straw powder obtained by the same method is used to prepare magnesium-modified straw biochar; coarse-graded magnesium-modified straw powder is used for granulation of ceramsite matrix. All the modified straw powders mentioned above are measured according to the mass of the modified product under specified dry conditions. This mass includes the magnesium-containing components retained in the modified product and is not replaced by the mass of the straw before modification.
[0028] Representative samples were taken from each batch of modified straw powder, and the total magnesium content was determined by ICP-OES after treatment with an appropriate digestion method, expressed in mg / g. The actual magnesium content in the modified product is based on the test results, and the amount of magnesium added in the impregnation solution is not directly used as the magnesium loading of the product.
[0029] Example 1: This example provides a functional composite ceramsite for water treatment.
[0030] The raw materials for preparing the porous ceramsite matrix, by mass parts, include: 65 parts dewatered sludge filter cake, 10 parts coarse-graded magnesium-modified straw powder, 18 parts clay, 5 parts lightly calcined magnesium oxide powder, and 2 parts fly ash. The dewatered sludge filter cake has a moisture content of 58%. The preparation method includes the following steps: (1) Fine-graded magnesium-modified straw powder, polyaluminum chloride, and cationic polyacrylamide were added to the sludge to be treated for conditioning. The fine-graded magnesium-modified straw powder was prepared according to the above-mentioned raw material pre-preparation method. The amount added was 10% of the dry weight of the sludge before conditioning, based on the mass of the modified product under the specified dry condition. The amount of polyaluminum chloride added, calculated as Al, was 1.0% of the dry weight of the sludge. The amount of cationic polyacrylamide added was 0.3% of the dry weight of the sludge. During conditioning, the fine-graded magnesium-modified straw powder was added and stirred in sequence, followed by the addition of polyaluminum chloride and stirring. Then, the cationic polyacrylamide was added and stirred slowly. After mechanical dewatering, a dewatered sludge filter cake with a moisture content of 58% was obtained.
[0031] Specifically, during conditioning, finely graded magnesium-modified straw powder was first added and stirred at 200 rpm for 20 minutes; then polyaluminum chloride was added and stirred at 200 rpm for 3 minutes; subsequently, cationic polyacrylamide was added and stirred at 40 rpm for 10 minutes. After conditioning, the mixture was filtered under 0.60 MPa pressure for 30 minutes, and the moisture content of the resulting filter cake was measured.
[0032] (2) The dewatered sludge filter cake, lightly calcined magnesium oxide powder, clay, fly ash, and coarse-graded magnesium-modified straw powder are mixed and granulated. The coarse-graded magnesium-modified straw powder is prepared by crushing corn straw, passing it through a 20-mesh sieve, retaining it on a 40-mesh sieve, and then impregnating it in a magnesium chloride solution for modification. Raw material balls are obtained, dried, and then sintered at 1050℃ for 40 minutes to obtain a porous ceramsite matrix.
[0033] In one embodiment, based on 10g per mass, 650g of dewatered sludge filter cake with a moisture content of 58%, 100g of coarse-graded magnesium-modified straw powder prepared according to the above-mentioned raw material pre-preparation method, 180g of clay, 50g of lightly calcined magnesium oxide powder, and 20g of fly ash are weighed. The above raw materials are mixed evenly, extruded, granulated, and rounded to form raw material balls. Raw material balls with a particle size of 4-6mm are sieved and dried at 105°C for 12 hours; if constant weight is not reached, drying continues.
[0034] The active MgO content of the lightly calcined magnesium oxide powder used was 68% (determined by the citric acid method), and the 200-mesh pass rate was 90%.
[0035] The dried raw material pellets were placed in a well-ventilated sintering furnace and sintered in air atmosphere for the first time. The temperature was increased to 500℃ at a rate of 3-5℃ / min and held for 30 minutes; then increased to 1050℃ at a rate of 5℃ / min and held for 40 minutes. After the holding period, the pellets were cooled in the furnace to obtain the sintered ceramsite matrix. Samples were collected for phase and composition analysis. No functional biochar was introduced at this stage for subsequent loading steps.
[0036] (3) The porous ceramsite matrix was placed under negative pressure and evacuated to -0.08 MPa for 10 minutes. The magnesium-modified straw biochar suspension was then impregnated and soaked at normal pressure for 40 minutes before being drained. The magnesium-modified straw biochar suspension was prepared by dispersing finely graded magnesium-modified straw powder in a 0.5 mol / L magnesium chloride solution after pyrolysis and carbonization at 500℃ for 2 hours under nitrogen protection.
[0037] Specific parameters can be as follows: Take fine-graded magnesium-modified straw powder prepared according to the above-mentioned raw material pre-preparation method, heat it to 500℃ at 10℃ / min under nitrogen protection, keep it at that temperature for 2 hours, cool it, and then grind it to obtain a particle size D. 90 Magnesium-modified straw biochar powder with a particle size of less than 10 μm.
[0038] Weigh 50.0 g of the above-mentioned biochar powder and add 450.0 g of magnesium chloride stock solution with a concentration of 0.50 mol / L. Disperse the solution under ultrasonic conditions of 40 kHz and nominal power of 200 W for 30 minutes, keeping the liquid temperature below 35℃ during dispersion. Then stir at 1000 r / min for 15 minutes to obtain a biochar suspension with a total mass of 500.0 g. The biochar mass fraction of the suspension is 10.0%, calculated as the ratio of the mass of biochar powder to the total mass of the suspension. Dissolved magnesium chloride in the stock solution is not included in the biochar mass.
[0039] Weigh 100.0g of dried ceramsite matrix, place it in a vacuum impregnation container, and evacuate to gauge pressure. Apply a pressure of 0.08 MPa and maintain it for 10 minutes; introduce the above suspension under negative pressure to completely submerge the ceramsite. Then slowly restore normal pressure and continue soaking for 40 minutes. Remove the ceramsite, place it on a sieve to drain for 10 minutes without washing with water, and collect the remaining suspension and leachate.
[0040] The suspension is prepared and used immediately, and stirred before being transferred and introduced into the impregnation container to ensure that the suspension entering the container is representative; the actual particle dispersion state and the entry into the pores are tested separately.
[0041] (4) The impregnated ceramsite is heat-treated at 520°C for 2.5 hours under a nitrogen atmosphere as an inert protective atmosphere to form a functional carbon layer in situ on the pore wall surface of the porous ceramsite matrix. After cooling, functional composite ceramsite for water treatment is obtained.
[0042] Specifically, the drained ceramsite is dried at 80°C for 12 hours to remove most of the free water, and then placed in a nitrogen-purified heat treatment furnace. Before heating, the furnace cavity is purged with nitrogen, and the amount of nitrogen introduced is no less than 5 times the effective volume of the furnace cavity; nitrogen is continuously introduced during heating, holding, and cooling.
[0043] The temperature was increased to 520℃ at a rate of 5℃ / min, and the time was started from the moment the set temperature was reached, and the temperature was held for 2.5 hours. After the holding period, the temperature was cooled to below 80℃ under nitrogen protection, removed, and sealed for storage, yielding composite ceramic particles for structural and compositional testing. The heat treatment exhaust gas was introduced into the alkali absorption device through a corrosion-resistant conduit.
[0044] Record the material quality before and after heat treatment, and retain the ceramic aggregate matrix from the same batch that was not impregnated but underwent the same post-heat treatment as a blank sample for subsequent composition and loading calculation.
[0045] The molar ratio of total MgO to total Al2O3 referred to in this article is calculated by converting the actual magnesium and aluminum content entering the sintering system into MgO and Al2O3 equivalents, respectively. The calculation includes magnesium and aluminum from the dewatered sludge filter cake and other feed components, and avoids double-counting of conditioning additives already included in the filter cake. This equivalent ratio describes the elemental composition of the formulation and is not directly equivalent to the phase ratio of free MgO to Al2O3 in the sintered product; the presence of free MgO is confirmed by product phase analysis.
[0046] The parts by mass in this specification represent the relative mass relationships between the raw materials, and it is not required that the total of all components be 100 parts. The dewatered sludge filter cake is measured according to its actual moisture content; the measurement status of other solid raw materials is described in the specific examples. The addition ratios of fine-graded magnesium-modified straw, polyaluminum chloride, and cationic polyacrylamide in the sludge conditioning stage are based on the dry matter mass of the sludge before conditioning; additives already added to the dewatered sludge filter cake are not counted again in subsequent formulation calculations.
[0047] In this application, the meaning of the net increase in organic carbon on the unit initial ceramsite matrix is: under the same batch and the same initial matrix mass, the mass and organic carbon mass fraction of the finished product and blank sample are determined respectively. ; in, The initial mass of the ceramic aggregate matrix added to each of the two groups; The quality of the finished product after loading; The mass of the blank matrix after undergoing the same heat treatment; and The values represent the organic carbon mass fractions for both components, expressed as decimals. The result is in gC / g matrix, which can be converted to mgC / g matrix by multiplying by 1000.
[0048] Ceramic aggregates of the same batch and with the same initial mass were used for functional layer loading tests and blank post-heat treatment tests. The resulting samples were subjected to consistent drying and weighing conditions, and the total carbon and inorganic carbon contents were determined. The difference between these two values yielded the organic carbon content. Based on the difference in organic carbon mass between the finished product and the blank sample, the net increase in organic carbon per unit initial ceramsite matrix was calculated. This indicator characterizes the net introduction of carbonaceous components and is not directly used as the mass of pure biochar or the chemical bonding ratio.
[0049] Example 2: This example provides a functional composite ceramsite for water treatment.
[0050] The raw materials for preparing the porous ceramsite matrix, by mass parts, include: 50 parts dewatered sludge filter cake, 5 parts coarse-graded magnesium-modified straw powder, 25 parts clay, 8 parts lightly calcined magnesium oxide powder, and 10 parts fly ash. The moisture content of the dewatered sludge filter cake is 55%.
[0051] The preparation method includes the following steps: (1) Fine-graded magnesium-modified straw powder, polyaluminum chloride, and cationic polyacrylamide were added to the sludge to be treated for conditioning. The fine-graded magnesium-modified straw powder was prepared from wheat straw and was added at 5% of the dry weight of the sludge; the polyaluminum chloride was added at 0.5% of the dry weight of the sludge (calculated as Al); and the cationic polyacrylamide was added at 0.1% of the dry weight of the sludge. After conditioning and mechanical dewatering, dewatered sludge filter cake was obtained.
[0052] (2) The dewatered sludge filter cake, lightly calcined magnesium oxide powder, clay, fly ash, and coarse-graded magnesium-modified straw powder are mixed and granulated. The coarse-graded magnesium-modified straw powder is prepared from wheat straw. Raw material balls are obtained, and after drying, they are sintered at 1000℃ to obtain a porous ceramsite matrix.
[0053] (3) The porous ceramsite matrix was placed under negative pressure and evacuated to -0.09 MPa for 10 minutes. It was then impregnated with magnesium-modified straw biochar suspension and soaked at normal pressure for 60 minutes before being drained. The magnesium chloride solution concentration of the suspension was 0.3 mol / L.
[0054] (4) The impregnated ceramsite is heat-treated at 500°C for 2 hours under a nitrogen atmosphere to form a functional carbon layer in situ on the pore wall surface of the porous ceramsite matrix. After cooling, functional composite ceramsite for water treatment is obtained.
[0055] Example 3: This example provides a functional composite ceramsite for water treatment.
[0056] The raw materials for preparing the porous ceramsite matrix include, by mass parts: 75 parts of dewatered sludge filter cake, 15 parts of coarse-graded magnesium-modified straw powder, 10 parts of clay, and 3 parts of lightly calcined magnesium oxide powder.
[0057] No fly ash was added in this embodiment. The moisture content of the dewatered sludge filter cake was 62%. The preparation method includes the following steps: (1) Fine-graded magnesium-modified straw powder, polyaluminum chloride, and cationic polyacrylamide were added to the sludge to be treated for conditioning. The fine-graded magnesium-modified straw powder was prepared from rice straw and was added at 20% of the dry weight of the sludge; the polyaluminum chloride was added at 2.0% of the dry weight of the sludge (calculated as Al); and the cationic polyacrylamide was added at 0.5% of the dry weight of the sludge. After conditioning and mechanical dewatering, dewatered sludge filter cake was obtained.
[0058] (2) The dewatered sludge filter cake, lightly calcined magnesium oxide powder, clay, and coarse-graded magnesium-modified straw powder are mixed and granulated. The coarse-graded magnesium-modified straw powder is prepared from rice straw. Raw material balls are obtained, and after drying, they are sintered at 1150℃ to obtain a porous ceramsite matrix.
[0059] (3) Place the porous ceramic matrix under negative pressure, evacuate to -0.07 MPa and maintain for 10 minutes, impregnate with magnesium-modified straw biochar suspension, soak under normal pressure for 30 minutes and then drain.
[0060] (4) The impregnated ceramsite is heat-treated at 550°C for 3 hours under a nitrogen atmosphere to form a functional carbon layer in situ on the pore wall surface of the porous ceramsite matrix. After cooling, functional composite ceramsite for water treatment is obtained.
[0061] Example 4: This example provides a functional composite ceramsite for water treatment, designed to provide verification of the sintering temperature boundary under single-factor variation.
[0062] The raw materials for preparing the porous ceramsite matrix, by mass, include: 65 parts dewatered sludge filter cake, 10 parts coarse-graded magnesium-modified straw powder, 18 parts clay, 5 parts lightly calcined magnesium oxide powder, and 2 parts fly ash. The moisture content of the dewatered sludge filter cake is 58%. The preparation method is the same as in Example 1, except that in step (2), the raw material pellets are dried and then sintered at 1000℃ to obtain the porous ceramsite matrix. All other preparation steps and parameters are completely consistent with those in Example 1.
[0063] Example 5: This example provides a functional composite ceramsite for water treatment, designed to provide boundary verification of heat treatment time with single-factor variation.
[0064] The raw materials for preparing the porous ceramsite matrix, by mass parts, include: 65 parts dewatered sludge filter cake, 10 parts coarse-graded magnesium-modified straw powder, 18 parts clay, 5 parts lightly calcined magnesium oxide powder, and 2 parts fly ash. The moisture content of the dewatered sludge filter cake is 58%.
[0065] The preparation method is the same as in Example 1, except that in step (4), the impregnated ceramsite is heat-treated at 520°C for 3 hours under a nitrogen atmosphere to form a functional carbon layer in situ on the pore wall surface of the porous ceramsite matrix. The remaining preparation steps and parameters are completely consistent with those in Example 1.
[0066] Example 6: This example provides a functional composite ceramsite for water treatment, designed to provide a cross-validation scheme for high organic matter components and high aluminum source agents.
[0067] The raw materials for preparing the porous ceramsite matrix, by weight, include: 75 parts dewatered sludge filter cake, 10 parts coarse-graded magnesium-modified straw powder, 10 parts clay, and 5 parts lightly calcined magnesium oxide powder. No fly ash was added in this embodiment. The moisture content of the dewatered sludge filter cake is 60%.
[0068] The preparation method includes the following steps: (1) Fine-graded magnesium-modified straw powder, polyaluminum chloride, and cationic polyacrylamide were added to the sludge to be treated for conditioning. The fine-graded magnesium-modified straw powder was prepared from corn straw and was added at 10% of the dry weight of the sludge; the polyaluminum chloride was added at 2.0% of the dry weight of the sludge (calculated as Al); and the cationic polyacrylamide was added at 0.3% of the dry weight of the sludge. After conditioning and mechanical dewatering, dewatered sludge filter cake was obtained.
[0069] (2) The dewatered sludge filter cake, lightly calcined magnesium oxide powder, clay and coarsely graded magnesium-modified straw powder are mixed and granulated. Raw material balls are obtained, and after drying, they are sintered at 1100℃ to obtain a porous ceramsite matrix.
[0070] (3) Place the porous ceramic matrix under negative pressure, evacuate to -0.08 MPa and maintain for 10 minutes, impregnate with magnesium-modified straw biochar suspension, soak under normal pressure for 40 minutes and then drain.
[0071] (4) The impregnated ceramsite is heat-treated at 520°C for 2.5 hours under a nitrogen atmosphere to form a functional carbon layer in situ on the pore wall surface of the porous ceramsite matrix. After cooling, functional composite ceramsite for water treatment is obtained.
[0072] Example 7: This example provides a functional composite ceramsite for water treatment, designed to provide a cross-validation scheme for a high inorganic substrate and a large amount of pore-forming agent.
[0073] The raw materials for preparing the porous ceramsite matrix, by mass parts, include: 50 parts dewatered sludge filter cake, 15 parts coarse-graded magnesium-modified straw powder, 25 parts clay, 8 parts lightly calcined magnesium oxide powder, and 2 parts fly ash. The dewatered sludge filter cake has a moisture content of 56%. The preparation method includes the following steps: (1) Fine-graded magnesium-modified straw powder, polyaluminum chloride, and cationic polyacrylamide were added to the sludge to be treated for conditioning. The fine-graded magnesium-modified straw powder was prepared from wheat straw and was added at 10% of the dry weight of the sludge; the polyaluminum chloride was added at 1.0% of the dry weight of the sludge (calculated as Al); and the cationic polyacrylamide was added at 0.3% of the dry weight of the sludge. After mechanical dewatering, dewatered sludge filter cake was obtained.
[0074] (2) The dewatered sludge filter cake, lightly calcined magnesium oxide powder, clay, fly ash and coarsely graded magnesium-modified straw powder are mixed and granulated. Raw material balls are obtained, and after drying, they are sintered at 1050℃ to obtain a porous ceramsite matrix.
[0075] (3) Place the porous ceramic matrix under negative pressure, evacuate to -0.08 MPa and maintain for 10 minutes, impregnate with magnesium-modified straw biochar suspension, soak under normal pressure for 40 minutes and then drain.
[0076] (4) The impregnated ceramsite is heat-treated at 520°C for 2.5 hours under a nitrogen atmosphere, and then cooled to obtain functional composite ceramsite for water treatment.
[0077] Example 8: This example provides a functional composite ceramsite for water treatment, designed to provide a cross-validation scheme of high skeleton support and low sintering temperature.
[0078] The raw materials for preparing the porous ceramsite matrix, by mass parts, include: 65 parts dewatered sludge filter cake, 5 parts coarse-graded magnesium-modified straw powder, 18 parts clay, 10 parts lightly calcined magnesium oxide powder, and 2 parts fly ash. The dewatered sludge filter cake has a moisture content of 57%. The preparation method includes the following steps: (1) Fine-graded magnesium-modified straw powder, polyaluminum chloride, and cationic polyacrylamide were added to the sludge to be treated for conditioning. The fine-graded magnesium-modified straw powder was prepared from rice straw and was added at 20% of the dry weight of the sludge; the polyaluminum chloride was added at 1.0% of the dry weight of the sludge (calculated as Al); and the cationic polyacrylamide was added at 0.3% of the dry weight of the sludge. After mechanical dewatering, dewatered sludge filter cake was obtained.
[0079] (2) The dewatered sludge filter cake, lightly calcined magnesium oxide powder, clay, fly ash and coarsely graded magnesium-modified straw powder are mixed and granulated. Raw material balls are obtained, and after drying, they are sintered at 1000℃ to obtain a porous ceramsite matrix.
[0080] (3) Place the porous ceramic matrix under negative pressure, evacuate to -0.08 MPa and maintain for 10 minutes, impregnate with magnesium-modified straw biochar suspension, soak under normal pressure for 40 minutes and then drain.
[0081] (4) The impregnated ceramsite is heat-treated at 520°C for 2.5 hours under a nitrogen atmosphere, and then cooled to obtain functional composite ceramsite for water treatment.
[0082] Comparative Example 1: Used to investigate the impact of changes in front-end straw magnesium salt modification treatment on the overall process and product performance.
[0083] Since this comparative ratio still adds lightly calcined magnesium oxide and retains the subsequent magnesium-containing impregnation step, it cannot be regarded as a magnesium-free control; its phase and load retention differences need to be analyzed in conjunction with the actual magnesium content, distribution and reaction state.
[0084] The raw materials for preparing the porous ceramsite matrix, by mass, include: 65 parts dewatered sludge filter cake, 10 parts coarse-graded ordinary corn stalk powder, 18 parts clay, 5 parts lightly calcined magnesium oxide powder, and 2 parts fly ash. The moisture content of the dewatered sludge filter cake is 62%. The preparation method is the same as in Example 1, except that in step (1) conditioning and step (2) granulation, the magnesium-modified straw powder is replaced with an equal amount of ordinary corn stalk powder that has not been impregnated with magnesium chloride solution. All other preparation steps and parameters are completely consistent with Example 1.
[0085] This comparative example changed the magnesium modification state of the straw used in steps (1) and (2), but still retained the addition of lightly burned magnesium oxide and subsequent impregnation with magnesium-containing biochar suspension, in order to investigate the impact of changes in the front-end straw magnesium modification treatment on the overall process and product performance.
[0086] Comparative Example 2: Used to examine the overall impact of replacing polyaluminum chloride with polyferric sulfate.
[0087] The raw materials for preparing the porous ceramsite matrix, by mass parts, include: 65 parts dewatered sludge filter cake, 10 parts coarse-graded magnesium-modified straw powder, 18 parts clay, 5 parts lightly calcined magnesium oxide powder, and 2 parts fly ash. The moisture content of the dewatered sludge filter cake is 59%.
[0088] The preparation method is the same as in Example 1, except that: in step (1), polyaluminum chloride is not added, but polyferric sulfate is used instead, and the amount of polyferric sulfate added, calculated as Fe, is 1.0% of the dry weight of the sludge. The remaining preparation steps and parameters are completely consistent with those in Example 1. Compared with Example 1, this comparative example uses polyferric sulfate instead of polyaluminum chloride in the dehydration stage. This comparative example is used to investigate the comprehensive effect of replacing polyaluminum chloride with polyferric sulfate in the conditioning stage; the aluminum in the raw material system can still be provided by components such as sludge, clay and fly ash.
[0089] Comparative Example 3: Used to investigate the changes in sludge dewatering and final ceramsite performance when no fine-graded magnesium-modified straw powder is added during the conditioning stage.
[0090] The raw materials for preparing the porous ceramsite matrix, by mass parts, include: 65 parts dewatered sludge filter cake, 10 parts coarse-graded magnesium-modified straw powder, 18 parts clay, 5 parts lightly calcined magnesium oxide powder, and 2 parts fly ash. The moisture content of the dewatered sludge filter cake obtained in this comparative example is 68%.
[0091] The preparation method is the same as in Example 1, except that in step (1), only polyaluminum chloride and cationic polyacrylamide are added to the sludge to be treated for conditioning, and fine-graded magnesium-modified straw powder is not added. The remaining preparation steps and parameters are completely consistent with those in Example 1. This comparative example reflects the overall effect of removing the conditioning component. Since the moisture content of the filter cakes of the two groups of dewatered sludge is different, the cake mass corresponding to the same wet mass fraction is also different.
[0092] Comparative Example 4: A porous ceramic aggregate matrix without functional carbon layer post-loading treatment is provided to investigate the comprehensive effects of vacuum impregnation and subsequent heat treatment on material properties.
[0093] The raw materials for preparing the porous ceramsite matrix include, by mass parts: 65 parts of dewatered sludge filter cake, 10 parts of coarse-graded magnesium-modified straw powder, 18 parts of clay, 5 parts of lightly calcined magnesium oxide powder, and 2 parts of fly ash.
[0094] The moisture content of the dewatered sludge filter cake was 58%. The preparation method was the same as in Example 1, except that after completing the mechanical dewatering in step (1) and the high-temperature sintering in step (2) to prepare the matrix ceramic particles, the obtained porous ceramic particle matrix was directly used as the finished product, without performing the vacuum impregnation in step (3) and the low-temperature heat treatment in step (4). Compared with Example 1, this comparative example omitted steps (3) and (4) and did not introduce the functional carbon layer formed by the above post-loading treatment.
[0095] Comparative Example 5: The maximum sintering temperature and holding time were changed simultaneously, and the results were used to compare the differences in overall performance between the two groups of sintering conditions.
[0096] If it is necessary to further confirm the independent influence of the maximum sintering temperature and the basis for selecting the upper limit, a temperature comparison should be conducted under the same conditions.
[0097] The raw materials for preparing the porous ceramsite matrix, by mass fraction, include: 65 parts dewatered sludge filter cake, 10 parts coarse-graded magnesium-modified straw powder, 18 parts clay, 5 parts lightly calcined magnesium oxide powder, and 2 parts fly ash. The moisture content of the dewatered sludge filter cake is 58%. The preparation method is the same as in Example 1, except that in step (2), the raw material balls are dried and then sintered at 1200℃ for 30 minutes to obtain the porous ceramsite matrix. All other preparation steps and parameters are completely consistent with Example 1. This comparative example uses a sintering condition of 1200℃ and 30 minutes, compared with the 1050℃ and 40 minutes sintering condition used in Example 1, to evaluate the differences in material properties corresponding to the two sintering regimes.
[0098] This scheme utilizes straw in a graded manner. Fine-graded magnesium-modified straw powder is used for sludge conditioning and as a raw material for preparing magnesium-modified straw biochar; coarse-graded magnesium-modified straw powder participates in the preparation of raw material pellets, and its loss during sintering is used to form pores. The aluminum and magnesium components entering the dewatered sludge filter cake, together with the inorganic components in other raw materials, participate in subsequent sintering.
[0099] In the functional carbon layer loading process, a magnesium-modified straw biochar suspension containing magnesium chloride is introduced into the accessible channels of a porous ceramsite matrix. After atmospheric pressure soaking and draining, it undergoes inert atmosphere heat treatment. When water is present in residual water or hydrated magnesium salts, the magnesium salts can undergo hot hydrolysis and dechlorination to form a magnesium-containing phase containing magnesium oxide. The simplified overall reaction can be expressed as: MgCl2+H2O→MgO+2HCl↑; From the perspective of interfacial interactions, oxygen-containing sites on the surface of biochar can interact with magnesium centers in magnesium-containing components, and the possible connection forms include Mg–O–C. This connection is used to describe an interfacial bonding mode between biochar and magnesium-containing components, and the formation of functional carbon layers and their loading on the inner walls of pores are not limited to a single coordination configuration.
[0100] Under biofilm formation conditions, the distribution of dissolved oxygen within the pores is influenced by the external dissolved oxygen concentration, pore structure, biofilm state, and microbial oxygen consumption. The sieved particle size of the coarse-graded straw is used to define the pore-forming material and is not directly used as a numerical value for the product pore depth or oxygen penetration depth.
[0101] To further demonstrate the necessity and beneficial effects of the technical features of this application, performance tests were conducted on Examples 1-8 and Comparative Examples 1-5. The specific test methods are as follows: 1. Moisture content of the filter cake after dehydration (%) Test method: Drying method Specific steps: (1) Sampling: Weigh about 3g of dehydrated filter cake sample into a weighing bottle (or petri dish) that has been pre-weighed, and record the total mass. .
[0102] (2) Drying: Place the sample in a forced-air drying oven and dry it to constant weight at 105±5℃. Generally, drying takes more than 8 hours. The constant weight standard can be referenced as follows: the mass difference between two adjacent weighings (with an interval of not less than 2 hours) should not exceed 0.1%.
[0103] (3) Weighing: Take out the dried sample, put it in a desiccator to cool to room temperature, and weigh the total mass of the remaining dried solid and the container. .
[0104] (4) Calculate the moisture content: .
[0105] 2. Bulk density (kg / m³) Test method: Natural stacking method Specific steps: (1) Dry the sample in an oven at 105~110℃ until constant weight. Prepare a volumetric cylinder with a known volume (e.g., 1L) and weigh the empty cylinder.
[0106] (2) Pass the sample through a standard funnel or scoop, allowing it to fall freely into the measuring cylinder from a height of about 50 mm from the opening without any external force. The sample should be filled to the brim and extend beyond the opening of the measuring cylinder.
[0107] (3) Use a ruler or scraper to scrape off the excess sample along the mouth of the measuring cylinder so that the sample surface is flush with the mouth of the cylinder. Be careful not to compact or vibrate the sample.
[0108] (4) Weigh the total mass of the volumetric cylinder filled with the sample.
[0109] (5) Calculate the bulk density. Bulk density (kg / m3) = (Total mass) / (Total mass) (empty cylinder mass) / capacity cylinder volume.
[0110] 3. Cylinder compressive strength (MPa) Test method: Pressure cylinder method Specific steps: (1) Weigh a certain amount of sample according to the standard requirements and put it into a steel pressure cylinder.
[0111] (2) Use a wooden mallet to tap the sample around the cylinder several times to make the sample naturally compact inside the cylinder.
[0112] (3) Install the guide tube and the stamping die. Check whether the lower scale line of the stamping die coincides with the upper edge of the guide tube; if they do not coincide, continue to tap the tube wall gently until they coincide completely.
[0113] (4) Place the pressure cylinder on the lower platen of the pressure testing machine and apply it at a constant speed of about 30~50 kg per second (about 0.3~0.5 kN / s).
[0114] (5) When the stamping die reaches a depth of 20mm, record the pressure value at this time.
[0115] (6) Calculate the cylinder compressive strength. Cylinder compressive strength = pressure value / bearing area.
[0116] 4.1h water absorption rate (%) Test method: Gravimetric method Specific steps: (1) Dry the sample in an oven at 105±5℃ to constant weight, and weigh the dry weight after cooling. Accurate to 0.1g; (2) Immerse the dried sample completely in distilled water or deionized water at 20±5℃, with the liquid level at least 20mm above the sample, and soak for 60min. (3) Remove the sample from the water and immediately wipe away the water adhering to the surface with a wrung-out wet towel (or wet cloth) until there is no visible water or water droplets on the surface; (4) Quickly weigh the wet weight of the sample after it has been wiped dry. ; (5) Calculate the water absorption rate in 1 hour: .
[0117] 5. Ammonia nitrogen removal rate (%) Test method: Nessler's reagent spectrophotometry Specific steps: (1) Contact a certain amount of filter material sample with a nitrogen-containing solution of known concentration (e.g., 10 mg / L) (e.g., constant temperature oscillation), and filter after adsorption for a certain period of time; (2) Take a certain amount of filtrate into a 50mL colorimetric tube, add 1.0mL of potassium sodium tartrate solution (to mask interfering ions), mix well; then add 1.0~1.5mL of Nessler's reagent and shake well.
[0118] (3) Let it stand for 10 minutes to allow the color reaction to develop; (4) At a wavelength of 420 nm, the absorbance was measured using a 10 mm optical path cuvette with a blank as a reference. (5) Calculate the residual ammonia nitrogen concentration in the filtrate based on the pre-drawn standard curve; (6) Calculate the ammonia nitrogen removal rate. Ammonia nitrogen removal rate (%) = (initial ammonia nitrogen concentration) / (initial ammonia nitrogen concentration) (Residual ammonia nitrogen concentration) / Initial ammonia nitrogen concentration × 100%.
[0119] 6. Total phosphorus removal rate (%) Test method: Molybdenum antimony spectrophotometry Specific steps: (1) Contact the filter material sample with a phosphorus-containing solution of known concentration (25℃, 120r / min constant temperature shaking for 24h), and then filter it; (2) Take an appropriate amount of filtrate into a colorimetric tube, add potassium persulfate to digest it, and convert various forms of phosphorus into orthophosphate; (3) Add ascorbic acid and molybdate solution to the digested sample in sequence and mix thoroughly; (4) Let it stand for 15 minutes to allow the color reaction to develop; (5) Measure the absorbance at a wavelength of 700 nm, using a blank as a reference; (6) Calculate the residual total phosphorus concentration in the filtrate based on the standard curve; (7) Calculate the total phosphorus removal rate. Total phosphorus removal rate (%) = (initial total phosphorus concentration) / (initial total phosphorus concentration) (Residual total phosphorus concentration) / Initial total phosphorus concentration × 100%.
[0120] 7. Detection of MgAl2O4 spinel phase Test method: X-ray diffraction (XRD) Specific steps: (1) Grind the sample into fine powder (usually requiring a particle size <75μm) and press it into a flat sample sheet; (2) Place the sample sheet into the X-ray diffractometer, set the scanning parameters (such as scanning range 2θ=10°~80°, step size 0.02°), and perform scanning; (3) Obtain the XRD diffraction pattern of the sample and record the 2θ angle and intensity of each diffraction peak; (4) Compare the diffraction peaks of the sample with the standard PDF card (such as the standard card of MgAl2O4); (5) If the diffraction pattern of the sample shows a characteristic peak corresponding to the MgAl2O4 standard card, it is judged as "present"; otherwise, it is "absent". Detailed test parameters are shown in Tables 1 to 4 below: Table 1 Experimental parameters for the embodiments
[0121] Table 2. Experimental parameters for the comparative examples.
[0122] Table 3 Experimental Data Table of Examples
[0123] The reported 24-hour biochar loss rates for each of the examples listed in Table 3 range from 5.2% to 8.5%, with Example 1 showing 6.5% ± 1.2%. These results reflect short-term retention under the immersion conditions used and do not directly represent retention performance under long-term hydraulic flushing conditions.
[0124] The compressive strength of the cylinders in the examples listed in Table 3 ranges from 3.6 to 6.5 MPa. In this scheme, after the porous ceramsite matrix is prepared, a functional carbon layer is introduced through negative pressure impregnation and inert atmosphere heat treatment. Under the listed test conditions, the ammonia nitrogen removal rate of Example 1 is 86.0%, which is higher than the 52.0% of Comparative Example 4 without the above post-loading treatment, indicating that the composite ceramsite corresponding to the above post-loading treatment has a higher ammonia nitrogen removal rate.
[0125] Table 4. Experimental data of the comparative examples
[0126] like Figures 1 to 3 As shown, the comparison between Example 1 and Comparative Example 1 indicates that, under the listed test conditions, changes in the magnesium modification state of the front-end straw are accompanied by changes in filter cake moisture content, product phase analysis results, and biochar retention performance. The reported 24-hour biochar loss rate for Example 1 was 6.5% ± 1.2%, while that for Comparative Example 1 was 38.0%. Since Comparative Example 1 still contains other magnesium sources, this comparison reflects the comprehensive impact of changes in the front-end straw magnesium modification treatment and is not a comparison between magnesium-free and magnesium-containing materials.
[0127] A comparison of Example 1 and Comparative Example 2 shows that after replacing polyaluminum chloride with polyferric sulfate, the filter cake moisture content decreased from 58.0% to 59.0%, the ammonia nitrogen removal rate decreased from 86.0% to 70.0%, the total phosphorus removal rate decreased from 71.1% to 88.0%, and the cylinder compressive strength decreased from 4.6 MPa to 4.7 MPa. These results indicate that the two groups of materials differ in different performance indicators, and it cannot be concluded that one group is superior to the other in all performance aspects.
[0128] No MgAl2O4 spinel phase was detected in Comparative Example 1, and its spinel content was below the detection limit of X-ray diffraction. The specific reasons need to be further confirmed by combining the distribution of magnesium and the quantitative results of phase composition.
[0129] like Figure 4 As shown, Example 1 was tested at 310, 410, 670, and 731 cm. - A distinct MgAl2O4 spinel characteristic peak appears at position ¹, while Comparative Example 1 shows almost no such peak, indicating that under the listed conditions, the spinel content in Comparative Example 1 is below the detection limit; simultaneously, the D peak (1354 cm⁻¹) of Example 1... - ¹) and G peak (1586cm) - ¹) The intensity is much higher than that of Comparative Example 1, indicating that the Raman signal intensity of the carbonaceous component in Example 1 is higher than that in Comparative Example 1 (the D / G intensity ratios of the two are similar, and the spectra are translated and superimposed, so the absolute intensity is only for reference). This result is consistent with its lower 24-hour biochar loss rate. The Raman results are consistent with the XRD and ammonia nitrogen removal data, which can provide supplementary evidence for the existence of the functional carbon layer.
[0130] A comparison of Example 1 and Comparative Example 3 shows that when fine-graded magnesium-modified straw powder is not added during the conditioning stage, the moisture content of the resulting filter cake changes from 58.0% to 68.0%, the 1-hour water absorption rate of the final ceramsite changes from 18.0% to 12.0%, and the ammonia nitrogen removal rate changes from 86.0% to 58.0%. This comparison is used to evaluate the overall process results after the conditioner component is removed; the difference in dry matter mass corresponding to the same wet mass fraction of filter cake also reflects the difference in the state of the two groups of subsequent sintering raw materials.
[0131] A comparison of Example 1 and Comparative Example 4 shows that Example 1, after vacuum impregnation and post-loading heat treatment, achieved an ammonia nitrogen removal rate of 86.0%, while Comparative Example 4, without the aforementioned post-loading treatment, achieved 52.0%. This result indicates that, under the experimental conditions employed, the material incorporating the aforementioned post-loading treatment exhibits a higher ammonia nitrogen removal rate. This comparison is not intended to differentiate the contributions of adsorption, bioconversion, and other processes, nor does it substitute the ammonia nitrogen removal rate for the total nitrogen removal effect.
[0132] A comparison of Example 1 and Comparative Example 5 shows that after sintering at 1200℃ for 30 minutes, the compressive strength of the ceramsite cylinder is 7.5 MPa, the water absorption rate after 1 hour is 8.0%, and the ammonia nitrogen removal rate is 65.0%. For Example 1, sintering at 1050℃ for 40 minutes, the corresponding indicators are 4.6 MPa, 18.0%, and 86.0%, respectively. These results reflect the differences in mechanical properties, water absorption, and water treatment performance under the two sintering conditions and are not considered as a single-factor experiment independently affecting the highest sintering temperature.
[0133] Example 6 used 75 parts dewatered sludge filter cake, 10 parts clay, and 2.0% polyaluminum chloride (calculated as Al) added during the conditioning stage. The compressive strength was 4.1 MPa, the ammonia nitrogen removal rate was 84.5%, and a magnesium aluminum spinel phase was detected. These results reflect the material properties under the listed cross-formulation and process conditions.
[0134] Example 7 uses 50 parts dewatered sludge filter cake, 25 parts clay, and 15 parts coarse-graded magnesium-modified straw powder. Its compressive strength is 5.8 MPa, water absorption rate is 17.0% in 1 hour, and ammonia nitrogen removal rate is 77.0%. The above results are used to describe the mechanical, water absorption, and water treatment properties of this formulation, and do not directly infer the pore depth or internal anoxic zones based on the water absorption rate.
[0135] Example 8 used a 20% fine-graded magnesium-modified straw powder addition ratio during the conditioning stage, 10 parts of lightly calcined magnesium oxide powder, and sintering conditions of 1000℃. The resulting filter cake had a moisture content of 57.0%, a compressive strength of ceramsite cylinder of 4.8 MPa, and a total phosphorus removal rate of 70.0%. These results reflect the feasibility of the above formulation and sintering conditions combination and are not attributed solely to the fluxing or alkalinity buffering effect of any single component.
Claims
1. A functional composite ceramsite for water treatment, comprising a porous ceramsite matrix and a functional carbon layer distributed within the pores of the porous ceramsite matrix, characterized in that, include: The porous ceramsite matrix is obtained by sintering raw materials including dewatered sludge filter cake, aluminum-containing components, magnesium-containing components and clay, and the phase of the porous ceramsite matrix includes magnesium aluminum spinel crystal phase. The dewatered sludge filter cake is obtained by conditioning sludge with fine-graded magnesium-modified straw powder, polyaluminum chloride and cationic polyacrylamide and then mechanically dewatering it; The functional carbon layer comprises straw biochar and magnesium oxide microcrystals, and is formed by the following process: the porous ceramsite matrix is immersed in a magnesium-modified straw biochar suspension containing magnesium chloride under negative pressure, and after being soaked and drained under normal pressure, it is heat-treated at 500-550℃ for 2-3 hours under an inert protective atmosphere.
2. The functional composite ceramsite for water treatment according to claim 1, characterized in that, The aluminum-containing component includes aluminum components conditioned from polyaluminum chloride, and the magnesium-containing component includes light-burned magnesium oxide powder; The raw materials for preparing the porous ceramsite matrix include, by mass parts: 50-75 parts of dewatered sludge filter cake, 5-15 parts of coarse-graded magnesium-modified straw powder, 10-25 parts of clay, 3-10 parts of lightly calcined magnesium oxide powder, and 0-10 parts of fly ash; wherein the moisture content of the dewatered sludge filter cake is 55%-62%.
3. A method for preparing the functional composite ceramsite for water treatment as described in claim 1, characterized in that, Includes the following steps: (1) Fine-graded magnesium-modified straw powder, polyaluminum chloride and cationic polyacrylamide were added to the sludge to be treated for conditioning, and the sludge was dewatered by mechanical dewatering to obtain dewatered sludge filter cake. (2) The dewatered sludge filter cake, lightly calcined magnesium oxide powder, clay and coarse-graded magnesium-modified straw powder are mixed and granulated to obtain raw material balls. The raw material balls are dried and sintered at 1000~1150℃ to obtain a porous ceramsite matrix. (3) The porous ceramsite matrix is placed under negative pressure and impregnated with magnesium-modified straw biochar suspension containing magnesium chloride. After soaking under normal pressure, it is drained. (4) The impregnated ceramsite is heat-treated at 500~550℃ for 2~3 hours under an inert protective atmosphere to form the functional carbon layer in situ on the pore wall surface of the porous ceramsite matrix. After cooling, the functional composite ceramsite for water treatment is obtained.
4. The method according to claim 3, characterized in that, The fine-graded magnesium-modified straw powder mentioned in step (1) has a particle size of less than 150 μm and is added at a rate of 5% to 20% of the dry weight of the sludge. The amount of polyaluminum chloride added, calculated as Al, is 0.5% to 2.0% of the dry weight of the sludge. The cationic polyacrylamide is added at a rate of 0.1% to 0.5% of the dry weight of the sludge. During the preparation process, add finely graded magnesium-modified straw powder in sequence and stir for 10-30 minutes, add polyaluminum chloride and stir for 2-5 minutes, and add cationic polyacrylamide and stir slowly for 5-15 minutes.
5. The method according to claim 3 or 4, characterized in that, The magnesium-modified straw biochar suspension mentioned in step (3) has a solid content of 5%~15% and a biochar particle size D. 90 For particles smaller than 10 μm, the magnesium chloride solution concentration should be 0.3–0.5 mol / L. During impregnation, first apply a vacuum to -0.07~-0.09MPa and maintain it for 10 minutes, then soak under normal pressure for 30~60 minutes; The inert protective atmosphere mentioned in step (4) is nitrogen atmosphere, the heat treatment temperature is 500~550℃, and the holding time is 2~3 hours.
6. The method according to claim 3, characterized in that, The coarse-graded magnesium-modified straw powder and the fine-graded magnesium-modified straw powder are prepared by crushing, grading and impregnating crop straw with magnesium chloride solution. The coarse-graded magnesium-modified straw powder passes through a 20-mesh sieve and is retained on a 40-mesh sieve, with a particle size of 425-850 μm. It is used for mixing and granulation in step (2) and forms pores through burn-off during the sintering process. The fine-graded magnesium-modified straw powder is passed through a 100-mesh sieve with a particle size of less than 150 μm and is used for sludge conditioning in step (1); the fine-graded magnesium-modified straw powder is then pyrolyzed and carbonized to prepare magnesium-modified straw biochar for step (3).
7. The method according to claim 5, characterized in that, The raw materials for preparing the porous ceramsite matrix include, by mass parts: The dewatered sludge filter cake comprises 50-75 parts of dewatered sludge filter cake, 5-15 parts of coarse-graded magnesium-modified straw powder, 10-25 parts of clay, 3-10 parts of lightly calcined magnesium oxide powder, and 0-10 parts of fly ash; the moisture content of the dewatered sludge filter cake is 55%-62%. The active MgO content of the lightly calcined magnesium oxide powder is not less than 65%, and the 200-mesh passing rate is not less than 85%.
8. The method according to claim 3, characterized in that, In step (3), the porous ceramsite matrix obtained in step (2) is placed in a vacuum impregnation tank, vacuumed to -0.07 to -0.09 MPa and maintained for 10 minutes, and the magnesium-modified straw biochar suspension is introduced for impregnation under the condition of maintaining negative pressure. After restoring normal pressure, it is soaked for 30 to 60 minutes and then drained. In step (4), the drained ceramsite is heated to 500-550°C under a nitrogen protective atmosphere and kept at that temperature for 2-3 hours. After cooling, the functional composite ceramsite for water treatment is obtained.
9. The method according to claim 8, characterized in that, The preparation method of the magnesium-modified straw biochar suspension is as follows: fine-graded magnesium-modified straw powder is pyrolyzed and carbonized at 500℃ for 2 hours under nitrogen protection, ground to a particle size D90 < 10μm, and dispersed in 0.3~0.5mol / L MgCl2 aqueous solution at a solid content of 8%~12%. A uniform suspension is prepared by ultrasonic dispersion and high-speed stirring.